Preparation method and application of CdTe-based semiconductor crystal

The preparation of CdTe-based semiconductor crystals through an electric field-assisted vacuum tube furnace method solves the problem of high temperature and high energy consumption in traditional methods, realizes efficient and low-cost crystal preparation, and improves material performance and production efficiency.

CN118932491APending Publication Date: 2024-11-12CHANGAN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411035101.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The traditional CdTe-based semiconductor crystal preparation method requires high temperature conditions, resulting in high energy consumption, high production costs and low resource utilization, which cannot meet the efficient and low-consumption production requirements of modern industry.

Method used

Using the electric field-assisted vacuum tube furnace method, a cylindrical blank is formed by uniaxial pressing, and the furnace is controlled to apply an electric field in a vacuum environment for flash burning, shortening the crystal growth time, improving the relative density and component purity, reducing the high-temperature exposure time and Loss of element volatility.

Benefits of technology

It improves the growth rate and relative density of crystals, reduces pores and defects, reduces production costs, improves material performance and production efficiency, and is suitable for the manufacture of high-purity and high-density semiconductor crystal materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932491A_ABST
    Figure CN118932491A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and application of a CdTe-based semiconductor crystal, and the preparation method comprises the following steps: firstly, weighing a certain mass of CdTe-based powder by using an analytical balance, and carrying out uniaxial pressing on the powder in a mold to form a cylindrical green body; and secondly, placing the cylindrical blank in a vacuum tube furnace, carrying out flash burning by controlling the furnace temperature and applying an electric field, keeping for a certain time under a preset current, and turning off a power supply to obtain the CdTe-based semiconductor crystal. According to the method, the growth speed of crystals in the sintering process is increased by utilizing the characteristic of rapid mass transfer of substances within a short time under the auxiliary condition of an electric field. In the sintering process, the activation energy can be effectively reduced under the action of an electric field, so that crystal grains can move and combine more quickly, and the time required by crystal growth is shortened. Meanwhile, the required sintering temperature can be quickly reached within a short time, and the time of crystal exposure at a high temperature is shortened, so that the volatilization loss of volatile substances and elements in a compound system is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of compound semiconductor material preparation, and in particular, relates to a preparation method and application of a CdTe-based semiconductor crystal. Background Art

[0002] X-ray and gamma-ray detectors, also known as nuclear radiation detectors, play a vital role in many key areas, including medical imaging, environmental protection, industrial monitoring, nuclear safety testing, and astrophysics research. These detectors can accurately detect and analyze nuclear radiation, providing important protection for scientific research and public safety.

[0003] Among the many materials that can be used for nuclear radiation detection, CdTe-based compound semiconductors stand out due to their excellent properties. First, CdTe-based compounds have a large bandgap, which enables them to effectively detect high-energy radiation. Secondly, its high resistivity ensures that the dark current generated during the detection process is low, thereby improving the signal-to-noise ratio of the detector. In addition, the large carrier mobility and lifetime product of CdTe-based materials means that more electrical signals can be generated during radiation detection, improving the sensitivity and response speed of the detector. More importantly, CdTe-based semiconductors can operate at room temperature without the need for additional cooling devices, which greatly simplifies the design and use of detectors.

[0004] However, the traditional methods for preparing CdTe-based semiconductor crystals are mainly melt method and solution method. Although these two methods can produce high-quality crystals, they have obvious disadvantages. First, these methods need to be carried out under high temperature conditions, and the energy consumption is very high, resulting in high production costs. Secondly, due to the complex process, the energy efficiency in the preparation process is low, and the resource utilization rate is not high, which does not meet the requirements of modern industry for efficient and low-consumption production methods.

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a method for preparing a CdTe-based semiconductor crystal, thereby solving the problems raised in the above-mentioned background technology.

[0007] In order to solve the above technical problems, the basic concept of the technical solution adopted by the present invention is: A method for preparing a CdTe-based semiconductor crystal and its application, comprising the following steps: Step (1), using an analytical balance to weigh a certain mass of CdTe-based powder, and uniaxially pressing the powder in a mold to form a cylindrical body; Step (2), placing the cylindrical body in a vacuum tube furnace, controlling the furnace temperature and applying an electric field for flash burning, maintaining the current at a preset current for a certain period of time and then turning off the power supply to obtain a CdTe-based semiconductor crystal; Step (3), surface treatment is performed on the CdTe-based semiconductor crystal obtained by flash calcination, so as to obtain a CdTe-based semiconductor crystal with a smooth surface.

[0008] Optionally, in step (1), the mass of the CdTe-based powder is weighed to be 100 to 300 mg, the thickness of the cylindrical body is 1 to 1.4 mm, the diameter is 5 to 10 mm, and the uniaxial pressure is 6 to 10 MPa.

[0009] Optionally, the CdTe-based semiconductor material includes three types of CdTe, CdZnTe and CdMnTe, with a stoichiometric ratio of CdTe, Cd 0.9 Zn 0.1 Te and Cd 0.9 Mn 0.1 High purity (5N) Te powder is used as raw material.

[0010] Optionally, before placing the cylindrical blank in the vacuum tube furnace in step (2), the cylindrical blank needs to be connected in series to the circuit.

[0011] Optionally, the step of obtaining the CdTe-based semiconductor crystal in step (2) is: Step (2.1) After placing the cylindrical blank in a vacuum tube furnace, the furnace temperature of the vacuum tube furnace is increased at a rate of 5°C to 10°C / min to a temperature required for flash burning; Step (2.2) applies a preset constant electric field to the cylindrical blank during the heating process until flash burning occurs; After flash burning occurs in step (2.3), the power supply is changed from a constant voltage state to a constant current state. After maintaining the current density for a certain period of time, the power supply and the heating furnace are turned off and the temperature is lowered to room temperature.

[0012] Optional, vacuum tube furnace with vacuum degree of 10 ~3 Pa~10 ~4 Pa, temperature is 390~590℃.

[0013] Optionally, the electric field strength is 200V / cm to 600V / cm, and the current density is 30mA / cm 2 ~70mA / cm 2 The flash burning time is 20s to 60s, and the cooling method is cooling with the furnace.

[0014] Optionally, step (3) performs surface treatment on the CdTe-based semiconductor crystal obtained by flash calcination: Step (3.1): Use 2000-grit sandpaper to polish both sides of the CdTe-based semiconductor crystal for 2 minutes each to remove the carbon that has penetrated into the crystal surface; Step (3.2): Use 7000 grit sandpaper to polish both sides of the crystal for 5 minutes each to remove the scratches for the first time; Step (3.3): Use a polishing solution prepared with MgO powder to polish both sides of the crystal for 5 minutes each to eliminate scratches for the second time; Step (3.4): The polished CdTe-based semiconductor crystal is washed with deionized water and then blown dry with nitrogen to complete the surface treatment.

[0015] A CdTe-based semiconductor ceramic prepared by the above preparation method is used to prepare a room temperature radiation X-ray detector After adopting the above technical solution, the present invention has the following beneficial effects compared with the prior art. Of course, any product implementing the present invention does not necessarily need to achieve all the advantages described below at the same time: The present invention utilizes the characteristics of rapid mass transfer in a short time under electric field assisted conditions to accelerate the growth rate of crystals during sintering. During the sintering process, the action of the electric field can effectively reduce the activation energy, so that the grains can move and combine more quickly, thereby shortening the time required for crystal growth. At the same time, the required sintering temperature can be quickly reached in a short time, reducing the exposure time of the crystals at high temperatures, thereby reducing the volatilization loss of volatile substances and elements in the compound system.

[0016] This method can not only ensure that the composition of the crystal is closer to the stoichiometric ratio and avoid composition deviation caused by element volatilization, but also improve the relative density of the crystal and reduce the pores and defects inside the crystal. By optimizing the electric field intensity and heating rate, the present invention can greatly improve the growth rate and relative density of the crystal while ensuring the quality of the crystal, thereby improving production efficiency and reducing production costs. This method is particularly suitable for manufacturing semiconductor crystal materials that require high purity and high density, such as CdTe-based semiconductor crystals, and has important industrial application value while improving material performance.

[0017] The specific implementation modes of the present invention are further described in detail below with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] The drawings described below are only some embodiments. For those skilled in the art, other drawings can be obtained based on these drawings without creative work. In the drawings: Figure 1 For CdTe, Cd in Examples 1, 2, and 3 0.9 Zn 0.1 Te, Cd 0.9 Mn0.1 Scanning electron microscope (SEM) image of the cross section of Te sample; Figure 2 is Cd in Example 2 0.9 Zn 0.1 Test results of electrical properties (I~V) of Te samples; Figure 3 is Cd in Example 2 0.9 Zn 0.1 Test results of X-ray room temperature radiation detector prepared from Te samples.

[0019] It should be noted that these drawings and textual descriptions are not intended to limit the conceptual scope of the present invention in any way, but are intended to illustrate the concept of the present invention for those skilled in the art by referring to specific embodiments. DETAILED DESCRIPTION

[0020] The present invention will now be described in further detail with reference to the accompanying drawings.

[0021] Embodiment 1: A flash preparation method of CdTe semiconductor crystals, comprising the following steps: Step (1): 140 mg of CdTe powder was weighed using an analytical balance, and the powder was uniaxially pressed in a stainless steel mold with a diameter of 5 mm at a pressure of 6 MPa to form a cylindrical body with a thickness of 1.4 mm; Step (2): Set the vacuum degree to 10 ~3 The furnace temperature of the vacuum tube furnace of Pa was raised to the required temperature for flash burning at a rate of 5℃ / min in vacuum. During the heating process, a preset constant electric field was applied to the cylindrical blank until flash burning occurred, and a flash burning experiment was performed. After flash burning occurred, the power was turned off after maintaining the preset current for a certain period of time. The sample was cooled with the furnace to obtain a CdTe semiconductor crystal. It should be noted that during the flash process, the electric field strength is 300V and the current density is 50mA / mm 2 , furnace temperature is 440℃, flash time is 30s; Step (3): Grind and polish both sides of the CdTe semiconductor crystal prepared by flash sintering with 2000-grit sandpaper for 2 minutes each to remove the carbon that has penetrated into the surface of the crystal. Then use 7000-grit sandpaper to polish both sides of the crystal for 5 minutes each to remove some scratches. Finally, use a polishing liquid prepared with MgO powder to polish both sides of the crystal for 5 minutes each to remove most scratches. After the crystal is washed with deionized water and dried with nitrogen, a room temperature radiation X-ray detector is prepared.

[0022] Figure 1(a) is a scanning electron microscope (SEM) photo of the cross section of the CdTe sample obtained in this example. It can be seen that the CdTe crystal flashed for 30 seconds under the assistance of the electric field is very dense, with a relative density of 96.8%.

[0023] Example 2: Cd 0.9 Zn 0.1 The flash preparation method of Te semiconductor crystal comprises the following steps: Step (1): Weigh 200 mg of Cd using an analytical balance 0.9 Zn 0.1 Te powder was uniaxially pressed in a stainless steel mold with a diameter of 10 mm under a pressure of 8 MPa to form a cylindrical green body with a thickness of 1 mm; Step (2): Set the vacuum degree to 10 ~3 The furnace temperature of the vacuum tube furnace of Pa was raised to the required temperature for flash burning at a rate of 10℃ / min in vacuum. During the heating process, a preset constant electric field was applied to the cylindrical blank until flash burning occurred, and a flash burning experiment was performed. After flash burning occurred, the power supply was turned off after maintaining the preset current for a certain period of time. The sample cooled with the furnace to obtain Cd 0.9 Zn 0.1 Te semiconductor crystal.

[0024] It should be noted that during the flash burning process, the electric field strength was set to 300V and the current density was set to 50mA / mm 2 , the furnace temperature is 460℃ and the flash time is 50s.

[0025] Step (3): Flash-sinter the Cd 0.9 Zn 0.1 The two sides of the Te semiconductor crystal were polished with 2000-grit sandpaper for 2 minutes each to remove the carbon that penetrated into the crystal surface. Then, the two sides of the crystal were polished with 7000-grit sandpaper for 5 minutes each to eliminate some scratches. Finally, the two sides of the crystal were polished with a polishing liquid prepared with MgO powder for 5 minutes each to eliminate most scratches. The crystal was washed with deionized water and dried with nitrogen to prepare a room temperature radiation X-ray detector.

[0026] Figure 1 (b) is the Cd obtained in this example 0.9 Zn 0.1 Scanning electron microscope (SEM) photo of the cross section of the Te sample. It can be seen that the Cd flashed for 50s under the assistance of electric field 0.9 Zn 0.1 Te crystals are already very dense, with a relative density of 98.6%. Figure 2 In this embodiment, Cd 0.9 Zn 0.1The electrical properties (I~V) test results of the Te sample show that the resistivity of the crystal is 1.12×10 10 Ω·cm. Figure 3 In this embodiment, Cd 0.9 Zn 0.1 Test results of TeX-ray room temperature radiation detector. Under different doses, the detector dark current is low ( Figure 3 (a)), at 20 kVp tube voltage, the sensitivity and detection limit of the detector are 6.86 μC·Gy air ~1 cm ~2 and 2.21 μGy air s ~1 .

[0027] Example 3: Cd 0.9 Mn 0.1 The flash preparation method of Te semiconductor crystal comprises the following steps: Step (1): Weigh 100 mg of Cd using an analytical balance 0.9 Mn 0.1 Te powder was uniaxially pressed in a stainless steel mold with a diameter of 5 mm under a pressure of 6 MPa to form a cylindrical green body with a thickness of 1 mm; Step (2): Set the vacuum degree to 10 ~3 The furnace temperature of the vacuum tube furnace of Pa was raised to the required temperature for flash burning at a rate of 10℃ / min in vacuum. During the heating process, a preset constant electric field was applied to the cylindrical blank until flash burning occurred, and a flash burning experiment was carried out. The electric field strength was set to 300V and the current density was 60mA / mm 2 The flashing time is 60s and the furnace temperature is 430℃. After the flashing occurs, the power is turned off after maintaining the preset current for a certain period of time. The sample cools down with the furnace to obtain Cd 0.9 Mn 0.1 Te semiconductor crystal; Step (3): Flash-sinter the Cd 0.9 Mn 0.1 The two sides of the Te semiconductor crystal were polished with 2000-grit sandpaper for 2 minutes each to remove the carbon that penetrated into the crystal surface. Then, the two sides of the crystal were polished with 7000-grit sandpaper for 5 minutes each to eliminate some scratches. Finally, the two sides of the crystal were polished with a polishing liquid prepared with MgO powder for 5 minutes each to eliminate most scratches. The crystal was washed with deionized water and dried with nitrogen to prepare a room temperature radiation X-ray detector.

[0028] Figure 1 (c) is the Cd obtained in this example 0.9 Mn 0.1Scanning electron microscope (SEM) photo of the cross section of the Te sample. It can be seen that the Cd flashed for 60s under the assistance of electric field 0.9 Mn 0.1 Te crystals are already very dense, with a relative density of 96.2%.

[0029] The present invention is not limited to the above-mentioned embodiments. Anyone should be aware that any structural changes made under the enlightenment of the present invention, and any technical solutions that are the same or similar to the present invention, fall within the protection scope of the present invention. The technology, shape, and structural parts not described in detail in the present invention are all well-known technologies.

Claims

1. A method for preparing a CdTe-based semiconductor crystal, characterized in that: The following steps are involved: Step (1), using an analytical balance to weigh a certain mass of CdTe-based powder, and uniaxially pressing the powder in a mold to form a cylindrical body; Step (2), placing the cylindrical body in a vacuum tube furnace, controlling the furnace temperature and applying an electric field for flash burning, maintaining the current at a preset current for a certain period of time and then turning off the power supply to obtain a CdTe-based semiconductor crystal; Step (3), surface treatment is performed on the CdTe-based semiconductor crystal obtained by flash calcination, so as to obtain a CdTe-based semiconductor crystal with a smooth surface.

2. The method for preparing a CdTe-based semiconductor crystal according to claim 1, characterized in that: In step (1), the mass of the CdTe-based powder is weighed to be 100-300 mg, the thickness of the cylindrical body is 1-1.4 mm, the diameter is 5-10 mm, and the uniaxial pressure is 6-10 MPa.

3. The method for preparing a CdTe-based semiconductor crystal according to claim 1, characterized in that: The CdTe-based semiconductor materials include CdTe, CdZnTe and CdMnTe. 0.9 Zn0.1Te and Cd 0.9 Mn 0.1 High purity (5N) Te powder is used as raw material.

4. The method for preparing a CdTe-based semiconductor crystal according to claim 1, characterized in that: Before placing the cylindrical body in the vacuum tube furnace in step (2), the cylindrical body needs to be connected in series to the circuit.

5. The method for preparing a CdTe-based semiconductor crystal according to claim 1, characterized in that: Step (2) in obtaining CdTe-based semiconductor crystals is as follows: Step (2.1) After placing the cylindrical blank in a vacuum tube furnace, the furnace temperature of the vacuum tube furnace is increased at a rate of 5°C to 10°C / min to a temperature required for flash burning; Step (2.2) applies a preset constant electric field to the cylindrical blank during the heating process until flash burning occurs; After flash burning occurs in step (2.3), the power supply is changed from a constant voltage state to a constant current state. After maintaining the current density for a certain period of time, the power supply and the heating furnace are turned off and the temperature is lowered to room temperature.

6. The method for preparing a CdTe-based semiconductor crystal according to claim 5, characterized in that: The vacuum degree of the vacuum tube furnace is 10 ~3 Pa~10 ~4 Pa, temperature is 390~590℃.

7. The method for preparing a CdTe-based semiconductor crystal according to claim 5, characterized in that: The electric field strength is 200V / cm to 600V / cm, and the current density is 30mA / cm 2 ~70mA / cm 2 The flash burning time is 20s to 60s, and the cooling method is cooling with the furnace.

8. The method for preparing a CdTe-based semiconductor crystal according to claim 1, characterized in that: Step (3) surface treatment of the CdTe-based semiconductor crystal obtained by flash calcination: Step (3.1): Use 2000-grit sandpaper to polish both sides of the CdTe-based semiconductor crystal for 2 minutes each to remove the carbon that has penetrated into the crystal surface; Step (3.2): Use 7000 grit sandpaper to polish both sides of the crystal for 5 minutes each to remove the scratches for the first time; Step (3.3): Use a polishing solution prepared with MgO powder to polish both sides of the crystal for 5 minutes each to eliminate scratches for the second time; Step (3.4): The polished CdTe-based semiconductor crystal is washed with deionized water and then dried with nitrogen to complete the surface treatment.

9. A CdTe-based semiconductor ceramic prepared as claimed in claims 1 to 8, used for preparing a room temperature radiation X-ray detector.