Nanofiber supporting framework material, proton exchange membrane, preparation method of proton exchange membrane and fuel cell
The alkali-functional nanofiber support framework is prepared by electrospinning and combined with perfluorosulfonic acid resin, which solves the problem of insufficient mechanical strength of the proton exchange membrane, and realizes a proton exchange membrane with high mechanical properties and swelling resistance, improving fuel cells overall performance.
Patent Information
- Application Number
- CN202411005627.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-12
AI Technical Summary
The existing proton exchange membranes have shortcomings in terms of mechanical strength and swelling resistance. In particular, the production process of the expanded polytetrafluoroethylene support layer is complex and the binding force is low, resulting in poor film thickness thinning effect and easy to cause stratification problems. .
Using nanofiber support framework material, a spinning solution composed of polybenzimidazole, strong alkali and organic alcohol is prepared by electrospinning to form an alkali-functional nanofiber support framework, and is combined with perfluorosulfonic acid resin to increase protons. Mechanical strength of the exchange membrane.
The mechanical strength of the proton exchange membrane has been improved to 77MPa~86MPa, the elongation rate of break is 165%~170%, and the elastic modulus is 68MPa~76MPa, which significantly improves the mechanical properties and swelling resistance of the membrane and extends the service life.
Smart Images

Figure CN118932541A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the field of fuel cell technology, and in particular to a nanofiber support skeleton material, a proton exchange membrane and a preparation method thereof, and a fuel cell. Background Art
[0002] Fuel cells are usually composed of proton exchange membranes, anode catalyst layers, cathode catalyst layers, gas diffusion layers, bipolar plates, and flow field plates. The proton exchange membrane is the core component of the fuel cell to generate current. It mainly transfers protons and blocks gases and electrons in the battery. Therefore, the proton exchange membrane is required to have high mechanical strength, electrical conductivity, chemical stability and anti-swelling properties. The quality of the proton exchange membrane directly determines the performance of the battery. The structure of the proton exchange membrane material is usually a polymer with sulfonate ion functional groups. In recent years, the most typical is the Nafion series of proton exchange membranes developed by DuPont, which uses perfluorosulfonic acid resin as the membrane material. The Nafion series of proton exchange membranes have excellent electrical conductivity and chemical stability, but poor mechanical strength and anti-swelling properties. Gore has developed the Goreselect series of proton exchange membranes based on Nafion membranes. While using perfluorosulfonic acid resin as the membrane material, it has developed expanded polytetrafluoroethylene as the membrane support layer, forming a composite membrane structure with a support layer. While maintaining electrical conductivity and chemical stability, it also greatly improves mechanical strength and anti-swelling properties, allowing the thickness of the membrane to be reduced to 12μm. Currently, the market share of the Gore select series of proton exchange membranes in the domestic fuel cell market has reached more than 90%.
[0003] At present, the reduction of the thickness of the proton exchange membrane generally relies on the addition of an expanded polytetrafluoroethylene support layer to the proton membrane. However, the production process of expanded polytetrafluoroethylene is complicated. At present, there are very few fluorine chemical companies in China that can produce expanded polytetrafluoroethylene, and the various performances are still far behind those of Gore in the United States. At the same time, the binding force between ordinary expanded polytetrafluoroethylene and perfluorosulfonic acid resin is low, and it is very easy to delaminate during use, and the perfluorosulfonic acid resin will fall off. Therefore, in order to prepare high-strength ultra-thin proton exchange membranes, it is urgent to develop a new support layer material with high strength and strong binding force with perfluorosulfonic acid resin. Summary of the invention
[0004] The present application provides a nanofiber support skeleton material, a proton exchange membrane and a preparation method thereof, and a fuel cell to solve the following technical problem: how to improve the strength of the proton exchange membrane.
[0005] In a first aspect, the present application provides a nanofiber support skeleton material, wherein the nanofiber support skeleton is prepared by electrospinning a spinning solution;
[0006] The raw material components of the spinning solution include: polybenzimidazole, strong base and organic alcohol; wherein, by mass fraction,
[0007] The content of the polybenzimidazole is 5% to 20%, and the content of the strong base is 1% to 10%.
[0008] Optionally, the strong base includes at least one of the following: potassium hydroxide, sodium hydroxide, calcium hydroxide, and barium hydroxide.
[0009] Optionally, the organic alcohol includes at least one of the following: ethanol, n-butanol, isobutanol, n-propanol, isopropanol, n-pentanol, isopentanol, n-hexanol, and isopropanol.
[0010] Optionally, the electrospinning process parameters include: spinning environment humidity, spinning environment temperature, spinning voltage and spinning distance; wherein,
[0011] The spinning environment humidity is 20% to 80%, the spinning environment temperature is 15° C. to 35° C., the spinning voltage is 18 kV to 22 kV, and the spinning distance is 10 cm to 30 cm.
[0012] In a second aspect, the present application provides a proton exchange membrane, the raw material components of which include the nanofiber support skeleton material described in any one of the embodiments of the first aspect and a perfluorosulfonic acid resin solution.
[0013] Optionally, the solid content of the perfluorosulfonic acid resin solution is 5% to 10%.
[0014] Optionally, the proton exchange membrane meets the following properties: mechanical strength of 77 MPa to 86 MPa, elongation at break of 165% to 170%, and elastic modulus of 68 MPa to 76 MPa.
[0015] In a third aspect, the present application provides a method for preparing a proton exchange membrane according to any one embodiment of the second aspect, the method comprising:
[0016] The perfluorosulfonic acid resin solution is coated on at least a portion of the surface of the nanofiber support skeleton material until no perfluorosulfonic acid resin solution remains on the surface of the nanofiber support skeleton material, and then dried to obtain a proton exchange membrane.
[0017] Optionally, the drying temperature is 40°C to 80°C.
[0018] In a fourth aspect, the present application provides a fuel cell, comprising the proton exchange membrane described in any one embodiment of the second aspect.
[0019] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0020] The nanofiber support skeleton material provided by the embodiment of the present application, polybenzimidazole has the advantages of good chemical stability and high mechanical strength. At the same time, the structure of polybenzimidazole contains a benzimidazole structure. The conjugation of the benzimidazole structure makes the NH protons in the structure acidic, and partial NH proton dissociation can be achieved; the strong base has good solubility in organic alcohols, and can completely dissociate hydroxide and metal ions. The strong base reacts with the dissociated part of the NH protons to neutralize, thereby forming ion pairs of nitrogen ions and metal ions, and the polybenzimidazole forms an ionic state and dissolves in the organic alcohol; by electrospinning a spinning solution containing polybenzimidazole, a strong base and an organic alcohol, a nanofiber support skeleton material containing base-functionalized benzimidazole anions and active metal cations can be obtained. Therefore, the nanofiber support skeleton material is applied to the proton exchange membrane. The alkali-functionalized nanofiber support skeleton material is hydrophilic in an ionic state, and the active metal cations therein can adsorb the sulfonic acid group of the perfluorosulfonic acid resin. The ionic attraction between the active metal cations and the sulfonic acid group can enhance the binding force between the nanofiber support skeleton material and the perfluorosulfonic acid resin, thereby improving the strength of the proton exchange membrane. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0022] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0023] Figure 1 A scanning electron microscope image of a nanofiber support skeleton material provided in an embodiment of the present application;
[0024] Figure 2 An average diameter distribution diagram of a nanofiber support skeleton material provided in an embodiment of the present application;
[0025] Figure 3 A diameter distribution diagram of a nanofiber support skeleton material provided in an embodiment of the present application when the content of polybenzimidazole in the raw material component is 10%;
[0026] Figure 4 A scanning electron microscope cross-sectional morphology image of a proton exchange membrane provided in an embodiment of the present application;
[0027] Figure 5A schematic diagram of a process for preparing a proton exchange membrane provided in an embodiment of the present application;
[0028] Figure 6 A polarization curve diagram of the voltage of a membrane electrode of a proton exchange membrane provided in an embodiment of the present application in a fuel cell as a function of current density;
[0029] Figure 7 A graph showing the variation of power density of a membrane electrode of a proton exchange membrane in a fuel cell as a function of current density provided in an embodiment of the present application;
[0030] Figure 8 A graph showing the change in open circuit voltage of a cell over time during a DOE dry-wet cycle mechanical durability test of a membrane electrode of a proton exchange membrane provided in an embodiment of the present application in a fuel cell. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0032] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0033] In the present application, the terms "include", "comprising", etc. mean "including but not limited to". "At least one", "at least one of the following" or similar expressions refer to any combination of these items, including any combination of single or plural items. For example, "at least one of a, b, or c", or "at least one of a, b, and c" can all mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0034] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0035] In a first aspect, the present application provides a nanofiber support skeleton material, wherein the nanofiber support skeleton is prepared by electrospinning a spinning solution;
[0036] The raw material components of the spinning solution include: polybenzimidazole, strong base and organic alcohol; wherein, by mass fraction,
[0037] The content of the polybenzimidazole is 5% to 20%, and the content of the strong base is 1% to 10%.
[0038] In the embodiments of the present application, polybenzimidazole has the advantages of good chemical stability and high mechanical strength. At the same time, the structure of polybenzimidazole contains a benzimidazole structure. The conjugation of the benzimidazole structure makes the NH protons in the structure acidic, and partial NH proton dissociation can be achieved; the strong base has good solubility in organic alcohols, and can completely dissociate hydroxide and metal ions. The strong base reacts with the dissociated part of the NH protons to neutralize, thereby forming an ion pair of nitrogen ions and metal ions, and the polybenzimidazole forms an ionic state and dissolves in the organic alcohol; by electrospinning a spinning solution containing polybenzimidazole, a strong base and an organic alcohol, a nanofiber support skeleton material containing base-functionalized benzimidazole anions and active metal cations can be obtained. Figure 1 This is a scanning electron microscope image of a nanofiber support skeleton material provided in the embodiment of the present application; see Figure 1 , a nanofiber support skeleton material (PBI fiber) obtained by electrospinning using a 2% KOH n-pentanol solution, and the particles on the fiber surface are KOH. The content of polybenzimidazole is limited to 5% to 20%, and the content of strong alkali is 1% to 10%, so that the strong alkali and organic alcohol can promote the complete dissolution of polybenzimidazole (PBI); if the content of the strong alkali is too high, it will destroy the surface of the nanofiber support skeleton material to a certain extent, generate too many strong alkali particles, and destroy the morphology of the nanofiber support skeleton material in the spinning preparation, thereby affecting the performance of the nanofiber support skeleton material. Exemplarily, the content of polybenzimidazole can be 5%, 7%, 9%, 11%, 13%, 15%, 17%, 19%, 20%, etc., and further, the content of the polybenzimidazole can be 10%; the content of the strong alkali can be 15%, 35%, 45%, 5%, 6%, 7%, 8%, 9%, 10%, etc., and further, the content of the strong alkali can be 2%.
[0039] In some embodiments, the strong base includes at least one of potassium hydroxide, sodium hydroxide, calcium hydroxide, and barium hydroxide.
[0040] In the embodiment of the present application, the strong base can be one or more of potassium hydroxide, sodium hydroxide, calcium hydroxide, and barium hydroxide, which can be dissolved in organic alcohols and react with the NH bonds on PBI to ionize PBI and promote the dissolution of PBI in organic alcohols. Among them, potassium hydroxide has strong enough alkalinity, not too large molecular weight, does not affect the spinning morphology, has good economy and solubility.
[0041] In some embodiments, the organic alcohol comprises at least one of ethanol, n-butanol, isobutanol, n-propanol, isopropanol, n-pentanol, isopentanol, n-hexanol, and isopropanol.
[0042] In the embodiment of the present application, the organic alcohol can be one or more of ethanol, n-butanol, isobutanol, n-propanol, isopropanol, n-pentanol, isopentanol, n-hexanol, and isopropanol. Among them, the boiling point of n-pentanol is about 138°C, and the volatilization speed is not too fast or too slow, which can make the electrospinning proceed smoothly.
[0043] Figure 2 This is a graph showing the average diameter distribution of a nanofiber support skeleton material provided in an embodiment of the present application; see Figure 2 , indicating that with the increase of polybenzimidazole content, the average diameter of the nanofiber support skeleton material increases greatly until 10%, and then increases gently; Figure 3 This is a diameter distribution diagram of a nanofiber support skeleton material provided in an embodiment of the present application when the content of polybenzimidazole in the raw material component is 10%; see Figure 3 , indicating that when the polymer PBI concentration is 10%, the average diameter of the PBI fiber is 170nm, the smallest fiber diameter is 125nm, and the largest fiber diameter is 280nm. As the polymer concentration increases, the average diameter of the PBI fiber also increases; when the polymer PBI concentration is low, the average diameter of the PBI fiber is small, but there are beads on the fiber. When the polymer PBI concentration is high, although the average diameter of the obtained PBI fiber is larger, the reduction in the fluidity of the spinning solution will be unfavorable for the production of PBI fibers. Therefore, when the spinning solvent is n-pentanol / KOH, selecting a polymer PBI concentration of 10wt% can obtain PBI fibers with a better structural morphology. Exemplarily, the raw material components of the spinning solution include: polybenzimidazole, potassium hydroxide and n-pentanol solution; wherein, by mass fraction, the content of polybenzimidazole is 10%, and the content of potassium hydroxide is 2%.
[0044] In some embodiments, the electrospinning process parameters include: spinning environment humidity, spinning environment temperature, spinning voltage and spinning distance; wherein,
[0045] The spinning environment humidity is 20% to 80%, the spinning environment temperature is 15° C. to 35° C., the spinning voltage is 18 kV to 22 kV, and the spinning distance is 10 cm to 30 cm.
[0046] In an embodiment of the present application, a strong base is dissolved in an organic alcohol solution, and the organic alcohol solution containing the strong base performs electrostatic spinning on polybenzimidazole; wherein, the spinning environment humidity and the spinning environment temperature will affect the solvent volatilization rate during the electrostatic spinning process. During the electrostatic spinning process, if the solvent evaporates too quickly, it will cause needle blockage to a certain extent, making it difficult to form fibers; and if it evaporates too slowly, it will be difficult to form fibers, and it will reach the receiving plate in a solution state. The spinning voltage can cause the solvent to be pulled out by the voltage to form electrostatic spinning. If the spinning voltage is too low, the fibers cannot be pulled out to a certain extent; if the spinning voltage is too high, the solvent will be adsorbed to a place outside the receiving plate to a certain extent. If the spinning distance is too close, it will be difficult to form fibers, and they will reach the receiving plate in a solution state; if the spinning distance is too far, the electrostatic field force will be too small, making it difficult for the receiving plate to receive the fibers. Exemplarily, the spinning environment humidity can be 20%, 30%, 40%, 50%, 60%, 70%, 80%, etc., the spinning environment temperature can be 15°C, 20°C, 25°C, 30°C, 35°C, etc., the spinning voltage can be 18kV, 19kV, 20kV, 21kV, 22kV, etc., and the spinning distance can be 10cm, 12cm, 14cm, 16cm, 18cm, 20cm, 22cm, 24cm, 26cm, 28cm, 30cm, etc.
[0047] In a second aspect, the present application provides a proton exchange membrane, wherein the raw material components of the proton exchange membrane include the nanofiber support skeleton material described in any one of the embodiments of the first aspect and a perfluorosulfonic acid resin solution (Nafion solution). Figure 4 This is a scanning electron microscope cross-sectional morphology of a proton exchange membrane provided in an embodiment of the present application; see Figure 4 , it was observed that the thickness of the proton exchange membrane was about 12 microns, and an obvious alkali-functionalized PBI spinning fiber skeleton could be observed in the middle of the membrane. And there was a strong ionic binding force between the skeleton and the interface of the proton exchange membrane. According to the mass measurement before and after the pore plugging, the mass fraction of the nanofiber support skeleton material support layer in the proton exchange membrane was 30%, and the mass fraction of the perfluorosulfonic acid resin was 70%.
[0048] In some embodiments, the solid content of the perfluorosulfonic acid resin solution is 5% to 10%.
[0049] In some embodiments, the solid content of the perfluorosulfonic acid resin solution is 8%.
[0050] In some embodiments, the proton exchange membrane meets the following properties: mechanical strength of 77 MPa to 86 MPa, elongation at break of 165% to 170%, and elastic modulus of 68 MPa to 76 MPa.
[0051] In an embodiment of the present application, a nanofiber support skeleton material is applied to a proton exchange membrane, and the alkali-functionalized nanofiber support skeleton material is hydrophilic in an ionic state, and the active metal cations therein can adsorb the sulfonic acid group of the perfluorosulfonic acid resin, and the ionic attraction between the active metal cations and the sulfonic acid group can enhance the binding force between the nanofiber support skeleton material and the perfluorosulfonic acid resin, thereby improving the strength of the proton exchange membrane. The solid content of the perfluorosulfonic acid resin solution is limited to 5% to 10%, because: the proton exchange membrane is fully formed, and the perfluorosulfonic acid resin solution is smoothly penetrated into the pores of the nanofiber support skeleton material. Exemplarily, the solid content of the perfluorosulfonic acid resin solution can be 5%, 6%, 7%, 8%, 9%, 10%, etc., and further, the solid content of the perfluorosulfonic acid resin solution can be 8%.
[0052] The above-mentioned proton exchange membrane meets the following mechanical properties: mechanical strength is 77MPa-86MPa; elongation at break can be 165%-170%; elastic modulus can be 68MPa-76MPa.
[0053] The proton exchange membrane is realized based on the above-mentioned nanofiber supported skeleton material. The specific raw material components and steps of the nanofiber supported skeleton material can refer to the above-mentioned embodiment. Since the proton exchange membrane adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.
[0054] In a third aspect, the present application provides a method for preparing a proton exchange membrane according to any one embodiment of the second aspect, Figure 5 A schematic diagram of a process for preparing a proton exchange membrane provided in an embodiment of the present application; see Figure 5 , the method comprising:
[0055] S1. Pour a perfluorosulfonic acid resin solution onto at least a portion of the surface of the nanofiber support skeleton material until no perfluorosulfonic acid resin solution remains on the surface of the nanofiber support skeleton material, and then dry to obtain a proton exchange membrane.
[0056] In some embodiments, the drying temperature is 40°C to 80°C.
[0057] In the embodiment of the present application, since the alkali-functionalized polybenzimidazole nanofiber support skeleton is relatively hydrophilic in ionic state, and the active metal cations can adsorb the sulfonic acid groups of the perfluorosulfonic acid resin, no vacuum is required, and direct casting can make the resin solution fully infiltrate into the gaps of the polybenzimidazole nanofiber support skeleton. After further drying in a 40℃~80℃ ordinary oven to form a film, the active metal cations on the interface surface of the support layer and the resin and the electrostatic ion pairs of the sulfonic acid groups can significantly increase the binding force between the two, providing the membrane with higher strength and service life. Finally, after performance testing, the mechanical strength of the membrane and the dry-wet cycle life of the single cell have been greatly improved.
[0058] For example, a suitable size of alkali-functionalized PBI fiber membrane is cut from the spun nanofiber support skeleton material (alkali-functionalized PBI electrospun fiber) and directly laid on a surface dish without any treatment. The diluted Solvay resin solution is used to coat the surface of the alkali-functionalized PBI spun fiber until there is no Nafion plugging liquid residue on the surface of the PBI fiber; the plugged membrane is taken out and laid on a glass plate, and dried at 40°C to 80°C to obtain a perfluorosulfonic acid proton exchange membrane with an alkali-functionalized PBI support layer.
[0059] The preparation method of the proton exchange membrane is implemented based on the above-mentioned proton exchange membrane. The specific raw material composition steps of the proton exchange membrane can refer to the above-mentioned embodiment. Since the preparation method of the proton exchange membrane adopts part or all of the technical solutions of the above-mentioned embodiment, it at least has all the beneficial effects brought by the technical solutions of the above-mentioned embodiment, which will not be repeated here one by one.
[0060] In a fourth aspect, the present application provides a fuel cell, comprising the proton exchange membrane described in any one embodiment of the second aspect.
[0061] The fuel cell is realized based on the above-mentioned proton exchange membrane. The specific raw material composition steps of the proton exchange membrane can refer to the above-mentioned embodiment. Since the fuel cell adopts part or all of the technical solutions of the above-mentioned embodiments, it has at least all the beneficial effects brought by the technical solutions of the above-mentioned embodiments, which will not be repeated here one by one.
[0062] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to national standards. If there is no corresponding national standard, then the conditions recommended by the manufacturer are followed.
[0063] Example 1
[0064] A nanofiber support skeleton material (alkali functionalized PBI electrospun fiber), the nanofiber support skeleton is prepared by electrostatic spinning of a spinning solution; the raw material components of the spinning solution include: polybenzimidazole, potassium hydroxide and n-pentanol; wherein, by mass fraction, the content of potassium hydroxide is 2%, and the content of polybenzimidazole is 10%; the process parameters of electrostatic spinning include: spinning environment humidity of 50%, spinning environment temperature of 25°C, spinning voltage of 20kV, and spinning distance of 20cm. Specifically, spinning is performed on a DFS-100 electrospinning test device under the conditions of spinning environment humidity (relative humidity) of 50%RH, spinning environment temperature of 25°C, propulsion rate of 0.001mL / min, spinning voltage of 20kV, spinning distance (distance from needle tip to receiver) of 20cm, and roller speed of 500r / min.
[0065] A method for preparing a proton exchange membrane comprises: adding water to a Nafion solution (25 wt%, pure water solution) purchased by Solvay and diluting it to a solid content of 8%. Cutting an alkali-functionalized PBI fiber membrane of a suitable size from the spun alkali-functionalized PBI electrospun fiber, and directly laying it flat on a surface dish without any treatment. Using the diluted Solvay resin solution to coat the surface of the alkali-functionalized PBI spun fiber until there is no Nafion plugging liquid residue on the surface of the PBI fiber. Taking out the plugged membrane and laying it flat on a glass plate, baking it in an oven at 60°C for 24 hours, a perfluorosulfonic acid proton exchange membrane with an alkali-functionalized PBI support layer can be obtained.
[0066] Example 2
[0067] A nanofiber support skeleton material (alkali functionalized PBI electrospun fiber), the nanofiber support skeleton is prepared by electrostatic spinning of a spinning solution; the raw material components of the spinning solution include: polybenzimidazole, potassium hydroxide and n-pentanol; wherein, by mass fraction, the content of potassium hydroxide is 2%, and the content of polybenzimidazole is 9%; the process parameters of electrostatic spinning include: spinning environment humidity of 30%, spinning environment temperature of 20°C, spinning voltage of 22kV, and spinning distance of 20cm. Specifically, spinning is performed on a DFS-100 electrospinning test device under the conditions of spinning environment humidity (relative humidity) of 30%RH, spinning environment temperature of 20°C, propulsion rate of 0.001mL / min, spinning voltage of 22kV, spinning distance (distance from needle tip to receiver) of 20cm, and roller speed of 500r / min.
[0068] A method for preparing a proton exchange membrane comprises: adding water to a Nafion solution (25 wt%, pure water solution) purchased by Solvay and diluting it to a solid content of 8 wt%. Cut an alkali-functionalized PBI fiber membrane of a suitable size from the spun alkali-functionalized PBI electrospun fiber, and directly lay it flat on a surface dish without any treatment. Use the diluted Solvay resin solution to coat the surface of the alkali-functionalized PBI spun fiber until there is no Nafion plugging liquid residue on the surface of the PBI fiber. Take out the plugged membrane and lay it flat on a glass plate, and bake it in an oven at 80°C for 12 hours to obtain a perfluorosulfonic acid proton exchange membrane with an alkali-functionalized PBI support layer.
[0069] Example 3
[0070] A nanofiber support skeleton material (alkali functionalized PBI electrospun fiber), the nanofiber support skeleton is prepared by electrostatic spinning of a spinning solution; the raw material components of the spinning solution include: polybenzimidazole, potassium hydroxide and n-pentanol; wherein, by mass fraction, the content of potassium hydroxide is 2%, and the content of polybenzimidazole is 11%; the process parameters of electrostatic spinning include: spinning environment humidity of 40%, spinning environment temperature of 20°C, spinning voltage of 18kV, and spinning distance of 20cm. Specifically, spinning is performed on a DFS-100 electrospinning test device under the conditions of spinning environment humidity (relative humidity) of 40%RH, spinning environment temperature of 20°C, propulsion rate of 0.001mL / min, spinning voltage of 18kV, spinning distance (distance from needle tip to receiver) of 20cm, and roller speed of 500r / min.
[0071] A method for preparing a proton exchange membrane comprises: adding water to a Nafion solution (25 wt%, pure water solution) purchased by Solvay and diluting it to a solid content of 8 wt%. Cutting an alkali-functionalized PBI fiber membrane of a suitable size from the spun alkali-functionalized PBI electrospun fiber, and directly laying it flat on a surface dish without any treatment. Using the diluted Solvay resin solution to coat the surface of the alkali-functionalized PBI spun fiber until there is no Nafion plugging liquid residue on the surface of the PBI fiber. Taking out the plugged membrane and laying it flat on a glass plate, baking it in an oven at 40°C for 24 hours, a perfluorosulfonic acid proton exchange membrane with an alkali-functionalized PBI support layer can be obtained.
[0072] Comparative Example 1
[0073] The Nafion solution purchased by Solvay (25 wt %, pure water solution) was diluted with water to a solid content of 8 wt %, and directly poured onto a glass plate without any treatment, and baked in an oven at 60° C. for 12 hours to obtain a conventional perfluorosulfonic acid proton exchange membrane.
[0074] The conductivity of the proton exchange membrane prepared in Examples 1 to 3 and Comparative Example 1 was characterized using a scribe740 device, and the EW value of the proton exchange membrane was characterized using an automatic titrator. The mechanical strength of the proton exchange membrane was characterized using a stretching machine, and the fuel cell performance of the proton exchange membrane was tested using a group 850e, and the dry-wet cycle performance was tested. For details, please refer to the conductivity of the proton exchange membrane shown in Table 1, the EW value of the proton exchange membrane shown in Table 2 (resin mass of 1 mol sulfonic acid group), and the mechanical strength of the proton exchange membrane shown in Table 3.
[0075] Table 1 Conductivity of proton exchange membrane
[0076]
[0077]
[0078] Table 2 EW values of proton exchange membranes
[0079] sample EW Example 1 850 Example 2 880 Example 3 875 Comparative Example 1 790
[0080] Table 3 Mechanical strength of proton exchange membrane
[0081] sample Mechanical strength (MPa) Elongation at break Elastic modulus (MPa) Example 1 85.3 170% 76.1 Example 2 82.6 165% 74.6 Example 3 77.8 168% 68.3 Comparative Example 1 23.9 90% 18.1
[0082] As can be seen from Table 1, since the conductivity of polybenzimidazole is lower than that of perfluorosulfonic acid resin, the comparative example without adding any PBI support layer has the highest conductivity value. As can be seen from Table 2, since polybenzimidazole does not contain sulfonate groups, the comparative example without adding PBI support layer has the lowest EW value. As can be seen from Table 3, since comparative example 1 is only a perfluorosulfonic acid resin membrane, the mechanical strength is relatively low. The addition of the alkali-functionalized polybenzimidazole nanofiber support skeleton in the embodiment of the present application makes the mechanical strength, elongation at break and elastic modulus of the proton exchange membrane reach a higher level.
[0083] Figure 6 A polarization curve diagram of the voltage of a membrane electrode of a proton exchange membrane provided in an embodiment of the present application in a fuel cell as a function of current density; Figure 7 A graph showing the power density of a membrane electrode of a proton exchange membrane in a fuel cell as a function of current density provided in an embodiment of the present application; see Figures 6-7 , Figure 6 and Figure 7 The proton membrane prepared in Example 1 and Comparative Example 1 is prepared under the same conditions as the membrane electrode and the polarization curve is tested in a fuel cell to obtain the curve of voltage and power density changing with current density. Figure 6 It can be seen from Example 1 that at 2000mA / cm 2At a current density of , the battery rated power can reach 0.678V, far exceeding the 0.633V of comparative example 1. Figure 7 It can be seen that Example 1 is at 2400mA / cm 2 At a current density of 1.544 mW / cm2, the battery power density can reach 1555.9 mW / cm2. 2 , far exceeding the 1424.1mW / cm of comparative example 1 2 The improvement ratio reached 9.2%. The battery performance of Example 1 was greatly improved compared with the fuel cell performance of Comparative Example 1, because its innovative PBI support skeleton greatly improved the dimensional stability of the proton membrane in the fuel cell. Figure 8 This is a graph showing the change of the open circuit voltage of a cell over time in a DOE dry-wet cycle mechanical durability test of a membrane electrode of a proton exchange membrane provided in an embodiment of the present application in a fuel cell; please refer to Figure 8 , indicating that the proton exchange membrane prepared in Example 1, thanks to its PBI nanospinning support layer with strong ion pair binding force, has a dry-wet cycle mechanical durability far exceeding that of Comparative Example 1. After running for 900 hours, the open circuit voltage has almost no decay, while the proton exchange membrane prepared in Comparative Example 1 has an open circuit voltage decay of 0.16 V compared with the initial value after running for 900 hours. The substantial improvement in dry-wet dry-wet cycle mechanical durability directly reflects the strong ion binding force between the PBI nanospinning support layer and the perfluorosulfonic acid resin, as well as its effect on improving the mechanical properties of the proton membrane.
[0084] From Table 3, it can be seen that the proton exchange membrane has high mechanical properties, and the dry-wet cycle performance test of the proton exchange membrane fuel cell shows that the dry-wet cycle performance of the fuel cell is good, which reflects the strong bonding force between the nanofiber support skeleton material and the perfluorosulfonic acid resin.
[0085] One or more technical solutions in the embodiments of the present application also have at least the following technical effects or advantages:
[0086] (1) Using a spinning solution containing polybenzimidazole, a strong base and an organic alcohol, an alkali-functionalized polybenzimidazole nanofiber support skeleton was prepared by a one-step electrospinning technique; since it was electrospun through an alkali solution, it directly contained alkali-functionalized benzimidazole anions and active metal cations;
[0087] (2) A perfluorosulfonic acid resin aqueous solution is used and diluted for plugging the pores of the alkali-functionalized polybenzimidazole nanofiber support skeleton. Since the alkali-functionalized polybenzimidazole nanofiber support skeleton is relatively hydrophilic in ionic state and the active metal cations can adsorb the sulfonic acid groups of the perfluorosulfonic acid resin, the resin solution can be fully infiltrated into the gaps of the polybenzimidazole nanofiber support skeleton by direct pouring without vacuum. After the membrane is formed, the electrostatic ion pairs of the active metal cations and the sulfonic acid groups on the interface surface of the support layer and the resin can significantly increase the binding force between the two, thereby providing the proton exchange membrane with higher strength and service life.
[0088] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A nanofiber support skeleton material, characterized in that: The nanofiber support skeleton is prepared by electrostatic spinning of a spinning solution; The raw material components of the spinning solution include: polybenzimidazole, strong base and organic alcohol; wherein, by mass fraction, The content of the polybenzimidazole is 5% to 20%, and the content of the strong base is 1% to 10%.
2. The nanofiber support skeleton material according to claim 1, characterized in that: The strong base includes at least one of the following: potassium hydroxide, sodium hydroxide, calcium hydroxide, and barium hydroxide.
3. The nanofiber support skeleton material according to claim 1, characterized in that: The organic alcohol includes at least one of the following: ethanol, n-butanol, isobutanol, n-propanol, isopropanol, n-pentanol, isopentanol, n-hexanol, and isopropanol.
4. The nanofiber support skeleton material according to any one of claims 1 to 3, characterized in that: The electrospinning process parameters include: spinning environment humidity, spinning environment temperature, spinning voltage and spinning distance; wherein, The spinning environment humidity is 20% to 80%, the spinning environment temperature is 15° C. to 35° C., the spinning voltage is 18 kV to 22 kV, and the spinning distance is 10 cm to 30 cm.
5. A proton exchange membrane, characterized in that: The raw material components of the proton exchange membrane include the nanofiber support skeleton material according to any one of claims 1 to 4 and a perfluorosulfonic acid resin solution.
6. The proton exchange membrane according to claim 5, characterized in that The solid content of the perfluorosulfonic acid resin solution is 5% to 10%.
7. The proton exchange membrane according to any one of claims 5 or 6, characterized in that: The proton exchange membrane meets the following mechanical properties: The mechanical strength is 77MPa-86MPa, the elongation at break is 165%-170%, and the elastic modulus is 68MPa-76MPa.
8. A method for preparing a proton exchange membrane according to any one of claims 5 to 7, characterized in that: The method comprises: The perfluorosulfonic acid resin solution is coated on at least a portion of the surface of the nanofiber support skeleton material until no perfluorosulfonic acid resin solution remains on the surface of the nanofiber support skeleton material, and then dried to obtain a proton exchange membrane.
9. The method according to claim 8, characterized in that The drying temperature is 40°C to 80°C.
10. A fuel cell, characterized in that: The fuel cell comprises the proton exchange membrane according to any one of claims 5 to 7.
Citation Information
Cited By
Multi-layer enhanced proton exchange membrane for flow battery and preparation method of multi-layer enhanced proton exchange membrane