Preparation method of cesium alloying Rb2MnBr4 (H2O) 2 material, anti-counterfeiting label, temperature detection device and information storage device

By preparing cesium alloyed Rb2MnBr4(H2O)2 material, the problems of easy cracking and instability of existing materials were solved, realizing temperature detection of variable optical information and information anti-counterfeiting applications, thus enhancing the security and reliability of information.

CN118932475APending Publication Date: 2024-11-12QUFU NORMAL UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410995173.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing anti-counterfeiting encryption materials based on photoluminescence changes are easily cracked by optical instruments, and metal halide perovskite materials are unstable under external stimuli, making it difficult to achieve multi-mode switching.

Method used

Cesium alloyed Rb2MnBr4(H2O)2 material was prepared by a synthesis method under specific ratios and conditions. The material exhibits high sensitivity and excellent recyclability under temperature and isopropanol solvent conditions, and can be used for anti-counterfeiting labels, temperature detection and information storage devices.

Benefits of technology

It realizes the change of optical information of materials under external stimuli, improves the security and reliability of information, and is applicable to the fields of temperature detection and information anti-counterfeiting.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932475A_ABST
    Figure CN118932475A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a cesium alloying Rb2MnBr4 (H2O) 2 material, and belongs to the field of inorganic material preparation. Aiming at the problems that photoluminescence information of the anti-counterfeiting material is easy to crack and the like, the method comprises the following steps: 1) dissolving CsBr, RbBr and MnBr2 in HBr to obtain a mixture; 2) adding the mixture into a high-pressure kettle, heating and then cooling; and 3) in the process, separating out CsxRb2-yMnBr4 (H2O) 2 single crystals. In the CsxRb2-yMnBr4 (H2O) 2 single crystal, the value range of x is 0 to 1, and the value range of y is 1 to 2. The CsxRb2-yMnBr4 (H2O) 2 single crystal prepared by the method shows high sensitivity to temperature and an isopropanol solvent, shows excellent reproducibility to temperature, and can be used in multiple fields such as anti-counterfeiting labels, temperature detection devices, information storage devices and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a preparation method of a cesium alloyed Rb2MnBr4(H2O)2 material, an anti-counterfeiting label, a temperature detection device and an information storage device, and belongs to the field of chemical industry. Background Art

[0002] The application of stimulus-responsive photoluminescent materials in the field of encryption has attracted much attention. However, the security of anti-counterfeiting encryption based on photoluminescence changes (luminescence intensity and color) is limited because it can be easily replaced by similar luminescent materials. Introducing other luminescent materials (such as rare earth metal complexes, indolecarbazole derivatives and carbon dots) to increase the overall complexity of the material's optical information is an effective way to improve anti-counterfeiting security. Although most reported materials improve information security by increasing the color of the luminescent material and changing the life of the material, since the added luminescent material is monochromatic under one or more stimuli, the encrypted data can be easily cracked by optical instruments, thereby reducing the security of the information. Therefore, it is urgent to find suitable information encryption materials with continuous photoluminescent color-changing domains under external stimuli.

[0003] Metal halide perovskite materials are considered to be the next generation of optoelectronic materials in the fields of photovoltaics, light-emitting diodes, radiation scintillators and lasers. Due to their low formation enthalpy and soft lattice properties, the structure of metal halide perovskite materials is easily destroyed by external factors such as heat, light and chemical fields. Metal halide perovskite materials have been used in multi-stimulus responsive materials due to their inherent instability. Although most reported metal halide perovskite materials can be used as anti-counterfeiting materials under external stimulus conditions, multi-mode switchable metal halide perovskite materials have not yet been explored. Therefore, the design of multi-stimulus responsive perovskite materials has great research value in the field of information anti-counterfeiting. Summary of the invention

[0004] The present application proposes a method for preparing a cesium alloyed Rb2MnBr4(H2O)2 material, which is highly sensitive to temperature and isopropanol solvent and has excellent reproducibility to temperature, and can be used in multiple fields such as anti-counterfeiting labels, temperature detection devices, and information storage devices.

[0005] In order to solve the above technical problems, the technical solution adopted by the present invention is a method for preparing a cesium alloyed Rb2MnBr4(H2O)2 material, comprising the following steps:

[0006] 1) dissolving CsBr, RbBr and MnBr2 in HBr to obtain a mixture;

[0007] 2) adding the mixture into an autoclave, heating it, and then cooling it;

[0008] 3) During this process, Cs is precipitatedx R 2-y MnBr4(H2O)2 single crystal.

[0009] Optimized, the preparation method of the above cesium alloyed Rb2MnBr4(H2O)2 material, Cs x R 2-y In MnBr4(H2O)2 single crystal, the value of x ranges from 0 to 1, and the value of y ranges from 1 to 2.

[0010] Optimized, in the preparation method of the above-mentioned cesium alloyed Rb2MnBr4(H2O)2 material, in step 1), the usage ratio of CsBr, RbBr and MnBr2 is that the sum of the weights of CsBr and RbBr is equal to twice the weight of MnBr2, that is, CsBr+RbBr=2MnBr2.

[0011] Optimized, in the preparation method of the above-mentioned cesium alloyed Rb2MnBr4(H2O)2 material, in step 1), the solid-liquid concentration of the mixture is 0.6 mol / L.

[0012] Optimized, in the preparation method of the above cesium alloyed Rb2MnBr4(H2O)2 material, in step 2), the autoclave is a polytetrafluoroethylene autoclave.

[0013] Optimized, in the preparation method of the above cesium alloyed Rb2MnBr4(H2O)2 material, in step 2), the mixture is heated at 180°C in an autoclave for 12 hours and then cooled to room temperature.

[0014] An anti-counterfeiting label is made of the above-mentioned cesium alloyed Rb2MnBr4(H2O)2 material.

[0015] A temperature detection device is made of the above-mentioned cesium alloyed Rb2MnBr4(H2O)2 material.

[0016] An information storage device, wherein a storage chip of the information storage device is made of the above-mentioned cesium alloyed Rb2MnBr4(H2O)2 material.

[0017] The beneficial effects of this application are:

[0018] The invention provides a method for preparing a Cs alloyed manganese-based bromide perovskite material. The material is highly sensitive to temperature and isopropanol solvent and can be effectively used in the fields of temperature detection and information anti-counterfeiting.

[0019] The Cs alloyed manganese-based bromide perovskite material prepared in the present application exhibits excellent regenerative properties with respect to temperature and can be used in the field of information (read-write-erase-read-write) storage.

[0020] The Cs alloyed manganese-based bromide perovskite material prepared in the present application exhibits continuously variable photoluminescence with respect to temperature and isopropanol solvent, and its variable optical information increases the storage security of information. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 is the XRD pattern of Rb2MnBr4 in this application;

[0022] Figure 2 Cs x R 2-x XRD patterns of MnBr4(H2O)2(x=0,0.2,0.4,0.6,0.8,1);

[0023] Figure 3 Cs 0.8 R 1.2 XRD pattern of MnBr4(H2O)2 after heating and cooling to room temperature;

[0024] Figure 4 Cs 0.8 R 1.2 XRD pattern of MnBr4(H2O)2 after heating at 373K;

[0025] Figure 5 Cs 0.8 R 1.2 XRD pattern of MnBr4(H2O)2 after heating at 473K;

[0026] Figure 6 Cs 0.8 R 1.2 XRD pattern of MnBr4(H2O)2 after heating at 673K;

[0027] Figure 7 For isopropanol treatment of Cs 0.8 R 1.2 XRD pattern after MnBr4(H2O)2;

[0028] Figure 8-1 Cs 0.8 R 1.2 MnBr4(H2O)2 thermochromic image;

[0029] Figure 8-2 Cs 0.8 R 1.2 Schematic diagram of MnBr4(H2O)2 information storage application;

[0030] Figure 8-3Actual images of the luminescence color of cesium alloyed Rb2MnBr4(H2O)2 material treated with isopropanol (a) 7 days and (b) 14 days (irradiation with 365nm ultraviolet light). DETAILED DESCRIPTION

[0031] The technical features of the present invention are further described below in conjunction with specific embodiments.

[0032] The present invention provides a method for preparing a cesium alloyed Rb2MnBr4(H2O)2 material, which is characterized by comprising the following steps:

[0033] 1) dissolving CsBr, RbBr and MnBrHBr in HBr to obtain a mixture;

[0034] 2) adding the mixture into a polytetrafluoroethylene autoclave, heating it, and then cooling it;

[0035] 3) During this process, Cs is precipitated x R 2-y MnBr4(H2O)2 single crystal.

[0036] Cs x R 2-y In the MnBr4(H2O)2 single crystal, the value range of x is 0 to 1, and the value range of y is 1 to 2. The usage ratio of CsBr, RbBr, and MnBr2 is that the sum of the weights of CsBr and RbBr is equal to twice the weight of MnBr2, that is, CsBr+RbBr=2MnBr2. The solid-liquid concentration of the mixture is 0.6 mol / L.

[0037] During the experiment, CsBr, RbBr, MnBr2 and HBr were dissolved in 25 mL polytetrafluoroethylene autoclave, heated at 180 °C for 12 h, kept undisturbed, and cooled to room temperature. x R 2-y MnBr4(H2O)2 single crystal. At this time, the input amount of CsBr is (0, 0.2, 0.4, 0.6, 0.8) mmol, the input amount of RbBr is (2, 1.8, 1.6, 1.4, 1.2, 1) mmol, the input amount of MnBr2 is 1 mmol), and 5 mL of HBr is used. The content of the polytetrafluoroethylene autoclave is 25 mL. During this experiment, the precipitated Cs x R 2-y In MnBr4(H2O)2, x = 0, 0.2, 0.4, 0.6, 0.8 or 1, y = 2, 1.8, 1.6, 1.4, 1.2 or 1. After the experiment, the XRD pattern of Cs x R 2-y The MnBr4(H2O)2 single crystal was analyzed and the XRD pattern is shown in the figure.

[0038] Through the spectrum analysis, it can be seen that the Cs x R 2-y MnBr4(H2O)2 single crystal is highly sensitive to temperature and isopropanol solvent, and can be effectively used in the field of temperature detection and information anti-counterfeiting. Therefore, an anti-counterfeiting label and a temperature detection device are provided in this embodiment. The anti-counterfeiting part of the anti-counterfeiting label adopts Cs x R 2-y The temperature detection part adopts Cs x R 2-y Preparation of MnBr4(H2O)2 single crystal.

[0039] The cesium alloyed Rb2MnBr4(H2O)2 material of the present application is applied to an acrylic plate to make an anti-counterfeiting pattern, and placed on a heating device (such as a heating plate, an oven). Different colors can be observed under 365nm ultraviolet light at different temperatures (such as 300K, 323K, 413K, 433, 453, 473K), and the current temperature can be identified by the color change.

[0040] The cesium alloyed Rb2MnBr4(H2O)2 material of the present application has a unique response ability to isopropanol solvent. When isopropanol solvent is dripped onto the cesium alloyed Rb2MnBr4(H2O)2 material, the material can show different colors of light at different time periods under 365nm ultraviolet light, so it can be used as an anti-counterfeiting material for information identification.

[0041] Through the spectrum analysis, it can be seen that the Cs x R 2-y MnBr4(H2O)2 single crystal exhibits excellent regeneration properties for temperature and can be used in the field of information (read-write-erase-read-write) storage. Therefore, in this embodiment, an information storage device is provided. The information storage chip of the information storage device adopts Cs x R 2-y MnBr4(H2O)2 single crystal production. x R 2-y MnBr4(H2O)2 single crystal material exhibits continuously variable photoluminescence with respect to temperature and isopropanol solvent, and its variable optical information increases the storage security of information.

[0042] The cesium alloyed Rb2MnBr4(H2O)2 material of the present application is sprayed on an acrylic plate to construct an information storage chip. The chip is placed on a 100°C heating plate. The cesium alloyed Rb2MnBr4(H2O)2 material will emit red light at 100°C. When the temperature is increased, the cesium alloyed Rb2MnBr4(H2O)2 material will emit green light at high temperature. Red light is the value 0 in binary, and other luminous colors except red light are 1. During the cooling process, the materials in the chip can be specified to exhibit different luminous colors, thereby demonstrating the binary information storage function. When the temperature is reduced by 100°C, the luminous colors in the chip are all converted to red, reflecting that the chip has a renewable function.

[0043] Of course, the above description is not a limitation of the present invention, and the present invention is not limited to the above examples. Any changes, modifications, additions or substitutions made by ordinary technicians in this technical field within the essential scope of the present invention should fall within the protection scope of the present invention.

Claims

1. A method for preparing cesium alloyed Rb2MnBr4(H2O)2 material, characterized in that: The following steps are involved: 1) dissolving CsBr, RbBr and MnBr2 in HBr to obtain a mixture; 2) adding the mixture into an autoclave, heating it, and then cooling it; 3) During this process, Cs is precipitated x R 2-y MnBr4(H2O)2 single crystal.

2. The method for preparing the cesium alloyed Rb2MnBr4(H2O)2 material according to claim 1, characterized in that: Cs x R 2-y In MnBr4(H2O)2 single crystal, the value of x ranges from 0 to 1, and the value of y ranges from 1 to 2.

3. The method for preparing the cesium alloyed Rb2MnBr4(H2O)2 material according to claim 1, characterized in that: In step 1), the usage ratio of CsBr, RbBr and MnBr2 is that the sum of the weights of CsBr and RbBr is equal to twice the weight of MnBr2, that is, CsBr+RbBr=2MnBr2.

4. The method for preparing the cesium alloyed Rb2MnBr4(H2O)2 material according to claim 1, characterized in that: In step 1), the solid-liquid concentration of the mixture is 0.6 mol / L.

5. The method for preparing the cesium alloyed Rb2MnBr4(H2O)2 material according to claim 1, characterized in that: In step 2), the autoclave is a polytetrafluoroethylene autoclave.

6. The method for preparing the cesium alloyed Rb2MnBr4(H2O)2 material according to claim 1, characterized in that: In step 2), the mixture is heated at 180° C. for 12 hours in an autoclave and then cooled to room temperature.

7. An anti-counterfeiting label, characterized by: Made of cesium alloyed Rb2MnBr4(H2O)2 material according to any one of claims 1-6.

8. A temperature detection device, characterized in that: Made of cesium alloyed Rb2MnBr4(H2O)2 material according to any one of claims 1-6.

9. An information storage device, characterized in that: The memory chip of the information storage device is made of the cesium alloyed Rb2MnBr4(H2O)2 material of any one of claims 1-6.