Novel environment-friendly dyeing technology using microcapsules
By combining microcapsules and ionic liquids, a novel environmentally friendly dyeing technology has been developed, solving the solubility and compatibility issues of cellulose fibers in solution dyeing. This has enabled efficient and environmentally friendly textile dyeing, expanded the dyeing range, and reduced energy consumption and chemical usage.
Patent Information
- Application Number
- CN202411086003.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-12
AI Technical Summary
Existing solution dyeing techniques are difficult to apply to cellulose fibers, mainly because cellulose fibers have poor solubility in traditional solvents and the interaction between dyes and solvents may alter the color or chemical integrity of the dyes.
By combining stock solution dyeing technology with microcapsules and ionic liquids, sodium alginate-indigo microcapsules were prepared and dissolved with cellulose in an ionic liquid. The high solubility of the ionic liquid was used to dissolve the cellulose, and the dye was encapsulated in microcapsules to maintain its chemical stability.
This method expands the application of solution dyeing to cellulosic fibers, improves dyeing compatibility and chemical stability, reduces dye loss, lowers production energy consumption and chemical usage, and achieves an environmentally friendly textile dyeing method.
Smart Images

Figure CN118932512A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of environmentally friendly dyeing, and in particular to a novel environmentally friendly dyeing technology utilizing microcapsules. Background Art
[0002] The textile industry has a considerable share of the global market, reaching £689.54 billion in 2023 and is expected to maintain a steady annual growth rate of 7% over the next decade, providing huge employment prospects worldwide. However, this expansion coexists with huge environmental challenges, especially dyeing effluent discharge. These processes require the use of large amounts of chemicals and dyes, and about 15% of dyes are discharged into the environment, causing serious ecological hazards such as ecotoxicity and irreversible damage to plants and animals, as well as carcinogenic and genotoxic effects. Therefore, there is an urgent need to focus on improving the sustainability of dyeing processes, emphasizing the urgent need for the textile industry to research environmentally friendly alternatives.
[0003] Faced with these environmental problems, people have begun to turn to the development of environmentally friendly dyeing technologies. Methods such as electrochemical reduction, supercritical CO2 dyeing, microbial dyeing, foam dyeing, and solution dyeing have emerged. However, these technologies face many limitations, including high energy consumption and limited chromatography. Among them, solution dyeing stands out for its simplicity and effectiveness. This technology incorporates dyes directly into the fiber during the spinning process, greatly reducing the need for chemical additives and heat. In 2021, Lenzing launched modal fibers based on solution dyeing. According to laboratory data provided by Lenzing, fibers produced by this process can reduce water consumption, electricity consumption, and wastewater generation by up to 99% compared with traditional dyeing methods. In addition, it eliminates the need for thermal energy and reduces chemical use by more than 80%. These findings emphasize the huge environmental and economic benefits of solution dyeing over traditional dyeing techniques, highlighting its potential for large-scale production.
[0004] However, the technology still relies on the viscose process and requires the use of chemicals to modify the fiber, which complicates the production process because the fiber cannot be dissolved in a single step. However, the application of solution dyeing is currently limited to synthetic fibers due to two major challenges: the resistance of cellulosic fibers to dissolve in traditional solvents and the possibility that direct interaction of the dye with the solvent may change the color or chemical integrity of the dye. Summary of the invention
[0005] The present invention provides a novel environmentally friendly dyeing technology using microcapsules, which combines the stock solution dyeing technology with microcapsules and ionic liquids, so that the application range of stock solution dyeing is expanded to cellulose fibers and cellulose solutions can be obtained, which may completely change the textile dyeing industry.
[0006] In order to achieve the above object, the present invention provides the following technical solution: a new environmentally friendly dyeing technology using microcapsules, which comprises the following steps:
[0007] Step 1, preparation of sodium alginate-indigo solution: 4% sodium alginate, 1% F-127 surfactant, 2% indigo, and 93% deionized water were added into a beaker and stirred at room temperature for 6 hours;
[0008] Step 2, preparation of indigo microcapsules: transfer the prepared sodium alginate-indigo solution into a syringe, use 5% calcium chloride solution as the receiving device of the negative electrode, connect the positive electrode to the syringe, set the injection volume to 1 ml / h for electrospraying; after the electrospraying is completed, separate the indigo microcapsules with a negative pressure funnel;
[0009] Step 3, preparation of microcapsule fiber solution: 3% cellulose and 97% ionic liquid are heated in an 85°C oil bath and stirred for 12 hours. After the cellulose is completely dissolved, the temperature is lowered to 70°C, indigo microcapsules are added, and stirring is continued for 15 minutes. The solution is transferred to a syringe and then placed in a vacuum drying oven and vacuum dried at 60°C for 2 hours to remove bubbles in the solution.
[0010] Step 4: Prepare fibers by wet spinning: Place the syringe into the injection pump, add deionized water into the water tank, adjust the needle speed to 5 ml / min, and adjust the collector speed to 30 r / min for spinning; after spinning, soak the resulting product in deionized water for more than 24 hours, changing the water at least three times during this period to ensure that the ionic liquid in the fiber is completely discharged, rewind the yarn on the collector and dry it to obtain the final product.
[0011] Preferably, the indigo is provided by alginate, cellulose, and 1-ethyl-3-methylimidazole diethyl phosphate.
[0012] Preferably, the cathode voltage is negative 2KV, and the anode voltage is positive 24 to 30KV.
[0013] Preferably, in the step 2, after the indigo microcapsules are separated, they are rinsed three times with deionized water to remove surface impurities of the indigo microcapsules.
[0014] Preferably, in step three, the amount of indigo microcapsules added is 1%-20%.
[0015] The beneficial effects of the present invention are that the technology improves the compatibility of dyeing cellulose fibers by using ionic liquids known for their excellent solubility to dissolve fibers such as cellulose. In addition, microencapsulation technology encapsulates the dye in a protective matrix. This dual-action method maintains the chemical stability of the dye and avoids compatibility issues by selecting an encapsulant with consistent solute properties. In addition, alginate is used as a bio-based encapsulation material in synergy with indigo dye to solve the problem of microplastic pollution, thus constituting a viable and environmentally friendly alternative to traditional textile dyeing methods. This technical solution combines solution dyeing technology with microcapsules and ionic liquids, which is expected to redefine fabric dyeing, expand the scope of application of solution dyeing to cellulose fibers, and has the potential to revolutionize the textile dyeing industry. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0017] Figure 1 Schematic diagram of the electrospray device of the present invention;
[0018] Figure 2 It is a schematic diagram of the wet spinning device of the present invention;
[0019] Figure 3 A schematic diagram of the composite fiber of the present invention;
[0020] Figure 4 This is a SEM photo of the AIM of the present invention;
[0021] Figure 5 is the particle size distribution of the dry AIM sample of the present invention;
[0022] Figure 6 Microscope images of wet AIM samples of the present invention (A and B are AIM-1, C and D are AIM-2, E and F are AIM-3);
[0023] Figure 7 Microscopic photographs of AIM-CF of the present invention (A is AIM-CF-1, B is AIM-CF-2, and C is AIM-CF-3);
[0024] Figure 8 SEM images of AIM-CF of the present invention (A and D are AIM-CF-1, B and E are AIM-CF-2, C and F are AIM-CF-3);
[0025] Fig. 9 FTIR spectra of the present invention (A is indigo, alginate, AIM-1, B is AIM-CF-1, AIM-CF-2AIM-CF-3, CF);
[0026] Fig.10 The TGA thermal analysis diagram of the present invention (A is indigo, alginate, AIM, B is CF, AIM-CF-2);
[0027] Fig.11 are the mechanical properties of the fiber of the present invention (A is the Young's modulus of the fiber, B is the tensile strength of the fiber, and C is the strain of the fiber);
[0028] Fig.12 is the absorbance of the cross-linked calcium chloride solution of the present invention;
[0029] Fig.13 is the indigo content in the aqueous solution after spinning of the present invention;
[0030] Fig.14 is the loss rate of indigo in the production process of the present invention;
[0031] Fig.15 The indigo content in the solution after washing with water for 48 hours in the present invention;
[0032] Fig.16 is the weight retention rate of the fiber of the present invention after 20 washings;
[0033] Fig.17 is the indigo content in the solution after the deionized water immersion experiment of the present invention;
[0034] Fig.18 Schematic diagram of AIM-CF-2 energy dispersive X-ray spectroscopy (EDS);
[0035] Fig.19 Includes comprehensive infrared information for AIM-1, alginate, indigo, pure cellulose fibers, and composite fibers;
[0036] Fig. 20 This is the gradient diagram of standard indigo dye at a wavelength of 604nm. DETAILED DESCRIPTION
[0037] The technical solution of the present invention will be clearly and completely described below in conjunction with the accompanying drawings of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] A novel environmentally friendly dyeing technology using microcapsules comprises the following steps:
[0039] Step 1, preparation of sodium alginate-indigo solution: 4% sodium alginate, 1% F-127 surfactant, 2% indigo, and 93% deionized water are added into a beaker and stirred at room temperature for 6 hours; wherein the indigo is provided by alginate, cellulose, and 1-ethyl-3-methylimidazole diethyl phosphate.
[0040] Step 2, preparation of indigo microcapsules: transfer the prepared sodium alginate-indigo solution into a syringe, use 5% calcium chloride solution as the negative electrode receiving device, connect the positive electrode to the syringe, set the injection volume to 1ml / h for electrospraying, such as Figure 1 As shown; after the electrospray is completed, the indigo microcapsules are separated using a negative pressure funnel; wherein the cathode voltage is negative 2KV, the cathode voltage is positive 24 to 30KV, and after the indigo microcapsules are separated, they are rinsed three times with deionized water to remove surface impurities of the indigo microcapsules.
[0041] Step 3, preparation of microcapsule fiber solution: heat 3% cellulose and 97% ionic liquid in an 85°C oil bath and stir for 12 hours. After the cellulose is completely dissolved, cool to 70°C, add indigo microcapsules, continue stirring for 15 minutes, transfer the solution to a syringe, and then put it into a vacuum drying oven and vacuum dry it at 60°C for 2 hours to remove bubbles in the solution; wherein the amount of indigo microcapsules added is 1%-20%.
[0042] Step 4: Prepare fiber by wet spinning: Place the syringe into the syringe pump, add deionized water into the water tank, adjust the needle speed to 5 ml / min, and adjust the collector speed to 30 r / min for spinning; after spinning, soak the obtained product in deionized water for more than 24 hours, during which the water is changed at least three times to ensure that the ionic liquid in the fiber is completely discharged, and rewind the yarn on the collector to dry to obtain the final product, such as Figure 2 , Figure 3 shown.
[0043] Experimental analysis methods / characterization techniques
[0044] Optical Microscope:
[0045] (a) Place the wet microsphere sample on a glass slide, cover it with a glass slide, and observe the color and morphology of the microcapsules under a microscope. (b) Detection of microcapsule composite fibers: Observe the color and morphology of the fibers under a microscope. Place the textile on a rectangular cutout sample holder with a width of 10.20 mm to ensure that the fibers stretch naturally. At the same time, the software supports the random selection of fiber samples at three different positions, measure the diameter, and take the average value.
[0046] Scanning Electron Microscopy (SEM):
[0047] The microstructure and surface of AIM and AIFC were examined by scanning electron microscopy (SEM). A 10 nm thick gold layer was vacuum stripped on the instrument (1 cm) and observed by TESCAN S8000.
[0048] Thermal stability analysis:
[0049] Thermal analyzer analyzes sodium alginate, indigo, AIM and AICF. Take about 500 mg of sample and put it in a tray, and test it at a rate of 10 degrees / minute from room temperature to 800 degrees.
[0050] Analysis of mechanical properties of composite fibers:
[0051] The analysis equipment was a DEBEN 200N Microtest tensile stage controller, and the tensile speed was set to 0.2mm / min. The AICF samples were glued in a 10.2mm sample plate to reduce the influence of the clamp. The fiber diameter was measured by optical microscopy, and the ultimate tensile strength and strain were determined by taking the fiber break point. Young's modulus was calculated from the slope of the linear portion of the stress-strain curve before the yield point.
[0052] FTIR Spectroscopy:
[0053] Infrared spectroscopy is used to determine the chemical bonds in raw materials, microcapsule samples and composite fibers. At the same time, it can check whether EMIM DEP remains in AICF after the cleaning procedure.
[0054] UV spectrophotometry detection:
[0055] Indigo standard curve formula: Dissolve commercial indigo in chloroform to obtain five known concentrations. Since indigo does not dissolve immediately in chloroform, place the standard solution in an ultrasonic bath for 10 minutes to ensure complete dissolution of the dye. Subsequently, record the absorbance value at the maximum absorbance wavelength (λmax) of 604nm.
[0056] Extraction and measurement of indigo in aqueous samples:
[0057] Extraction was performed using chloroform to determine the indigo concentration in aqueous samples. The aqueous indigo sample was mixed with chloroform to transfer the dye into the organic phase. After extraction, the absorbance of the organic phase was measured at λ = 604 nm. The indigo concentration in the sample was calculated using a calibration curve. The LoD and LoQ of this method were 0.02 mg / L and 0.08 mg / L, respectively.
[0058] Determination of indigo in cross-linked calcium chloride solution: The cross-linked AIM and calcium chloride solution were vacuum filtered. Then 20 ml of the initial filtrate was extracted with 5 ml of chloroform, and the indigo concentration in the extract was measured. The chloroform solution was used as a blank control, and the absorbance was read at the maximum absorption wavelength.
[0059] Analysis of indigo in the solution after spinning: After wet spinning was completed, 100 ml of sample was extracted from the spinning pool with 5 ml of chloroform for analysis. This involved three replicate tests for each batch of AIM-CF-1 to AIM-CF-5 and the average absorbance value was recorded.
[0060] 48 hours washing test:
[0061] Dilute Formil laundry detergent and 20 ml of Formil laundry disinfectant to a total volume of 2 liters.
[0062] (b) Washing test: about 0.2 g of fiber was placed in 40 ml of prepared washing liquid, stirred at 45°C and 300 rpm for 48 hours. After washing, 20 ml of washing liquid was extracted with 5 ml of chloroform and concentrated to 1 ml, and the indigo content was tested, with the washing liquid as a blank control. The absorbance reading was the average of three tests.
[0063] 48-hour fiber immersion test in deionized water: 0.2 g of each fiber sample was immersed in 40 ml of deionized water and magnetically stirred at 300 rpm for 48 hours at room temperature. Subsequently, 20 ml of each sample was extracted with 5 ml of chloroform, and deionized water was used as a blank control. The average absorbance at the peak absorption wavelength was calculated by three measurements.
[0064] In summary, the absorbance values obtained for all tests were compared with the indigo standard curve to infer the concentration of indigo in the corresponding solution.
[0065] Evaluation of fiber weight retention after multiple wash cycles:
[0066] Sample preparation: Select multiple fiber samples, each weighing about 0.2 g. Place them in a vacuum oven and dry them at 50°C for 2 hours. Immediately after taking them out, weigh the exact weight of each sample using an analytical balance, and measure each sample three times to determine the average weight.
[0067] Washing procedure: Immerse each fiber sample in 40 ml of the specified washing liquid (as described in Section 2.4.8-a). Maintain a constant temperature of 45°C and a stirring speed of 300 rpm for two hours. Then, remove the washing liquid and rinse the fiber three times with deionized water. Re-inject 40 ml of fresh washing liquid and repeat the stirring for two hours. This washing process should be repeated twenty times. Finally, rinse the sample three times with deionized water and place it in a vacuum oven for a two-hour drying phase. After drying, weigh the fiber using an analytical balance and make three measurements to determine the average weight.
[0068] Data Analysis: Fiber weight retention was evaluated by comparing the weight of each sample after washing with the weight before washing as shown in formula (1). The retention was calculated as the initial weight divided by the final post-wash weight and expressed as a percentage.
[0069]
[0070] F W ---Fiber weight retention rate (percentage)
[0071] F B ---Weight of fiber before washing
[0072] F A ---The weight of the fiber after washing
[0073] Quantification of dye utilization in the production process:
[0074] Quantifying Indigo Loss: Indigo loss is divided into losses during microsphere crosslinking and wet spinning. To determine indigo loss during the crosslinking stage, multiply the concentration in the solution after crosslinking by the total volume of the solution. A similar method is used to calculate indigo loss during spinning.
[0075] Estimation of total indigo consumption: This involves the mass of indigo used for fiber microsphere manufacturing. Each production cycle uses 20 grams of indigo and sodium alginate solution, which produces approximately 10 grams of microspheres. The amount of indigo added to the fiber microspheres is calculated by multiplying the mass of indigo in the mixture by the mass of microcapsules added to the fiber and then dividing by the total amount of microcapsules produced.
[0076] Dye loss rate calculation: The dye loss rate is the ratio of the weight of indigo lost during the production process to the weight used for fiber production, reflecting the proportion of dye loss compared to the initial dye used in the manufacturing process.
[0077] Li ndigo =L spinning +L cross-link (2)
[0078] L cross-link =C indigo-after-crosslinking ×V cross-linking(3)
[0079] L spinning =C indigo-after-spinning ×V spinning (4)
[0080] U indigo =U indigo-AIMsolution ×M AIMaddinfibre / M AIMproduced (5)
[0081] Ri ndigoloss =L indigo / U indigo ×100% (6)
[0082] L indigo Indigo loss during the entire production process
[0083] L cross-link Indigo loss during cross-linking
[0084] L spinning Indigo loss during wet spinning
[0085] C indigo-after-crosslinking The concentration of indigo in the solution after cross-linking
[0086] C indigo-after-spinning Concentration of indigo in solution after wet spinning
[0087] V cross-linking Total volume of cross-linking solution
[0088] V spinning Total volume of wet spinning solution
[0089] U indigo The total mass of indigo used in one experiment
[0090] U indigo-AIMsolution The quality of indigo used in the microsphere mixture
[0091] M AIMaddinfibre The mass of microcapsules added to the fiber
[0092] M AIMproduced Total mass of microcapsules produced
[0093] R indigo loss Indigo loss rate
[0094] Results and Discussion:
[0095] In order to explore the production process of AlM and the mechanism of microcapsule dyeing fibers, various AIM, AIM-CF and cellulose fibers (blank control group) were prepared. The specific process parameters and formulas are shown in Tables 1 and 2.
[0096] Table 1: AIM parameters
[0097]
[0098] Table 2: Parameters of textile samples
[0099]
[0100] Microcapsule characteristics analysis:
[0101] Figure 4 This is the SEM image of the microstructure of AIM in the dry state. The size, shape, and structure of the microspheres are highly uniform, and the surface morphology is smooth. No obvious indigo powder is seen on the surface of the microspheres, indicating that most of the indigo core has been completely wrapped by the alginate shell.
[0102] The AIM particle size was analyzed using Image J software. Figure 5 ,The bar graph shows the particle size distribution of the microspheres. Most of the microspheres have a particle size between 0 and 300 nanometers, indicating that the AIM particle size is relatively regular.
[0103] Figure 6 AF is the microscope image of AIM (wet sample). Wet samples are larger than dry samples and are more suitable for microscopic observation. Figure 6 We found that the depth of AIM color is directly related to the indigo content of the microspheres. Specifically, as the percentage of indigo increases, the color becomes darker, and this relationship can be used to tune AIM color.
[0104] But it also brings a problem. When the microspheres are dried, the particle size decreases. This conversion process will cause the color of the dried microcapsules to become significantly darker, especially as the indigo concentration increases. The color will become darker and darker, and the AIM-3 microcapsules even appear dark black. Considering the standard color depth of general textiles on the market, we carefully selected microcapsules with a 1% indigo content (AIM-1) as the main raw material for manufacturing composite dyed fibers suitable for later applications.
[0105] Research and improvement of fiber dyeing effect
[0106] The dyeing effect of AIM-CF (alginate-indigo microcapsule composite fiber) was carefully examined by microscopic examination, such as Figure 7 As shown, Figure 7 The AC depicts fibers containing the same microcapsules (AIM-1), albeit in different proportions. It is noteworthy that the hue of the composite fibers deepens with increasing microcapsule content. Adjusting the amount of microcapsules introduced during the manufacturing process allows precise control of the fiber dyeing depth.
[0107] Subsequent magnified images revealed that fibers with increased microcapsule concentrations exhibited a denser dispersion of microcapsules, resulting in fibers with richer hues and denser color distribution. Significantly, the resulting dyeing effects were similar to those achieved through traditional dyeing techniques. Conversely, fibers with reduced microcapsule content exhibited a sparser distribution of microcapsules within the fiber matrix, ultimately producing a discontinuous dyeing effect that resulted in a unique aesthetic. This unique dyeing effect may have the potential to be further explored and utilized in the fashion industry.
[0108] Fiber microstructure:
[0109] SEM images show the morphology of the composite fibers. Figure 4 It can be seen from the AC that the surface of AIM-CF becomes more uneven as the percentage of AIM-1 increases. Figure 4 In the AC, spherical microspheres can be seen on the fiber surface. Figure 4 As shown in Figure 2, df is the cross-sectional image of the fiber. There are some large particles inside the fiber, which may be caused by the aggregation of microcapsules during wet spinning. AIM-CF-2 energy dispersive X-ray spectroscopy (EDS) is shown in Figure 2. Fig.18 This finding is further supported by the results shown in Figure 2. Since the shell of the microcapsules is made of sodium alginate and calcium chloride is the cross-linking agent of this substance, only the microcapsules show calcium symbols in the calcium image, while cellulose does not contain calcium. Therefore, obvious calcium ion signals can be seen on the large particles in the image.
[0110] At the same time, the voids visible near some large particles indicate a lack of chemical bonding between sodium alginate and cellulose. This finding is significant because it affects the mechanical strength of cellulose fibers. Strategies such as uniformly dispersing microcapsules before spinning (for example, using ultrasonic vibration or a high-speed disperser) can alleviate this problem. The DF enlarged image shows that there are scaly fracture surfaces on the cross-section of the fiber, indicating that the fiber is still subjected to specific forces and has a specific direction during the manufacturing process. In addition, several microcapsules can be observed on the cross-section, indicating that the microcapsules are randomly distributed in the fiber.
[0111] Chemical Analysis (TGA / FT-IR):
[0112] Fig.19 Comprehensive infrared information including AIM-1, alginate, indigo, pure cellulose fiber and composite fiber is shown. The infrared spectrum of indigo shows a characteristic C=O vibration at 1625 cm -1 (Stretched), 1069cm -1 (Swing) and 698cm -1 There is a specific peak at (sway). 1698cm -1The nearby signals can be attributed to the stretching vibration of CN groups and the swinging of CH and NH groups. -1 The five-membered ring signal was observed at 1609, 1584, 1481, 1459, 1315, 1196, 1009, 878, 751, 712 and 697 cm -1 The stretching vibration and bending vibration are shown at 3100-3520cm (Baran et al., 2010). In addition, the spectrum of sodium alginate shows -1 Stretching vibration of OH and NH groups at 1636 cm -1 The stretching vibration of the C=C functional group and 1000-1100cm -1 It is in the polysaccharide fingerprint region and is related to CC and CO stretching vibrations.
[0113] Fig.10 A shows a partial magnified infrared spectrum of sodium alginate, indigo, and AIM-1. 1428 cm -1 The six-membered ring signal peak at 1000 cm-1 confirmed the presence of indigo in AIM-1. However, in AIM-1, this signal is relatively weak. This can be attributed to the fact that ATR-IR only evaluates the surface of the sample, using the total internal reflection property that produces an attenuated wave. Most of the indigo may be encapsulated in the sodium alginate, with only a very small amount of indigo distributed on the surface of the microspheres. Therefore, the weak signal confirms that the indigo is fully encapsulated by alginate. In addition, the peaks from 3100 to 3500 cm-1 show that the indigo is not fully encapsulated in the alginate. -1 , the microcapsules and sodium alginate showed the same OH and NH signal peaks, confirming the presence of sodium alginate in AIM-1.
[0114] In addition, the sodium alginate on the surface of the microspheres cross-links with calcium ions, which affects the spectrum. Compared with the original sodium alginate signal, the 1422 cm -1 The nearby peak is weaker and shifts to higher frequencies, from 1417 cm -1 Move to 1422cm -1 In addition, the asymmetric stretch moved from 1636.07 to 1636.43 cm -1 , this upward trend is consistent with the results reported by Volesky and Matthew (Cathell & Schauer, 2007).
[0115] Fig.10 B shows that both the composite fiber and the pure cellulose fiber exhibit characteristic cellulose peaks (i.e., 3338 cm -1 OH bond, 2897cm -1 for CH bonds and 1017cm -1is a CO bond) (Rosa et al., 2010). This observation confirms the presence of cellulose in the composite fibers. In addition, the 1238 cm -1 There is no characteristic peak (emimDEP representing P=O bonds) at the fiber, indicating that the solvent has been completely removed from the fiber (Fitzpatrick et al., 2012)
[0116] Fig.10 The TGA curves of pristine indigo, alginate, and our prepared microcapsules are shown. The weight loss versus temperature curve of alginate shows that the initial weight loss is around 65-100°C, which is mainly due to the hydrophilicity that is characteristic of alginate leading to water loss. The most significant weight loss occurs in the temperature range of 220-250°C, which is due to the cleavage of glycosidic bonds and other related bonds in the alginate chain. Compared with alginate, the degradation behavior of indigo is highly thermally stable, with most of the weight loss occurring around 350-400°C, probably due to the cleavage of inter- and intra-molecular bonds associated with the aromatic ring. The higher residue content of indigo confirms its better thermal stability. The thermal degradation behavior of AIM-1 is between the weight loss curves of alginate and indigo, as shown in the figure. AIM-1 shows water evaporation around 55-100°C, which is also seen in alginate. The significant degradation of AIM-1 occurs in the range of 220-500°C due to the combined effects of indigo and alginate. The degradation curve of AIM-1 was gentler than that of its precursor, which indicated that the developed microcapsules had better thermal stability than the raw material.
[0117] Fig.10 TGA thermograms of pure cellulose fiber (CF) and microcapsule embedded cellulose fiber (AIM-CF-2) are provided. In CF, two major degradations were observed, occurring at around 70 to 110 °C and around 300 °C. The initial weight loss is due to the evaporation of water molecules, while the later weight loss is due to the decomposition and degradation of the chemical structure. In the case of AIM-CF-2, significant water loss was also observed in AIM-1 and cellulose. The degradation behavior of AIM-CF-2 has different steps, which is due to the presence of embedded microcapsules and cellulose. The microcapsules are well embedded in the cellulose fibers, which significantly improves the thermal stability and helps in producing high-quality fibers. Analysis of fiber mechanical properties (tensile test):
[0118] By checking the mechanical properties data (such as Fig.11Figure 3 shows the correlation between the microcapsule content and the mechanical properties of the composite fibers. Specifically, the Young's modulus and tensile strength of the composite fibers increase, while the tensile elongation decreases, as the microcapsule content increases. This trend can be attributed to the size distribution of the dry microcapsules, which are mainly in the range of 100 to 200 nanometers. Given that this size is commensurate with some nanofillers, the microcapsules appear to impart a reinforcement effect to the composites, similar to traditional nanofillers. The introduction of such fillers reduces the free volume available in the composites, thereby increasing the stiffness of the laminate.
[0119] Analysis of indigo loss during production;
[0120] Fig. 20 A gradient plot of the standard indigo dye at a wavelength of 604 nm is presented, which corresponds to the peak absorption wavelength determined in the standard solution concentration.
[0121] Fig.12 The concentration of indigo in the aqueous calcium chloride solution after cross-linking is shown. The absorbance does not change significantly and remains very low. Considering the precision threshold of the spectrophotometer, it can be inferred that no indigo is detected in the calcium chloride solution. This phenomenon can be attributed to the inherent insolubility of indigo in water. After mixing with sodium alginate, indigo sinks into the calcium chloride solution in the form of tiny droplets under the action of gravity. Upon contact, sodium alginate induces a cross-linking reaction, forming an intermolecular cross-linked network that hinders the movement of molecules, thereby encapsulating indigo within the microspheres. Therefore, the post-reaction analysis shows that there is no indigo in the calcium chloride solution.
[0122] Fig.13 Data correlating the indigo concentration and absorbance in the residual solution after the wet spinning procedure are shown. The results show that the amount of indigo spilling into the solution after spinning is minimal, ranging between 0.018 mg / L and 0.032 mg / L. This residual indigo may originate from the microcapsules, where the indigo is randomly embedded, possibly resulting in surface deposition. The subsequent addition of these microcapsules to the cellulose ionic solution may result in the transfer of the surface-deposited indigo into the ionic liquid and its absorption into the aqueous phase during the mixing process.
[0123] Fig.14 The reduction of indigo throughout the spinning process was further elucidated, indicating that the loss was only 1‰ to 2‰. Our method is significantly lower than traditional dyeing methods, which typically result in 40% to 50% dye loss. This efficiency makes the raw materials more economical and greatly reduces the dye concentration in the final wastewater. In addition, because ionic liquids were used as solvents in this experiment, it is possible to recycle the wet spinning solution, thereby facilitating the recovery of ionic liquids and lost dyes. This method is expected to significantly reduce the impact on the environment, in line with the goal of a truly green and sustainable textile manufacturing process.
[0124] Analysis of dyed fiber washing resistance:
[0125] Fig.15 The accompanying data in the Figures depict the results of a comprehensive washing test on the fibers. After 48 hours of washing, the concentration of indigo in the remaining solution was significantly lower, indicating that the cellulosic fibers dyed in this way have excellent washing resistance and exhibit strong color fastness. There are two reasons for this washing resistance. The first is the hydrophobic nature of indigo, which makes it essentially insoluble in water, Fig.17 This property is further demonstrated by the data confirming the absence of indigo after soaking in deionized water and showing that the composite fibers are within the detection limits of UV spectrophotometry. In addition, the indigo is not chemically modified during the dyeing process, which helps maintain its physical properties and improves its performance in wash tests.
[0126] The second reason is that this dyeing technique encapsulates indigo in microcapsules wrapped in a sodium alginate shell, which is then integrated into cellulose-based composite fibers. This double encapsulation significantly improves the chemical durability of indigo compared to fibers dyed by traditional methods, where the dye is directly exposed to environmental factors. As a result, this encapsulation improves the color fastness observed in water and washing durability evaluations.
[0127] Fig.16 The stability of the fiber weight over multiple wash cycles is shown. The mass of the composite fibers remained constant compared to pure cellulose fibers, indicating that the microencapsulated composite fibers exhibit a structure that is not much different from traditional cellulose fibers. This weight stability demonstrates the fibers' ability to resist shrinking or stretching, confirming their suitability for everyday use. The high weight retention also indicates that the composite fibers experience minimal loss of indigo during washing, further highlighting the fibers' excellent wash resistance and, crucially, color fastness.
[0128] Compared with traditional dyeing consumption;
[0129] A comparative analysis of dyeing and innovative dyeing methods shows that the latter has significant environmental benefits. The traditional method consumes 6 kWh of electricity, 170 g of chemicals and 100-150 liters of water for every kilogram of fiber produced, generating large amounts of wastewater and sulfur-containing gas emissions. This high resource consumption depletes natural resources and causes water pollution and deterioration of air quality. In contrast, the new method eliminates additional dyeing after fiber production, resulting in zero electricity and zero chemical use, and significantly reduces water consumption to 15-20 liters per kilogram of fiber, with minimal wastewater discharge (12-15 liters) and no gas emissions. These reductions highlight a cleaner, more resource-efficient method that helps achieve sustainable development and saves costs for manufacturers, as shown in Table 3.
[0130]
[0131] In addition, reduced chemical use mitigates specific health risks for workers, such as respiratory problems and skin diseases, and reduces the ecological impacts of wastewater discharge, including soil and water contamination. The durability and color fixation of fibers produced using this new method have been shown to be superior to those of conventionally dyed fibers. This advancement marks a key step toward sustainable textile production that meets global environmental goals and responds to growing consumer demand for environmentally friendly products, potentially improving the industry’s reputation and market competitiveness.
[0132] in conclusion:
[0133] In conclusion, the research described in this article represents a significant advance in the field of sustainable textile manufacturing, introducing an innovative method for synthesizing indigo-alginate microcapsules. This new technique heralds a departure from traditional fiber dyeing methods, eliminating the need to use reducing and oxidizing agents during the indigo treatment process. Only water and ionic liquid remain after the reaction, which can be recycled - highlighting the potential for significantly reducing environmental impact.
[0134] The process detailed in this article does not involve any environmentally harmful chemicals, thereby reducing waste generation and is the epitome of true “green” technology. In addition, it increases the efficiency of subsequent fiber processing, saving energy and costs.
[0135] In addition, the study introduces a versatile technology that can adjust the color tone of the resulting fibers by adjusting the concentration of microcapsules within the fibers and the indigo content within the microcapsules. The dyed fibers show significant resistance to fading and excellent wash fastness, ensuring minimal color transfer during washing. In addition, these fibers show enhanced mechanical properties compared to unmodified cellulose fibers.
[0136] Overall, these advances make a compelling case for the textile industry to adopt this environmentally friendly technology, with the potential to revolutionize fiber dyeing and help mitigate microplastic pollution.
[0137] The above is only a specific embodiment of the present invention, but the protection scope of the present invention is not limited thereto. Any person skilled in the art can easily think of changes or substitutions within the technical scope disclosed by the present invention, which should be included in the protection scope of the present invention. Therefore, the protection scope of the present invention should be based on the protection scope of the claims.
Claims
1. A new environmentally friendly dyeing technology using microcapsules, Features , including the following steps: Step 1, preparation of sodium alginate-indigo solution: 4% sodium alginate, 1% F-127 surfactant, 2% indigo, and 93% deionized water were added into a beaker and stirred at room temperature for 6 hours; Step 2, preparation of indigo microcapsules: transfer the prepared sodium alginate-indigo solution into a syringe, use 5% calcium chloride solution as the receiving device of the negative electrode, connect the positive electrode to the syringe, set the injection volume to 1 ml / h for electrospraying; after the electrospraying is completed, separate the indigo microcapsules with a negative pressure funnel; Step 3, preparation of microcapsule fiber solution: 3% cellulose and 97% ionic liquid are heated in an 85°C oil bath and stirred for 12 hours. After the cellulose is completely dissolved, the temperature is lowered to 70°C, indigo microcapsules are added, and stirring is continued for 15 minutes. The solution is transferred to a syringe and then placed in a vacuum drying oven and vacuum dried at 60°C for 2 hours to remove bubbles in the solution. Step 4: Prepare fibers by wet spinning: Place the syringe into the injection pump, add deionized water into the water tank, adjust the needle speed to 5 ml / min, and adjust the collector speed to 30 r / min for spinning; after spinning, soak the resulting product in deionized water for more than 24 hours, changing the water at least three times during this period to ensure that the ionic liquid in the fiber is completely discharged, rewind the yarn on the collector and dry it to obtain the final product.
2. A novel environmentally friendly dyeing technology using microcapsules according to claim 1, Features: The raw materials are provided by indigo, alginate, cellulose and 1-ethyl-3-methylimidazole diethyl phosphate.
3. A novel environmentally friendly dyeing technology using microcapsules according to claim 1, Features: The negative electrode voltage is negative 2KV, and the positive electrode voltage is positive 24 to 30KV.
4. A novel environmentally friendly dyeing technology using microcapsules according to claim 1, Features: In the step 2, after the indigo microcapsules are separated, they are rinsed three times with deionized water to remove surface impurities of the indigo microcapsules.
5. A novel environmentally friendly dyeing technology using microcapsules according to claim 1, Features: In the step 3, the amount of indigo microcapsules added is 1%-20%.