Gallium nitride single crystal substrate
By doping germanium in the inclined interface growth area of the gallium nitride single crystal substrate with high concentration doping germanium and controlling the diameter distribution of the etching pit, the problem of large dislocation strain field in alkali-based etching is solved, and the device characteristics and dislocation distribution uniformity are improved.
Patent Information
- Application Number
- CN202410102668.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2023-05-12
- Filing Date
- 2024-01-24
- Publication Date
- 2024-11-12
AI Technical Summary
The larger etching pits formed by existing gallium nitride single crystal substrates during alkali-based etching lead to a large dislocation strain field, affecting device characteristics, and it is difficult to accurately identify the type of dislocation through the etching pit size.
By doping germanium at high concentrations in the growth area of the inclined interface, the peak in the pit diameter histogram is controlled to reduce the number of large pits and ensure that device characteristics are not affected.
It effectively reduces dislocations with large strain field in device characteristics, improves the device characteristics of gallium nitride single crystal substrate, and ensures uniform dislocation distribution during etching.
Smart Images

Figure CN118932488A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a gallium nitride single crystal substrate. Background Art
[0002] For example, Patent Document 1 discloses a method for manufacturing a gallium nitride single crystal substrate, wherein the manufacturing method comprises: a step of preparing a base substrate, wherein the base substrate is composed of a single crystal of a group III nitride semiconductor and has a mirror-finished main surface, wherein the low-index crystal plane closest to the main surface is the (0001) plane; a first step of growing a first layer, wherein a single crystal of a group III nitride semiconductor having a top surface with the (0001) plane exposed is directly epitaxially grown on the main surface of the base substrate, and a plurality of recesses formed by inclined interfaces other than the (0001) plane are generated on the top surface, and the inclined interfaces are gradually expanded as they progress toward the top of the main surface of the base substrate, so that the (0001) plane disappears from the top surface, thereby forming a surface composed only of the inclined interfaces; and a second step of growing a second layer having a mirror-finished surface, wherein a single crystal of a group III nitride semiconductor is epitaxially grown on the first layer, thereby disappearing the inclined interfaces, wherein in the first step, a plurality of recesses are generated on the top surface of the single crystal, and the (0001) plane disappears, thereby forming a plurality of valleys and a plurality of tops on the surface of the first layer.
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent Application Publication No. 2020-33211 Summary of the invention
[0006] Problems to be solved by the invention
[0007] The object of the present invention is to improve the characteristics of a device fabricated on a gallium nitride single crystal substrate.
[0008] Solutions to Solve Problems
[0009] According to one embodiment of the present invention,
[0010] Provided is a gallium nitride single crystal substrate having a diameter of 50 mm or more, wherein the low-index crystal plane closest to the main surface is the (0001) plane, wherein:
[0011] The density of the etch pits formed when the main surface is etched with an alkaline etching solution is less than 1×10 6 cm -2 ,
[0012] When the diameter of the first peak appearing on the smallest side among the peaks appearing in the histogram of the pit diameters is defined as a, the total number of pits having a diameter exceeding 4a is less than 1 / 1000 of the number of pits constituting the first peak.
[0013] Effects of the Invention
[0014] According to the present invention, the characteristics of a device manufactured on a gallium nitride single crystal substrate can be improved. BRIEF DESCRIPTION OF THE DRAWINGS
[0015] Figure 1 This is a flowchart showing a method for manufacturing a gallium nitride single crystal substrate according to one embodiment of the present invention.
[0016] Figure 2A This is a schematic cross-sectional view showing a part of a method for manufacturing a gallium nitride single crystal substrate according to an embodiment of the present invention.
[0017] Figure 2B This is a schematic cross-sectional view showing a part of a method for manufacturing a gallium nitride single crystal substrate according to an embodiment of the present invention.
[0018] Figure 2C This is a schematic cross-sectional view showing a part of a method for manufacturing a gallium nitride single crystal substrate according to an embodiment of the present invention.
[0019] Figure 3A This is a schematic cross-sectional view showing a part of a method for manufacturing a gallium nitride single crystal substrate according to an embodiment of the present invention.
[0020] Figure 3B This is a schematic cross-sectional view showing a part of a method for manufacturing a gallium nitride single crystal substrate according to an embodiment of the present invention.
[0021] Figure 4A This is a schematic cross-sectional view showing a part of a method for manufacturing a gallium nitride single crystal substrate according to an embodiment of the present invention.
[0022] Figure 4B This is a schematic cross-sectional view showing a part of a method for manufacturing a gallium nitride single crystal substrate according to an embodiment of the present invention.
[0023] Figure 5 This is a SEM image showing an example of an etch pit formed on the main surface of the gallium nitride single crystal substrate according to one embodiment of the present invention.
[0024] Fig. 6A It is a histogram of the diameter of the etch pit in Example 1.
[0025] Figure 6B Yes Fig. 6A The resulting graph is enlarged in the vertical direction.
[0026] Fig. 7A It is a histogram of the diameter of the etch pit in Example 2.
[0027] Figure 7B Yes Fig. 7A The resulting graph is enlarged in the vertical direction.
[0028] Fig. 8A It is a histogram of the diameter of the etch pit of the comparative example.
[0029] Figure 8B Yes Fig. 8A The resulting graph is enlarged in the vertical direction.
[0030] Description of Reference Numerals
[0031] 10 substrate; 30 first layer; 32 inclined interface expansion layer; 34 inclined interface maintenance layer; 40 second layer; 42 c-plane expansion layer; 44 main growth layer; 50 gallium nitride single crystal substrate (substrate); 60 first c-plane growth region; 70 inclined interface growth region; 80 second c-plane growth region; 90 stacked structure. DETAILED DESCRIPTION
[0032] <Insights Obtained by the Inventors>
[0033] First, the findings obtained by the inventors are described.
[0034] It is known that when etching is performed on the c-plane of a gallium nitride (GaN) single crystal substrate, for example, using an alkaline etching solution, an etch pit corresponding to the dislocation is formed. In addition, a method of specifying the type of dislocation (edge-shaped, mixed, spiral) by the size (diameter) of the etch pit is also known to those skilled in the art, but this method may not be universally applicable. The size of the etch pit formed by alkaline etching corresponds to the size of the strain of the lattice around the dislocation core. Therefore, this is because in addition to the type of dislocation, the size of the etch pit is also affected by the impurities captured by the dislocation or the precipitates on the dislocation, the distance to other nearby dislocations, etc.
[0035] For the above reasons, it is difficult to identify the type of dislocation (edge-shaped, mixed, spiral) by the size of the etch pit, but it can be said that for dislocations that form larger etch pits, the strain field around the dislocation core is also larger. For dislocations with a larger strain field, the possibility of having a larger Burgers vector is higher, and such dislocations become micropipe defects with a hollow dislocation core (hollow core), which easily become abnormal diffusion paths for impurities. The inventors found that the dislocations with a larger strain field have an adverse effect on the characteristics of devices made on gallium nitride single crystal substrates.
[0036] The size of the etch pit also depends greatly on the etching conditions. Therefore, it is meaningless to discuss the absolute value of the size of the etch pit. However, among the several etch pits of different sizes detected by etching, the etch pit with the smallest size is very likely to correspond to the edge dislocation with the smallest strain field around the dislocation core. Therefore, the inventors have discovered the following technology: by investigating the histogram of the diameter of the etch pit, the diameter and number of other etch pits are investigated based on the diameter of the peak with the smallest diameter among the peaks appearing in the histogram, so as to grasp the presence or absence of dislocation defects that have an adverse effect on the characteristics of the device made on the gallium nitride single crystal substrate. In addition, it was found that when the diameter of the etch pit that will serve as the benchmark is set to a, the etch pit with a diameter exceeding 4a corresponds to the dislocation that has accumulated the above-mentioned large strain, and such dislocations are more likely to have an adverse effect on the device characteristics.
[0037] Furthermore, the inventors have conducted in-depth research on methods for reducing (or eliminating) dislocations that have accumulated large strains as described above. As a result, they have discovered that by doping germanium (Ge) at a high concentration in the inclined interface growth region in the step of growing the inclined interface as a growth surface (the first step described later) as described in Patent Document 1, a gallium nitride single crystal substrate having almost no large etch pits exceeding 4a in diameter (that is, substantially no dislocations that have accumulated large strains and are likely to have a high adverse effect on device characteristics) can be manufactured when etching is performed using an alkaline etching solution.
[0038] <One embodiment of the present invention>
[0039] Hereinafter, one embodiment of the present invention will be described with reference to the drawings.
[0040] (1) Method for manufacturing gallium nitride single crystal substrate
[0041] First, a method for manufacturing a gallium nitride single crystal substrate according to the present embodiment will be described. Figure 1 : is a flowchart showing the method for manufacturing a gallium nitride single crystal substrate according to the present embodiment. Figure 2A to Figure 2C , Figure 3A , Figure 3B , Figure 4A , Figure 4B is a schematic cross-sectional view showing a part of the method for manufacturing a gallium nitride single crystal substrate according to the present embodiment. Figure 3B In the figure, the thin solid line s represents the crystal plane in the middle of the growth. Figure 2C , Figure 3A , Figure 3B , Figure 4A , Figure 4B In the figure, the dashed lines represent dislocations.
[0042] like Figure 1As shown, the method for manufacturing a gallium nitride single crystal substrate according to the present embodiment includes, for example, a base substrate preparation step S100 , a first step S200 , a second step S300 , a slicing step S400 , and a grinding step S500 .
[0043] (S100: Base substrate preparation step)
[0044] like Figure 2A As shown, in the base substrate preparation step S100, a base substrate 10 composed of a gallium nitride single crystal is prepared. In the base substrate preparation step S100 of this embodiment, a commercially available gallium nitride single crystal substrate (a self-supporting substrate rather than a template) can be used as the base substrate 10. In addition, the base substrate 10 composed of a gallium nitride single crystal can also be produced by the VAS (Void-Assisted Separation) method described in Patent Document 1.
[0045] The base substrate 10 may be Ge-doped, Si-doped, or undoped, and a Ge-doped GaN layer is particularly preferred. This can reduce the Ge concentration difference between the base substrate 10 and the first layer 30 described later.
[0046] It should be noted that, in the following, in a GaN crystal having a wurtzite structure, <0001> The axis is called the "c-axis" and the (0001) plane is called the "c-plane". It should be noted that the (0001) plane is sometimes called the "+c plane (gallium polar plane)" and the (000-1) plane is sometimes called the "-c plane (nitrogen (N) polar plane)". In addition, the <1-100> axis is called the "m-axis" and the {1-100} plane is called the "m-plane".
[0047] The m-axis may also be expressed as the <10-10> axis. The <11-20> axis is referred to as the "a-axis", and the {11-20} plane is referred to as the "a-plane".
[0048] (S200: First step (first layer growth step))
[0049] On the base substrate 10 prepared in the base substrate preparation step S100, as Figure 2B As shown, GaCl gas and NH 3 gas are supplied to the heated base substrate 10 by, for example, HVPE method, so that a GaN single crystal having a top surface 30 u with a c-plane 30 c exposed is epitaxially grown directly on the main surface 10 s of the base substrate 10 . Thus, the first layer 30 is grown.
[0050] At this time, a plurality of recesses 30p formed by being surrounded by inclined interfaces 30i other than the c-plane are generated on the top surface 30u of the single crystal. As the inclined interfaces 30i gradually expand toward the upper side of the main surface 10s of the base substrate 10, the c-plane 30c gradually shrinks. As a result, the c-plane 30c disappears from the top surface 30u. As a result, Figure 2C As shown, a first layer 30 is grown whose surface consists only of inclined interfaces 30i.
[0051] That is, in the first step S200 , the first layer 30 is three-dimensionally grown in a single crystal state so that the main surface 10 s of the base substrate 10 is intentionally roughened.
[0052] In the first step S200, for example, the first layer 30 is grown under a predetermined first growth condition. As the first growth condition of the present embodiment, for example, the growth temperature in the first step S200 is lower than the growth temperature in the second step S300 described later. Specifically, the growth temperature in the first step S200 is, for example, 980° C. to 1020° C., preferably 1000° C. to 1020° C.
[0053] In addition, as the first growth condition of the present embodiment, for example, the ratio of the supply rate of the NH3 gas as the nitriding agent gas to the supply rate of the GaCl gas as the Group III source gas in the first step S200 (hereinafter also referred to as "V / III ratio") may be greater than the V / III ratio in the second step S300 described later. Specifically, the V / III ratio in the first step S200 is, for example, 2 or more and 20 or less, preferably 2 or more and 15 or less.
[0054] In the present embodiment, under the first growth condition, Ge is doped into the first layer 30 (especially the inclined interface growth region 70 described later) at a high concentration. As a result, on the surface of the second layer 40 described later, it is possible to reduce dislocations that have accumulated large strains, thereby effectively increasing the existence ratio of dislocations with smaller strain fields. Ge doping is performed, for example, using germanium tetrachloride (GeCl4) gas. The GeCl4 gas is supplied, for example, from a gas cylinder, or by placing the raw material container in a constant temperature bath maintained at about 5°C and bubbling the GeCl4 with a carrier gas while making it liquid. The carrier gas can use either H2 gas or N2 gas, or both H2 gas and N2 gas. Preferably, in either case, the flow rate is controlled by a mass flow controller so that the partial pressure of the GeCl4 gas becomes 0.3 to 30 Pa, so that the Ge concentration of the first layer 30 (especially the inclined interface growth region 70) becomes 3×10 18 ~9×10 20 cm -3 Make appropriate adjustments in the manner.
[0055] It should be noted that other conditions in the first growth condition of this embodiment are as follows, for example.
[0056] Growth pressure: 90-105 kPa, preferably 90-95 kPa
[0057] Partial pressure of GaCl gas: 1.5~15kPa
[0058] N2 gas flow rate / H2 gas flow rate: 0~1
[0059] Partial pressure of GeCl4 gas: 0.3~30Pa
[0060] Here, the first step S200 of the present embodiment is classified into two steps based on, for example, the morphology of the first layer 30 during growth. Specifically, the first step S200 of the present embodiment includes, for example, a sloped interface expansion step S220 and a sloped interface maintenance step S240. Through these steps, the first layer 30 includes, for example, a sloped interface expansion layer 32 and a sloped interface maintenance layer 34.
[0061] (S220: Inclined Interface Enlarging Process)
[0062] First, if Figure 2B As shown, the inclined interface expansion layer 32 of the first layer 30 composed of GaN single crystal is epitaxially grown directly on the primary surface 10s of the base substrate 10 under the above-mentioned first growth condition.
[0063] In the initial stage of the growth of the inclined interface expansion layer 32 , the inclined interface expansion layer 32 grows with the c-plane 30 c as the growth plane in the normal direction (direction along the c-axis) of the primary surface 10 s of the base substrate 10 .
[0064] By gradually growing the inclined interface expansion layer 32 under the first growth condition, such as Figure 2B As shown in FIG. 1 , a plurality of recesses 30p formed by the inclined interfaces 30i other than the c-plane are generated on the top surface 30u where the c-plane 30c is exposed in the inclined interface expansion layer 32. A plurality of recesses 30p formed by the inclined interfaces 30i other than the c-plane are randomly formed on the top surface 30u. Thus, the inclined interface expansion layer 32 is formed in which the c-plane 30c and the inclined interfaces 30i other than the c-plane are mixed on the surface.
[0065] It should be noted that the "inclined interface 30i" mentioned here means a growth interface inclined relative to the c-plane 30c, including a small face with a low index other than the c-plane, a small face with a high index other than the c-plane, or an inclined face that cannot be represented by a face index. It should be noted that the small face other than the c-plane is, for example, {11-2m}, {1-10n}, etc., wherein m and n are integers other than 0.
[0066] By further growing the inclined interface expansion layer 32 under the first growth condition, such as Figure 2B As shown in FIG. 1 , as the base substrate 10 is advanced upward, the inclined interface 30i other than the c-plane is gradually expanded in the inclined interface expansion layer 32, and the c-plane 30c is gradually reduced. It should be noted that at this time, as the base substrate 10 is advanced upward, the inclination angle of the inclined interface 30i relative to the main surface 10s of the base substrate 10 gradually decreases. As a result, most of the inclined interface 30i finally becomes a {11-2m} plane with m≥3.
[0067] If the inclined interface enlargement layer 32 is further grown, Figure 2C As shown, the c-plane 30c of the inclined interface expansion layer 32 disappears from the top surface 30u, and the surface of the inclined interface expansion layer 32 is composed only of the inclined interface 30i. Thus, the inclined interface expansion layer 32 having a mountain shape formed by continuously connecting cones is formed.
[0068] In the present embodiment, in the initial stage of the growth of the inclined interface expansion layer 32, the inclined interface 30i is not generated on the main surface 10s of the base substrate 10, and the inclined interface expansion layer 32 is grown with a predetermined thickness using the c-plane 30c as the growth plane, and then an inclined interface 30i other than the c-plane is generated on the surface of the inclined interface expansion layer 32. As a result, a plurality of valleys 30v are formed at positions upwardly away from the main surface 10s of the base substrate 10. At this time, when the base substrate 10 doped with Ge is used, it is preferable to adjust the Ge concentration difference between the base substrate 10 and the region grown using the c-plane 30c as the growth plane to, for example, 1×10 18 cm -3 the following.
[0069] Through the growth process of the inclined interface expansion layer 32 as described above, dislocations propagate in a zigzag manner as follows. Specifically, Figure 2CAs shown, multiple dislocations extending in the direction along the c-axis in the base substrate 10 propagate from the base substrate 10 toward the c-axis direction of the inclined interface expansion layer 32. In the region of the inclined interface expansion layer 32 that grows with the c-plane 30c as the growth plane, the dislocations propagate from the base substrate 10 toward the c-axis direction of the inclined interface expansion layer 32. However, when the growth plane of the dislocations propagating in the direction along the c-axis changes to the inclined interface 30i due to the expansion of the inclined interface, the dislocations propagate in a zigzag manner toward a direction substantially perpendicular to the inclined interface 30i. That is, the dislocations propagate in a zigzag manner in a direction inclined relative to the c-axis. Thus, in the process after the inclined interface expansion process S220, the dislocations are locally gathered in the approximate center of the multiple recesses 30p formed by the inclined interface 30i. Among the dislocations gathered in the approximate center of the recess 30p, the dislocations having opposite Burgers vectors disappear when they converge. Another part forms a dislocation loop, and the propagation in the direction along the c-axis is suppressed. As a result, it is possible to reduce the dislocation density on the surface of the second layer 40 described later. On the other hand, dislocations that do not converge with other dislocations continue to propagate as they are, and some dislocations converge with other dislocations to propagate while forming a larger Burgers vector.
[0070] At this time, on the inclined interface expansion layer 32, based on the difference in growth planes during the growth process, a first c-plane growth region 60 is formed which grows with the c-plane 30c as the growth plane, and an inclined interface growth region 70 (gray part in the figure) is formed which grows with the inclined interface 30i other than the c-plane as the growth plane.
[0071] In addition, at this time, in the first c-plane growth region 60, a concave portion 60a is formed at the position where the inclined interface 30i is generated, and a convex portion 60b is formed at the position where the c-plane 30c disappears. In addition, in the first c-plane growth region 60, a pair of inclined portions 60i are formed on both sides of the convex portion 60b as the locus of the intersection of the c-plane 30c and the inclined interface 30i.
[0072] (S240: Inclined Interface Maintaining Step)
[0073] After the c-plane 30c disappears from the surface of the inclined interface expansion layer 32, as shown in FIG. Figure 3A As shown in the figure, the growth of the first layer 30 is continued at a predetermined thickness while maintaining the state that the surface is composed of only the inclined interface 30i. Thus, an inclined interface maintaining layer 34 having no c-plane and only the inclined interface 30i on the surface is formed on the inclined interface expansion layer 32. By forming the inclined interface maintaining layer 34, the c-plane 30c can be reliably eliminated in the entire range of the surface of the first layer 30.
[0074] At this time, similarly to the inclined interface expanding step S220, the growth condition in the inclined interface maintaining step S240 is maintained under the above-mentioned first growth condition. Thus, the inclined interface maintaining layer 34 can be grown using only the inclined interface 30i as a growth surface.
[0075] In addition, at this time, under the first growth condition, the tilted interface maintaining layer 34 is grown with the tilted interface 30i as the growth plane, so that as described above, at the position where the tilted interface 30i is exposed in the tilted interface expansion layer 32, the dislocations that are zigzag-propagated in a direction tilted relative to the c-axis also continue to propagate in the same direction in the tilted interface maintaining layer 34.
[0076] In this case, the sloped interface maintaining layer 34 grows with the sloped interface 30 i as a growth plane, so that the entire sloped interface maintaining layer 34 becomes a part of the sloped interface growth region 70 .
[0077] In the inclined interface growth region 70, oxygen is easily absorbed compared to the first c-plane growth region 60. Therefore, the oxygen concentration in the inclined interface growth region 70 is higher than the oxygen concentration in the first c-plane growth region 60. It should be noted that the oxygen absorbed into the inclined interface growth region 70 is, for example, oxygen that is unintentionally mixed into the HVPE device, or oxygen released from components (quartz components, etc.) constituting the HVPE device. As oxygen is absorbed into the inclined interface growth region 70, the lattice constant becomes larger and the crystal deforms toward the convex side. The c-plane shape of the GaN substrate manufactured by the VAS method is usually concavely curved. If a GaN substrate manufactured by the VAS method is used in the base substrate 10, the c-plane shape, which is initially concave, gradually deforms toward the convex side due to the thicker growth of the inclined interface growth region 70, and approaches a plane, so the c-axis distribution becomes smaller. As a result, the radius of curvature of the c-plane 40c of the main growth layer 44 described later can be increased.
[0078] It should be noted that the oxygen concentration in the first c-plane growth region 60 is, for example, 5×10 16 cm -3 Below, preferably 3×10 16 cm -3 On the other hand, the oxygen concentration in the inclined interface growth region 70 is, for example, 3×10 18 cm -3 Above and 5×10 19 cm -3 the following.
[0079] Here, by doping Ge at a high concentration in the inclined interface growth region 70, dislocations with large accumulated strain can be reduced on the surface of the second layer 40 described later. Ge has the effect of hindering the movement of dislocations (pinning effect, pinning), and has the property that the larger the strain field of the dislocation, the easier it is for the impurities to gather in the dislocation core due to the Cottrell effect. As mentioned above, there are dislocations that gather in the concave portion 30p and form a large Burgers vector. By doping Ge at a high concentration in the inclined interface 30i (especially the inclined interface growth region 70), the dislocations with particularly large strain fields among the gathered dislocations are pinned by Ge. The progress of the pinned dislocation to other slip planes is hindered, so it is difficult to maintain propagation in the original form, and the probability of decomposing into two or more dislocations to maintain propagation and progress increases. The decomposed dislocations become dislocations with smaller strain fields than before, so the existence ratio of dislocations with smaller strain fields can be increased on the surface of the second layer 40. By decomposing the dislocations with a large strain field, the number of dislocations increases, but the absolute number of dislocations with a large strain field is originally small, so the number of dislocations increased by the above decomposition is negligibly small compared to the number of dislocations that are concentrated in the approximate center of the concave portion 30p of the inclined interface 30i and reduced. Thus, the dislocations with a large strain field that have an adverse effect on device characteristics can be selectively reduced.
[0080] Compared to the first c-plane growth region 60 grown with the c-plane 30c as the growth plane, Ge is easily absorbed in the inclined interface growth region 70 grown with the inclined interface 30i other than the c-plane as the growth plane, just like oxygen. Therefore, when Ge is doped at the time of forming the inclined interface 30i, the Ge concentration of the inclined interface 30i becomes higher than that of the c-plane 30c. In addition, in the inclined interface 30i, dislocations are bent in a direction inclined relative to the c-axis and gathered in the approximate center of the recess 30p, so by doping Ge at the time of forming the inclined interface 30i, dislocations with large strain fields can be effectively reduced.
[0081] The Ge concentration of the inclined interface growth region 70 is preferably 3×10 18 ~9×10 20 cm -3 The O concentration or Ge concentration in the inclined interface growth region 70 can be measured, for example, by secondary ion mass spectrometry (SIMS). The effect of increasing the existence ratio of dislocations with a small strain field is shown in the case where the Ge concentration in the inclined interface growth region 70 exceeds 5×10 18 cm -3 It began to show significantly at 5×10 19 cm -3 If the Ge concentration in the inclined interface growth region 70 exceeds 5×10 21 cm -3, then the crystal grows abnormally (such as polycrystallization).
[0082] Through the above-described first step S200 , the first layer 30 including the sloped interface expansion layer 32 and the sloped interface maintaining layer 34 is formed.
[0083] In the first step S200 of the present embodiment, it is preferred that the height from the main surface 10s of the base substrate 10 to the top 30t of the first layer 30 (the maximum height in the thickness direction of the first layer 30, hereinafter also referred to as the thickness of the first layer 30) is set to, for example, 0.5 mm or more and 3 mm or less. If the thickness of the first layer 30 is less than 0.5 mm, it may not be possible to fully obtain the effect of increasing the existence ratio of dislocations with smaller strain fields on the surface of the second layer 40. In contrast, by setting the thickness of the first layer 30 to be greater than 0.5 mm, the effect of increasing the existence ratio of dislocations with smaller strain fields can be fully obtained. On the other hand, if the thickness of the first layer 30 exceeds 3 mm, the effect of increasing the existence ratio of dislocations with smaller strain fields on the surface of the second layer 40 is likely to be saturated, which is disadvantageous in terms of production cost. In contrast, by setting the thickness of the first layer 30 to be less than 3 mm, the effect of increasing the existence ratio of dislocations with smaller strain fields can be efficiently obtained.
[0084] (S300: Second Step (Second Layer Growth Step))
[0085] After the first layer 30 is grown so that the c-plane 30c disappears, as shown in FIG. Figure 3B as well as Figure 4A As shown, on the first layer 30, a GaN single crystal is further epitaxially grown.
[0086] At this time, the inclined interface 40i is gradually reduced and the c-plane 40c is gradually expanded as the main surface 10s of the base substrate 10 is advanced. Thus, the inclined interface 30i formed on the surface of the first layer 30 disappears. As a result, the second layer 40 having a mirror-finished surface grows.
[0087] In the second step S300, for example, the second layer 40 is grown under a predetermined second growth condition. As the second growth condition of the present embodiment, the growth temperature in the second step S300 is, for example, higher than the growth temperature in the first step S200. Specifically, the growth temperature in the second step S300 is, for example, 990° C. to 1120° C., preferably 1020° C. to 1100° C.
[0088] In addition, as the second growth condition of the present embodiment, the V / III ratio in the second step S300 may also be adjusted. For example, the V / III ratio in the second step S300 may be smaller than the V / III ratio in the first step S200. Specifically, the V / III ratio in the second step S300 is, for example, greater than 1 and less than 10, preferably greater than 1 and less than 5.
[0089] The second step S300 of this embodiment is classified into two steps based on the morphology of the second layer 40 during growth. Specifically, the second step S300 of this embodiment includes, for example, a c-plane expansion step S320 and a main growth step S340. Through these steps, the second layer 40 includes, for example, a c-plane expansion layer 42 and a main growth layer 44.
[0090] It should be noted that other conditions in the second growth condition of this embodiment are as follows, for example.
[0091] Growth pressure: 90-105 kPa, preferably 90-95 kPa
[0092] Partial pressure of GaCl gas: 1.5~15kPa
[0093] N2 gas flow rate / H2 gas flow rate: 1~20
[0094] (S320: c-surface enlargement step)
[0095] like Figure 3B As shown, the c-plane extension layer 42 of the second layer 40 composed of GaN single crystal is epitaxially grown on the first layer 30 under the above-mentioned second growth condition.
[0096] At this time, as the surface goes upward in the first layer 30 , the c-plane 40 c is expanded, while the inclined interface 40 i other than the c-plane is reduced.
[0097] Specifically, by the growth under the second growth condition, the c-plane expansion layer 42 grows in a direction perpendicular to the c-axis (i.e., along the plane direction or the lateral direction) from the inclined interface 30i of the inclined interface maintaining layer 34 with the inclined interface 40i as the growth plane. If the c-plane expansion layer 42 is grown in the lateral direction, the c-plane 40c of the c-plane expansion layer 42 begins to be exposed again above the top 30t of the inclined interface maintaining layer 34. Thus, the c-plane expansion layer 42 is formed in which the c-plane 40c and the inclined interfaces 40i other than the c-plane are mixed on the surface.
[0098] As the c-plane expansion layer 42 further grows in the lateral direction, the c-plane 40c gradually expands and the inclined interface 40i of the c-plane expansion layer 42 gradually shrinks. Thus, the concave portion 30p formed by the plurality of inclined interfaces 30i on the surface of the first layer 30 is gradually filled.
[0099] Then, when the c-plane expansion layer 42 is further grown, the inclined interface 40i of the c-plane expansion layer 42 completely disappears, and the concave portion 30p formed by the plurality of inclined interfaces 30i on the surface of the first layer 30 is completely filled. As a result, the surface of the c-plane expansion layer 42 becomes a mirror surface (flat surface) composed only of the c-plane 40c.
[0100] At this time, during the growth of the first layer 30 and the c-plane expansion layer 42, the dislocation density can be reduced by locally gathering dislocations. Specifically, dislocations that propagate in a zigzag manner in the direction inclined relative to the c-axis in the first layer 30 continue to propagate in the same direction in the c-plane expansion layer 42. As a result, dislocations are locally gathered at the convergence portion of adjacent inclined interfaces 40i above the approximate center between a pair of tops 30t in the c-plane expansion layer 42. Among the multiple dislocations gathered at the convergence portion of adjacent inclined interfaces 40i in the c-plane expansion layer 42, dislocations having opposite Burgers vectors disappear when they converge. In addition, a portion of the multiple dislocations gathered at the convergence portion of adjacent inclined interfaces 40i forms a loop, and the propagation in the direction along the c-axis (i.e., the surface side of the c-plane expansion layer 42) is suppressed. It should be noted that another part of the multiple dislocations gathered at the convergence portion of the adjacent inclined interfaces 40i in the c-plane expansion layer 42 changes its propagation direction from the direction inclined relative to the c-axis to the direction along the c-axis again, and propagates to the surface side of the second layer 40. By making a part of the multiple dislocations disappear or suppressing the propagation of a part of the multiple dislocations to the surface side of the c-plane expansion layer 42 in this way, the dislocation density on the surface of the second layer 40 can be reduced. In addition, by locally gathering dislocations, a low dislocation density region can be formed above the portion of the second layer 40 where the dislocations propagate in the direction inclined relative to the c-axis.
[0101] Here, in the c-plane expansion process S320, it is also preferred to dope Ge in high concentration into the second layer 40 (especially the c-plane expansion layer 42). During the growth of the inclined interface 40i in the c-plane expansion layer 42, by doping Ge in high concentration in the same manner as in the inclined interface growth region 70, the increase of dislocations that have accumulated large strains in the c-plane 40c of the second layer 40 can be suppressed. In addition, during the growth of the inclined interface 40i, by doping Ge in high concentration, dislocations that have accumulated large strains can be further reduced. When doping Ge into the c-plane expansion layer 42, it can be doped at the same concentration as that of Ge doped in the inclined interface growth region 70, or it can be doped at a different concentration. When doping at a concentration different from that of the inclined interface growth region 70, it is preferred to continuously change the Ge concentration during the growth of the second layer 40. At this time, the partial pressure of the GeCl4 gas is preferably adjusted in the range of 0.3 to 40 Pa.
[0102] At this time, in the c-plane expansion layer 42 , the c-plane 40 c gradually expands, and a second c-plane growth region 80 described later that grows with the c-plane 40 c as a growth plane is formed while gradually expanding upward in the thickness direction.
[0103] In the c-plane expansion step S320, since the surface of the c-plane expansion layer 42 becomes a mirror surface composed only of the c-plane 40c, the height of the c-plane expansion layer 42 in the thickness direction (the maximum height in the thickness direction) is, for example, greater than the height from the valley 30v to the top 30t of the inclined interface maintaining layer 34.
[0104] (S340: Main Growth Step (c-plane Growth Step))
[0105] When the inclined interface 40i disappears in the c-plane expansion layer 42 and the surface is mirror-finished, as shown in FIG. Figure 4A As shown, a main growth layer 44 is formed with a c-plane 40c as a growth plane and a predetermined thickness on the c-plane expansion layer 42. Thus, a main growth layer 44 is formed which has no inclined interface 40i and has only the c-plane 40c on the surface.
[0106] At this time, similarly to the c-plane expansion step S320, the growth conditions in the main growth step S340 are maintained under the above-mentioned second growth conditions. Thus, the main growth layer 44 can be grown by step-flow growth with the c-plane 40c as the growth plane.
[0107] In the main growth step S340, GaCl gas, NH3 gas, and dichlorosilane (SiH2Cl2) gas as an n-type dopant gas may be supplied to the base substrate 10 heated to a predetermined growth temperature, so that a silicon (Si)-doped GaN layer is epitaxially grown as the second layer 40. GeCl4 gas or the like may be supplied as an n-type dopant gas instead of SiH2Cl2 gas, so that a Ge-doped GaN layer is epitaxially grown. It should be noted that a GaN layer doped with iron (Fe), manganese (Mn), carbon (C), etc. may also be epitaxially grown as the second layer 40.
[0108] In the main growth process S340, when Ge is doped into the second layer 40, the doping may be performed at the same concentration as that of Ge doped into the c-plane expansion layer 42 in the c-plane expansion process S320, or at a different concentration. When doping is performed at a concentration different from that in the c-plane expansion process S320, it is preferred that the Ge concentration be continuously changed during the growth of the main growth process S340. At this time, the partial pressure of the GeCl4 gas is preferably adjusted within the range of 0.3 to 50 Pa. In addition, in the main growth process S340, when doping with a dopant other than Ge (for example, Si), it is preferred that the Ge concentration be gradually reduced during the growth of the main growth process S340, and after the Ge concentration reaches the detection lower limit based on SIMS, the concentration of the dopant other than Ge be gradually increased.
[0109] In addition, at this time, since the inclined interface growth region 70 absorbs oxygen and the crystal lattice is extended, the c-axis distribution of the second layer 40 becomes smaller, so that the radius of curvature of the c-plane 40c of the main growth layer 44 grown thereon can be made larger than the radius of curvature of the c-plane 10c of the base substrate 10. As a result, the deviation of the deviation angle of the c-axis in the main growth layer 44 relative to the normal to the surface can be made smaller than the deviation of the deviation angle of the c-axis 10ca in the base substrate 10 relative to the normal to the main surface 10s.
[0110] In this case, the main growth layer 44 is grown with only the c-plane 40c as a growth plane without exposing the inclined interface 40i, so that the entire main growth layer 44 becomes a second c-plane growth region 80 described later.
[0111] In the main growth step S340, the thickness of the main growth layer 44 is set to, for example, 300 μm or more and 10 mm or less. By setting the thickness of the main growth layer 44 to 300 μm or more, at least one or more substrates 50 can be sliced from the main growth layer 44 in the slicing step S400 described later. On the other hand, by setting the thickness of the main growth layer 44 to 10 mm or less, when the final thickness is set to 650 μm and a 700 μm thick substrate 50 is sliced from the main growth layer 44, at least 10 substrates 50 can be obtained even if a cut loss of about 200 μm is taken into account.
[0112] Through the above second step S300, the second layer 40 including the c-plane expansion layer 42 and the main growth layer 44 is formed. As a result, the stacked structure 90 of the present embodiment is formed.
[0113] It should be noted that the above steps from the first step S200 to the second step S300 are continuously performed in the same chamber in a manner that the base substrate 10 is not exposed to the atmosphere. Thus, it is possible to suppress the formation of an unintended high oxygen concentration region (a region having an excessively high oxygen concentration compared to the inclined interface growth region 70) at the interface between the first layer 30 and the second layer 40.
[0114] (S400: Slicing process)
[0115] Next, if Figure 4B As shown, for example, the main growth layer 44 is sliced using a wire saw along a cut plane substantially parallel to the surface of the main growth layer 44. Thus, at least one gallium nitride single crystal substrate 50 (also referred to as substrate 50) is formed as an as-cut substrate. At this time, the thickness of the substrate 50 is set to, for example, 300 μm or more and 700 μm or less.
[0116] At this time, the curvature radius of the c-plane 50c of the substrate 50 cut out from the main growth layer 44 is larger than the curvature radius of the c-plane 10c of the base substrate 10 for the above-mentioned reasons. As a result, the deviation of the deviation angle θ of the c-axis 50ca with respect to the normal line of the main surface 50s of the substrate 50 (the extreme difference of the deviation angle θ within the substrate surface) can be made smaller than the deviation of the deviation angle of the c-axis 10ca of the base substrate 10.
[0117] (S500: grinding process)
[0118] Next, both surfaces of the substrate 50 are polished by a polishing device. In this case, the thickness of the final substrate 50 is set to, for example, 250 μm or more and 650 μm or less.
[0119] Through the above steps, the substrate 50 of the present embodiment is manufactured.
[0120] (Process for producing a semiconductor stack and process for producing a semiconductor device)
[0121] After manufacturing the substrate 50, for example, a semiconductor functional layer composed of a group III nitride semiconductor may be epitaxially grown on the substrate 50 to produce a semiconductor stack. After producing the semiconductor stack, electrodes are further formed on the semiconductor stack, and the semiconductor stack is cut to cut out chips of a specified size. Thus, a semiconductor device may also be produced. By reducing the dislocations that have accumulated large strains on the surface of the substrate 50, the characteristics of the semiconductor device (device) produced on the substrate 50 can be improved.
[0122] (2) Gallium nitride single crystal substrate (nitride semiconductor self-supporting substrate, nitride crystal substrate)
[0123] Next, the gallium nitride single crystal substrate 50 according to the present embodiment will be described.
[0124] In the present embodiment, the substrate 50 obtained by the above-described manufacturing method is a self-supporting substrate composed of a GaN single crystal.
[0125] The diameter of the substrate 50 is, for example, not less than 50 mm. The thickness of the substrate 50 is, for example, not less than 300 μm and not more than 1 mm.
[0126] The conductivity of the substrate 50 is not particularly limited. However, when the substrate 50 is used to manufacture a semiconductor device as a vertical Schottky barrier diode (SBD), the substrate 50 is, for example, an n-type, and the n-type impurity in the substrate 50 is, for example, Si or germanium (Ge), and the n-type impurity concentration in the substrate 50 is, for example, 1.0×10 18 cm -3 Above and 1.0×10 20 cm -3 the following.
[0127] The substrate 50 has, for example, a principal surface 50s that serves as an epitaxial growth surface. In the present embodiment, the low-index crystal plane closest to the principal surface 50s is, for example, the c-plane 50c.
[0128] It should be noted that the main surface 50 s of the substrate 50 is, for example, mirror-finished, and the root mean square roughness RMS of the main surface 50 s of the substrate 50 is, for example, less than 1 nm.
[0129] In addition, in the present embodiment, the impurity concentration in the substrate 50 obtained by the above-mentioned manufacturing method is lower than that of a substrate obtained by a flux method, an ammonothermal method, or the like.
[0130] Specifically, the hydrogen concentration in the substrate 50 is, for example, less than 1×10 17 cm -3 , preferably 5×10 16 cm -3 the following.
[0131] In addition, in this embodiment, the substrate 50 is formed by slicing the main growth layer 44 grown with the c-plane 40c as the growth plane, and therefore does not include the inclined interface growth region 70 grown with the inclined interface 30i or the inclined interface 40i as the growth plane. That is, the entire substrate 50 is composed of a low oxygen concentration region.
[0132] Specifically, the oxygen concentration in the substrate 50 is, for example, 5×10 16 cm -3 Below, preferably 3×10 16 cm -3 the following.
[0133] (c-plane curvature and deviation of the off angle)
[0134] In the present embodiment, the curvature radius of the c-plane 50 c of the substrate 50 is, for example, larger than the curvature radius of the c-plane 10 c of the base substrate 10 used in the above-described method of manufacturing the substrate 50 .
[0135] Specifically, the radius of curvature of the c-plane 50 c of the substrate 50 is, for example, not less than 23 m, preferably not less than 30 m, and more preferably not less than 40 m.
[0136] In the present embodiment, the upper limit of the curvature radius of the c-plane 50c of the substrate 50 is preferably as large as possible, and is therefore not particularly limited. When the c-plane 50c of the substrate 50 is substantially flat, the curvature radius of the c-plane 50c may be considered to be infinite.
[0137] In this embodiment, since the curvature radius of the c-plane 50c of the substrate 50 is large, the deviation of the off angle θ of the c-axis 50ca with respect to the normal line of the principal surface 50s of the substrate 50 can be made smaller than the deviation of the off angle of the c-axis 10ca of the base substrate 10.
[0138] Specifically, when the X-ray rocking curve of the (0002) surface of the substrate 50 is measured and the deviation angle θ of the c-axis 50ca relative to the normal of the main surface 50s is measured based on the diffraction peak angle of the (0002) surface, the deviation calculated based on the extreme difference of the deviation angle θ from the center of the main surface 50s to the diameter of 29.6 mm is, for example, less than 0.075°, preferably less than 0.057°, and more preferably less than 0.043°.
[0139] In this embodiment, the lower limit of the deviation of the off angle θ of the c-axis 50ca of the substrate 50 is preferably as small as possible, and is not particularly limited. When the c-surface 50c of the substrate 50 is substantially flat, the deviation of the off angle θ of the c-axis 50ca of the substrate 50 may be 0°.
[0140] In addition, in the present embodiment, since the curvature of the c-plane 50 c is isotropically reduced with respect to the principal surface 50 s of the substrate 50 , the direction dependence of the radius of curvature of the c-plane 50 c is small.
[0141] Specifically, the difference between the curvature radius of the c-plane 50c along the a-axis and the curvature radius of the c-plane 50c along the m-axis obtained by the above-mentioned measurement method is, for example, less than 50% of the larger curvature radius, preferably less than 20%.
[0142] (Dislocation density)
[0143] In this embodiment, the above-described manufacturing method reduces the dislocation density on the surface of the second layer 40 compared to the dislocation density on the main surface 10s of the base substrate 10. Thus, dislocations are also reduced on the main surface 50s of the substrate 50 formed by slicing the second layer 40.
[0144] When the substrate 50 is manufactured using only the base substrate 10 composed of a high-purity GaN single crystal produced by the VAS method, the number of non-luminescent centers caused by foreign matter or point defects in the substrate 50 is small.
[0145] Therefore, when observing the main surface of the substrate 50 of the present application using a multiphoton excitation microscope, more than 95% (preferably more than 99%) of the dark spots observed are not non-luminescent centers caused by foreign matter or point defects, but correspond to dislocations. It should be noted that "multiphoton excitation microscope" is sometimes also called a two-photon excitation fluorescence microscope.
[0146] In the present embodiment, a region having a particularly high dislocation density due to concentration of dislocations is not formed, but a region having a low dislocation density is uniformly formed.
[0147] Specifically, in this embodiment, when the main surface 50s of the substrate 50 is observed in a 250 μm square field of view using a multiphoton excitation microscope and the dislocation density is obtained from the dark spot density, there is no dislocation density exceeding 1×10 6 cm -2 The dislocation density is less than 5×10 5 cm -2 The region exists in 80% or more of the main surface 50s, preferably exists in 90% or more, and more preferably exists in 95% or more.
[0148] In other words, in the present embodiment, the average dislocation density of the entire principal surface 50s of the substrate 50 is less than 1×10 6 cm -2 , preferably less than 5.5×10 5 cm -2 , more preferably 3×10 5 cm -2 the following.
[0149] (Erosion pit histogram)
[0150] When the main surface 50s of the substrate 50 is etched with an alkaline etching solution, a Figure 5The etching pits are as shown. In the present embodiment, the substrate 50 is immersed in a melt (temperature 470°C) in which potassium hydroxide (KOH) and sodium hydroxide (NaOH) are mixed at a ratio of 1:1 for 20 minutes and then etched. Then, the main surface 50s of the etched substrate 50 is observed using SEM, and the diameter of each etching pit is calculated by image analysis. A histogram of the diameter of the etching pit is prepared based on the data of the diameter of the etching pit obtained. It should be noted that the diameter of the etching pit can be the maximum diameter of each etching pit area obtained by image analysis, or it can be the equivalent circle diameter. In the present embodiment, the diameter of the peak that appears on the side with the smallest diameter among the peaks that appear in the histogram of the diameter of the etching pit (hereinafter also referred to as the first peak) is set to a and standardized, and the level (scale width) of the horizontal axis is set to 0.1a scale. The vertical axis is the number (frequency) of etching pits in the measurement area.
[0151] The density of the pits formed when etching is performed on the main surface 50s of the substrate 50 of the present embodiment under the above-mentioned conditions (the number of pits per unit area) is approximately equivalent to the dislocation density. The size of the pits can vary depending on the etching conditions, but if the pits are present at too high a density, adjacent pits overlap each other, making it difficult to measure the diameter of the pits. Therefore, in order to make meaningful measurements, the density of the pits is preferably less than 1×10 6 cm -2 , more preferably less than 5.5×10 5 cm -2 , more preferably 3×10 5 cm -2 It should be noted that the histogram of the density of the pits and the diameter of the pits is preferably based on an area of 1 mm 2 The above area is measured.
[0152] For the substrate 50 of the present embodiment, when the diameter of the first peak is set to a, the total number (total number) of pits with a diameter exceeding 4a is less than 1 / 1000 of the number of pits constituting the first peak. This can be said to mean that there are actually no pits with a diameter exceeding 4a, but sometimes larger pits are formed due to damage or foreign matter on the substrate 50, so it is expressed as less than 1 / 1000. For such a substrate 50, it can be said that there are substantially no dislocations that accumulate large strains that deteriorate device characteristics. Therefore, the characteristics of the device manufactured on the substrate 50 can be improved.
[0153] For the substrate 50 of the present embodiment, the total number of etch pits with a diameter of 2a or more is preferably 1 / 10 or less of the number of etch pits constituting the first peak, and more preferably 1 / 100 or less. The etch pits with a diameter of 2a or more may correspond to dislocations that affect the device characteristics of the substrate 50, so by making the total number of etch pits with a diameter of 2a or more 1 / 10 or less (more preferably 1 / 100 or less) of the number of etch pits constituting the first peak, the device characteristics manufactured on the substrate 50 can be improved.
[0154] For the substrate 50 of this embodiment, the number of etch pits constituting the first peak is preferably more than 50% of the total (more preferably more than 70%). As described above, in the first step S200, by doping Ge at a high concentration into the inclined interface growth region 70, the existence ratio of dislocations with a smaller strain field can be increased, thereby increasing the number of etch pits constituting the first peak. Dislocations with a smaller strain field will not have a significant impact on the device characteristics of the substrate 50, so a higher proportion of etch pits constituting the first peak means that the device characteristics made on the substrate 50 are good.
[0155] For the substrate 50 of the present embodiment, when the frequency of the first peak is set to A, the peaks appearing in the histogram of the diameter with a frequency of A / 10 or more are preferably two, including the first peak. The number of peaks appearing in the histogram of the pits can be said to correspond to the number of constituent types of dislocation defects corresponding to the pits. For the crystals in which multiple peaks are observed, in addition to simple edge-shaped and mixed dislocations, there are more deformations of impurities or point defects combined with them in a complex manner, that is, it is a crystal with a high possibility of generating more impurity energy levels or defect energy levels, and the deviation of characteristics when manufacturing devices is large. In other words, it can be said that it is a crystal with a high possibility of poor device yield. In contrast, for the crystals in which the peaks appearing in the histogram with a frequency of A / 10 or more are two, including the first peak, it is taught that the dislocations present in the crystal are only simple edge-shaped dislocations and mixed dislocations, that is, the deviation of characteristics when manufacturing devices is small, and it can be said that it is a crystal with a good device yield.
[0156] In addition, for the substrate 50 of the present embodiment, the second peak is present in the range of a diameter exceeding a and less than 2a, and the number of pits constituting the second peak is preferably less than the number of pits constituting the first peak. The diameter of the pits forming the second peak in the range of a diameter exceeding a and less than 2a means that it is highly likely to correspond to a simple mixed dislocation, and the small number of pits constituting the second peak, in other words, the large number of pits constituting the first peak, indicates that the dislocations in the crystal are mainly composed of dislocations with less strain around the dislocation core. These characteristics mean that the device characteristics manufactured on the substrate 50 are good.
[0157] <Other Implementation Methods>
[0158] The embodiments of the present invention have been described in detail above, but the present invention is not limited to the above-described embodiments, and various modifications can be made without departing from the gist of the present invention.
[0159] In the above-mentioned embodiment, the case where the base substrate 10 is a commercially available gallium nitride single crystal substrate or a GaN self-supporting substrate produced by the VAS method is described, but the base substrate 10 is not limited to a GaN self-supporting substrate produced by the VAS method, for example, it can also be a GaN self-supporting substrate produced by other methods.
[0160] In the above embodiment, the substrate 50 is mainly described as being of n-type, but the substrate 50 may be of p-type or have semi-insulating properties. For example, when a semiconductor device as a high electron mobility transistor (HEMT) is manufactured using the substrate 50, it is preferred that the substrate 50 has semi-insulating properties.
[0161] In the above-described embodiment, the case where the growth temperature is mainly adjusted as the first growth condition in the first step S200 is described. However, growth conditions other than the growth temperature may be adjusted, or the growth temperature and growth conditions other than the growth temperature may be adjusted in combination.
[0162] In the above-described embodiment, the case where the growth temperature is mainly adjusted as the second growth condition in the second step S300 is described. However, growth conditions other than the growth temperature may be adjusted, or the growth temperature and growth conditions other than the growth temperature may be adjusted in combination.
[0163] In the above-mentioned embodiment, the case where the growth condition in the inclined interface maintaining process S240 is maintained with the above-mentioned first growth condition in the same manner as the inclined interface expansion process S220 is described, but if the growth condition in the inclined interface maintaining process S240 satisfies the first growth condition, the growth condition in the inclined interface maintaining process S240 may also be different from the growth condition in the inclined interface expansion process S220.
[0164] In the above-mentioned embodiment, the case where the growth conditions in the main growth process S340 are maintained with the above-mentioned second growth conditions in the same way as the c-plane expansion process S320 is described, but if the growth conditions in the main growth process S340 satisfy the second growth conditions, the growth conditions in the main growth process S340 can also be made different from the growth conditions in the c-plane expansion process S320.
[0165] In the above-described embodiment, the case where the main growth layer 44 is sliced using a wire saw in the slicing step S400 is described. However, for example, an outer peripheral blade slicer, an inner peripheral blade slicer, an electric discharge machine, or the like may be used.
[0166] In the above-mentioned embodiment, the case where the manufacturing process is terminated after the substrate 50 is manufactured is described, but the substrate 50 may be used as the base substrate 10 and the processes S200 to S500 may be performed again. Thus, the substrate 50 with a further reduced dislocation density can be obtained. In addition, the substrate 50 with a further reduced deviation of the deviation angle θ of the c-axis 50ca can be obtained. In addition, the substrate 50 with a further reduced dislocation that has accumulated a large strain can be obtained. In addition, the processes S200 to S500 using the substrate 50 as the base substrate 10 may be regarded as one cycle and the cycle may be repeated multiple times. Thus, the dislocation density of the substrate 50 may be gradually reduced corresponding to the number of repeated cycles. In addition, the deviation of the deviation angle θ of the c-axis 50ca in the substrate 50 may be gradually reduced corresponding to the number of repeated cycles. In addition, the substrate 50 with a reduced dislocation that has accumulated a large strain corresponding to the number of repeated cycles can be obtained.
[0167] [Example]
[0168] Next, examples of the present invention will be described. These examples are examples of the present invention, and the present invention is not limited to these examples.
[0169] (1) Fabrication of GaN single crystal substrate
[0170] Gallium nitride single crystal substrates of Example 1, Example 2, and Comparative Example were produced as follows.
[0171] [Conditions for producing the gallium nitride single crystal substrate of Example 1] (Base substrate)
[0172] Material: GaN
[0173] Production method: VAS method
[0174] Diameter: 2 inches
[0175] Thickness: 400μm
[0176] The closest low-index crystal plane to the main plane: c-plane
[0177] There is no patterning such as mask layer on the main surface.
[0178] Root mean square roughness of the main surface RMS: 2nm
[0179] Deviation angle of the main surface: 0.4° in the m direction
[0180] FWHM of (10-10) plane diffraction in XRC measurement: 100 arcsec (first layer)
[0181] Material: GaN
[0182] Growth method: HVPE method
[0183] First growth condition:
[0184] The growth temperature was set to 980° C. or higher and 1020° C. or lower, and the V / III ratio was set to 2 or higher and 20 or lower. Furthermore, Ge was doped into the inclined interface growth region under the following conditions.
[0185] Ge doping method: GeCl4 gas
[0186] Partial pressure of GeCl4 gas: 0.35Pa
[0187] Ge concentration in the tilted interface growth region: 5×10 18 cm -3
[0188] Thickness from the main surface of the base substrate to the surface of the first layer: 1 mm (second layer)
[0189] Material: GaN
[0190] Growth method: HVPE method
[0191] Second growth condition:
[0192] The growth temperature is set to 1050° C. to 1080° C., and the V / III ratio is set to 2 to 5. Ge is not doped in the c-plane expansion step S320 , and Ge is doped in the main growth step S340 to achieve the following c-plane Ge concentration.
[0193] Thickness from the main surface of the base substrate to the surface of the second layer: 2 mm
[0194] Ge concentration on c-plane: 3×10 19 cm -3
[0195] It should be noted that when the Ge concentration of each layer changes from the first layer to the second layer, the Ge concentration difference of each layer is adjusted to 1×10 18 cm -3 the following.
[0196] (Slicing conditions)
[0197] Thickness of GaN single crystal substrate: 400μm
[0198] Kerf loss: 200μm
[0199] [Conditions for fabricating gallium nitride single crystal substrate of Example 2] (Base substrate)
[0200] Same as Example 1.
[0201] (First floor)
[0202] Ge concentration in the tilted interface growth region: 5×10 19 cm -3
[0203] The above-mentioned aspects are the same as those of Example 1.
[0204] (Second floor)
[0205] In the c-plane expansion step S320, the Ge concentration of the inclined interface 40i is 5×10 19 cm -3 Ge is doped in the manner of.
[0206] The above-mentioned aspects are the same as those of Example 1.
[0207] (Slicing conditions)
[0208] Same as Example 1.
[0209] [Production Conditions of Gallium Nitride Single Crystal Substrate of Comparative Example] (Base Substrate)
[0210] Same as Example 1.
[0211] (First floor)
[0212] The process is the same as Example 1 except that Ge doping is not performed.
[0213] (Second floor)
[0214] Same as Example 1.
[0215] (Slicing conditions)
[0216] Same as Example 1.
[0217] (2) Evaluation of the pit histogram
[0218] The main surfaces of the gallium nitride single crystal substrates of Example 1, Example 2, and Comparative Example were etched with an alkaline etching solution under the following conditions to form etch pits.
[0219] Etching solution: Alkaline solution consisting of 500g KOH and 500g NaOH
[0220] Melt temperature: 470℃
[0221] Soaking time: 20 minutes
[0222] The main surface of the gallium nitride single crystal substrate with etch pits was observed using SEM (manufactured by Hitachi High-Technologies Corporation, SU5000). The measurement field of view was set to 127μm×95.3μm (magnification 1000 times), and the image (1143μm×1048μm) formed by combining 9 horizontal × 11 vertical SEM images (99 in total) was analyzed to measure the etch pits. Specifically, the image was binarized using image processing software (Image J), the etch pit area was filled, and the larger of the width and height of the etch pit area was calculated as the diameter of the etch pit. It should be noted that when filling the etch pit area, areas representing smaller garbage or linear pit areas caused by processing damage, etc. were removed.
[0223] A histogram of the diameter of the pits was prepared based on the data of the diameter of the pits obtained. In this embodiment, the diameter of the peak (first peak) appearing on the side with the smallest diameter among the peaks appearing in the histogram of the diameter of the pits was set to 1 and standardized, and the level of the horizontal axis was set to 0.1 scale.
[0224] exist Fig. 6A , Figure 6B The histograms of Example 1 are shown in Fig. 7A , Figure 7B The histograms of Example 2 are shown in FIG. Figure 8B The histograms of the comparative examples are shown in FIG. Fig. 6A , Figure 6B , Fig. 7A , Figure 7B , Figure gA, Figure 8B In the figure, the horizontal axis represents the standardized pit diameter, and the vertical axis represents the number (frequency) of pits in the measurement area. Figure 6B , Figure 7B , Figure 8B are respectively Fig. 6A , Fig. 7A , and the histogram of Figure gA is enlarged in the vertical axis (frequency) direction. In addition, Table 1 also shows the number of pits constituting the first peak, the number of pits with a diameter less than 2, the number of pits with a diameter of 2 or more and less than 4, and the number of pits with a diameter of 4 or more observed in the histograms of Example 1, Example 2, and Comparative Example.
[0225]
Table 1
[0226] First Peak Diameter less than 2 The diameter is greater than 2 and less than 4 Diameter 4 or more Example 1 3890 6232 350 2 Example 2 3582 5602 22 0 Comparative Example 4192 6071 386 49
[0227] like Fig. 8A , Figure 8B As shown in Table 1, in the substrate of the comparative example in which Ge was not doped into the first layer (tilted interface growth region), a small number of etch pits with a diameter exceeding 4 were measured. Fig. 6A , Figure 6B , Fig. 7A , Figure 7B As shown in Table 1, in the substrates of Example 1 and Example 2 in which Ge was highly doped in the inclined interface growth region, essentially no pits with a diameter exceeding 4 were measured (the total number of pits with a diameter exceeding 4 was less than 1 / 1000 of the number of pits constituting the first peak).
[0228] As described above, it was confirmed that by doping the first layer (inclined interface growth region) with Ge at a high concentration, when the diameter of the first peak in the histogram of the pit diameter is set to a, the total number of pits with a diameter exceeding 4a can be reduced (can be less than 1 / 1000 of the number of pits constituting the first peak). In other words, for the gallium nitride single crystal substrates of Examples 1 and 2, it can be said that there are substantially no dislocations that accumulate large strains that cause deterioration of device characteristics, and thus the device characteristics can be improved.
[0229] In addition, as shown in Table 1, in the substrate of Example 1, the number of pits constituting the first peak was 3890, and the total number of pits with a diameter of 2 or more was 352. That is, it was confirmed that in the substrate of Example 1, the total number of pits with a diameter of 2 or more was less than 1 / 10 of the number of pits constituting the first peak. In the substrate of Example 2, the number of pits constituting the first peak was 3582, and the total number of pits with a diameter of 2 or more was 22. That is, it was confirmed that in the substrate of Example 2, the total number of pits with a diameter of 2 or more was less than 1 / 100 of the number of pits constituting the first peak. On the other hand, in the substrate of the comparative example, the total number of pits constituting the first peak was 4192, and the total number of pits with a diameter of 2 or more was 435.
[0230] In addition, the number of etch pits constituting the first peak in the substrate of Example 1 was 59% of the total, and the number of etch pits constituting the first peak in the substrate of Example 2 was 64% of the total. In other words, it was confirmed that the number of etch pits constituting the first peak in the substrates of Examples 1 and 2 was more than 50% of the total.
[0231] In addition, according to Fig. 6A , Fig. 7A It was confirmed that in the substrates of Examples 1 and 2, when the frequency of the first peak was set to A, there were two peaks including the first peak appearing in the histogram of the diameter with a frequency of A / 10 or more.
[0232] In addition, according to Fig. 6A , Fig. 7A It was confirmed that in the substrates of Examples 1 and 2, there was a second peak in the range of diameter greater than 1 and less than 2, and the number of etch pits constituting the second peak was less than the number of etch pits constituting the first peak.
[0233] <Preferred embodiment of the present invention>
[0234] Preferred embodiments of the present invention are described below.
[0235] (Note 1)
[0236] A gallium nitride single crystal substrate having a diameter of 50 mm or more, wherein the low-index crystal plane closest to the main surface is the (0001) plane, wherein:
[0237] The density of the etch pits formed when the main surface is etched with an alkaline etching solution is less than 1×10 6 cm -2 ,
[0238] When the diameter of the first peak appearing on the smallest side among the peaks appearing in the histogram of the pit diameters is defined as a, the total number of pits having a diameter exceeding 4a is less than 1 / 1000 of the number of pits constituting the first peak.
[0239] (Note 2)
[0240] The gallium nitride single crystal substrate according to Supplementary Note 1, wherein the total number of etch pits having a diameter of 2a or more is 1 / 10 or less of the number of etch pits constituting the first peak.
[0241] More preferably, the total number of etch pits having a diameter of 2a or more is 1 / 100 or less of the number of etch pits constituting the first peak.
[0242] (Note 3)
[0243] The gallium nitride single crystal substrate according to Supplementary Note 1, wherein the number of etch pits constituting the first peak accounts for more than 50% of the total.
[0244] More preferably, the number of the etch pits constituting the first peak accounts for 70% or more of the total.
[0245] (Note 4)
[0246] According to the gallium nitride single crystal substrate described in Supplementary Note 1, when the frequency of the first peak is set to A, there are two peaks appearing in the histogram with a frequency of A / 10 or more, including the first peak.
[0247] (Note 5)
[0248] The gallium nitride single crystal substrate according to Supplementary Note 1, wherein the second peak is present within a range where the diameter exceeds a and is less than 2a, and the number of etch pits constituting the second peak is smaller than the number of etch pits constituting the first peak.
[0249] (Note 6)
[0250] According to any one of Notes 1 to 5, the gallium nitride single crystal substrate, wherein the density and histogram of the etch pits are based on an area of 1 mm 2 The above area is measured.
Claims
1. A gallium nitride single crystal substrate having a diameter of 50 mm or more, wherein the low-index crystal plane closest to the main surface is the (0001) plane, wherein: The density of the etch pits formed when the main surface is etched with an alkaline etching solution is less than 1×10 6 cm -2 , When the diameter of the first peak appearing on the smallest side among the peaks appearing in the histogram of the pit diameters is defined as a, the total number of pits having a diameter exceeding 4a is less than 1 / 1000 of the number of pits constituting the first peak.
2. The gallium nitride single crystal substrate according to claim 1, wherein: The total number of pits having a diameter of 2a or more is 1 / 10 or less of the number of pits constituting the first peak.
3. The gallium nitride single crystal substrate according to claim 1, wherein: The number of the etch pits constituting the first peak accounts for more than 50% of the total.
4. The gallium nitride single crystal substrate according to claim 1, wherein: When the frequency of the first peak is set to A, there are two peaks appearing in the histogram with a frequency of A / 10 or more, including the first peak.
5. The gallium nitride single crystal substrate according to claim 1, wherein: There is a second peak in the range where the diameter exceeds a and is smaller than 2a, and the number of pits constituting the second peak is smaller than the number of pits constituting the first peak.
6. The gallium nitride single crystal substrate according to any one of claims 1 to 5, wherein The density and histogram of the pits are based on an area of 1 mm 2 The above area is measured.