Composite fiber material for decorative material and preparation method

By using composite fiber materials of polylactic acid, phosphorus-containing polylactic acid and biminimum-modified carbon nanotubes, the flammability and brittleness of polylactic acid fibers are solved, and the flame retardant, antibacterial and mechanical properties are improved, suitable for decoration Material.

CN118932547AInactive Publication Date: 2024-11-12ANHUI SOYA DECORATIVE MATERIALS
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411299461.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-18
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Polylactic fibers have flammable and brittle defects in decorative materials and have failed to effectively improve their antibacterial properties.

Method used

Using polylactic acid, phosphorus-containing polylactic acid and bimini quaternary ammonium modified carbon nanotubes as raw materials, composite fiber materials are prepared through melt extrusion and spinning processes, and using the flame retardant properties of phosphorus-containing polylactic acid and bimini quaternary ammonium modification The antibacterial properties of carbon nanotubes improve the flame retardant and antibacterial properties of the materials.

Benefits of technology

The prepared composite fiber material has excellent flame retardant properties, antibacterial properties and mechanical properties, and is suitable for decorative materials, improving the application value of polylactic fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932547A_ABST
    Figure CN118932547A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of fiber materials, and discloses a composite fiber material for a decorative material and a preparation method thereof.( 4, 4 '-(phenylphosphoryl) bis (piperazine-4, 1-diyl)) diethylene is synthesized with 1-allyl piperazine and phenylphosphoryl dichloride as raw materials and triethylamine as a catalyst, the structure is novel, the preparation method is simple, and the composite fiber material is suitable for industrial production. Under the initiation of dicumyl peroxide, the phosphorus-containing polylactic acid and maleic anhydride are copolymerized and grafted to polylactic acid to obtain the phosphorus-containing polylactic acid. The preparation method comprises the following steps: by taking 1, 2-bis (diethylamino) ethane and epoxy chloropropane as raw materials, carrying out quaternization to obtain an epoxy gemini quaternary ammonium salt intermediate, and then carrying out epoxy ring opening on the epoxy gemini quaternary ammonium salt intermediate and an oxidized multi-arm carbon nanotube to obtain the gemini quaternary ammonium salt modified carbon nanotube. Finally, polylactic acid, phosphorus-containing polylactic acid and the gemini quaternary ammonium salt modified carbon nanotubes are subjected to extrusion granulation and spinning, and the composite fiber material for the decorative material is obtained. The prepared composite fiber for decoration has good flame retardant property, antibacterial property and mechanical property.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of fiber materials, in particular to a composite fiber material for decorative materials and a preparation method thereof. Background Art

[0002] As people's awareness of energy and environmental protection continues to increase, renewable and degradable bio-based polymer materials have received widespread attention. Among them, the bio-based polymer material polylactic acid is widely used in medical agriculture, rail transportation and other fields due to its high transparency, excellent mechanical strength and easy processing. The polylactic acid fiber prepared from polylactic acid has good high strength and biocompatibility, and is widely used in decorative items such as bed sheets and curtains. However, polylactic acid has flammable and brittle defects, so it needs to be modified to improve the application of polylactic acid fiber in decorative materials.

[0003] For example, the patent with the authorization announcement number CN 105754082 B discloses a phosphorus-containing ionomer copolymer flame-retardant polylactic acid fiber and its preparation method. The invention prepares a phosphorus-containing ionomer comonomer, and then reacts it with lactide through a ring-opening polymerization reaction to obtain a phosphorus-containing ionomer copolymer flame-retardant polylactic acid, and finally melt-spins to obtain a phosphorus-containing ionomer copolymer flame-retardant polylactic acid fiber. The polylactic acid fiber prepared by the invention has excellent flame retardant properties and mechanical properties, and can be used in the fields of automotive interiors, decorative materials, clothing and home textiles. However, the antibacterial properties of polylactic acid fibers are not improved. Summary of the invention

[0004] The technical problem to be solved by the present invention is to provide a composite fiber material for decorative materials and a preparation method thereof, using green and environmentally friendly polylactic acid as a raw material to prepare the composite fiber material for decoration having good environmental performance, excellent flame retardant properties, mechanical properties and antibacterial properties.

[0005] The technical solution adopted by the present invention is: a composite fiber material for decorative materials, which is prepared from the following raw materials in parts by weight: 100 parts of polylactic acid, 50-100 parts of phosphorus-containing polylactic acid, and 5-20 parts of gemini quaternary ammonium salt-modified carbon nanotubes;

[0006] According to the above technical solution, preferably, the method for preparing the composite fiber material comprises the following steps:

[0007] Polylactic acid, phosphorus-containing polylactic acid and gemini quaternary ammonium salt-modified carbon nanotubes are added to a twin-screw melt extruder at 180°C for extrusion granulation, then added to a spinning machine for spinning, and finally cooled, oiled, stretched and wound to obtain a composite fiber material for decorative materials.

[0008] According to the above technical solution, preferably, the temperature of the spinning machine is 200-240°C, the spinning speed is 800-1000m / min; and the stretching temperature is 80°C.

[0009] According to the above technical solution, preferably, the preparation method of the phosphorus-containing polylactic acid is:

[0010] (1) Under a nitrogen atmosphere, the temperature is controlled at -5 to 0°C, 1-allylpiperazine is added to an acetone solvent, stirred to dissolve, and then phenylphosphoryl dichloride and triethylamine are added thereto, stirred to react for 20-50 minutes, the temperature is raised to 20-30°C, and the reaction is continued for 1-4 hours. After the reaction is completed, the mixture is washed with deionized water, allowed to stand, the lower layer of liquid is separated, concentrated, and dried to obtain (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))bisethylene;

[0011] (2) maleic anhydride and dicumyl peroxide are dissolved in acetone solvent, polylactic acid is added thereto, the mixture is stirred and mixed evenly, dried, and transferred to a torque rheometer at a speed of 50 r / min, (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))ethylene is added thereto, and melt grafting reaction is carried out at 170-180°C for 6-15 minutes. After the reaction is completed, chloroform is refluxed for purification, ethanol precipitation is performed, filtration is performed, washing is performed, and drying is performed to obtain phosphorus-containing polylactic acid.

[0012] According to the above technical solution, in a more preferred case, in (1), the weight ratio of 1-allylpiperazine, phenylphosphoryl dichloride and triethylamine is (12-16):10:(10-12).

[0013] According to the above technical solution, in a more preferred case, in (2), the weight ratio of maleic anhydride, diisopropylbenzene peroxide, polylactic acid, and (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))ethylenediamine is (2-5):(0.4-0.8):100:(1-10).

[0014] According to the above technical solution, preferably, the preparation method of the gemini quaternary ammonium salt modified carbon nanotubes is:

[0015] S1. Under a nitrogen atmosphere, 1,2-bis(diethylamino)ethane and epichlorohydrin are added to an ethanol solvent, stirred and dispersed, and stirred and reacted at 25-40° C. for 3-6 hours. After the reaction is completed, vacuum distillation is performed, cooling, suction filtration, and drying to obtain an epoxy gemini quaternary ammonium salt intermediate;

[0016] S2. Under a nitrogen atmosphere, add the oxidized multi-arm carbon nanotubes to deionized water, disperse them ultrasonically, add the epoxy gemini quaternary ammonium salt intermediate and triethylamine aqueous solution, stir and react at 65-75°C for 24-36 hours. After the reaction is completed, filter, wash with acetone, and dry to obtain gemini quaternary ammonium salt modified carbon nanotubes.

[0017] According to the above technical solution, in a more preferred case, in S1, the weight ratio of 1,2-bis(diethylamino)ethane to epichlorohydrin is 10:(10-14).

[0018] According to the above technical solution, in a more preferred case, in S2, the weight ratio of the oxidized multi-arm carbon nanotubes to the epoxy gemini quaternary ammonium salt intermediate is 10:(3-5).

[0019] According to the above technical solution, in a more preferred case, in S2, the mass fraction of the triethylamine aqueous solution is 25%.

[0020] The beneficial effects of the present invention are:

[0021] The present invention prepares phosphorus-containing polylactic acid and gemini quaternary ammonium salt-modified carbon nanotubes through a series of reactions, utilizes the flame retardant elements contained in the phosphorus-containing polylactic acid to perform flame retardancy, and the gemini quaternary ammonium salt in the gemini quaternary ammonium salt-modified carbon nanotubes performs antibacterial, and the decorative composite fiber material obtained by further spinning the two and polylactic acid has good antibacterial and flame retardant properties. Since the carbon nanotubes used in the present invention are easy to agglomerate, the present invention organicizes them, increases their dispersibility in organic matter, and evenly disperses them in the decorative composite fiber material. When subjected to external force, they can serve as stress concentration points, absorb more energy, and then increase the mechanical properties of the composite fiber material. The decorative composite fiber prepared by the present invention has good flame retardancy, antibacterial and mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a reaction route of 4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))bisethylene;

[0023] Figure 2 This is the reaction route for modifying carbon nanotubes with gemini quaternary ammonium salts. DETAILED DESCRIPTION

[0024] 1 g of multi-arm carbon nanotubes was added to 200 mL of mixed acid (sulfuric acid and nitric acid in a volume ratio of 3:1), ultrasonically dispersed for 30 min, refluxed and stirred at 80°C for 30 min, and after the reaction was completed, cooled to room temperature, deionized water was added, centrifuged, filtered, and dried to obtain oxidized multi-arm carbon nanotubes.

[0025] The following non-limiting embodiments may enable a person skilled in the art to more fully understand the present invention, but are not intended to limit the present invention in any way.

[0026] The present invention provides a method for preparing a composite fiber material for decoration, comprising the following steps:

[0027] (1) Under a nitrogen atmosphere, the temperature is controlled at -5 to 0°C, 12-16 parts by weight of 1-allylpiperazine is added to an acetone solvent, stirred to dissolve, and then 10 parts of phenylphosphoryl dichloride and 10-12 parts of triethylamine are added thereto, stirred to react for 20-50 minutes, the temperature is raised to 20-30°C, and the reaction is continued for 1-4 hours. After the reaction is completed, the mixture is washed with deionized water, allowed to stand, the lower layer of liquid is separated, concentrated, and dried to obtain (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))bisethylene.

[0028] (2) Dissolve 2-5 parts of maleic anhydride and 0.4-0.8 parts of dicumyl peroxide in acetone solvent by weight, add 100 parts of polylactic acid thereto, stir and mix evenly, dry, transfer it to a torque rheometer at a speed of 50 r / min, add 1-10 parts of (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))ethylenediamine, carry out melt grafting reaction at 170-180°C for 6-15 minutes, and after the reaction is completed, reflux chloroform for purification, precipitate with ethanol, filter, wash, and dry to obtain phosphorus-containing polylactic acid.

[0029] (3) Under a nitrogen atmosphere, 10 parts by weight of 1,2-bis(diethylamino)ethane and 10-14 parts of epichlorohydrin are added to an ethanol solvent, stirred and dispersed, and stirred and reacted at 25-40° C. for 3-6 hours. After the reaction is completed, the mixture is distilled under reduced pressure, cooled, filtered, and dried to obtain an epoxy gemini quaternary ammonium salt intermediate.

[0030] (4) Under a nitrogen atmosphere, 10 parts by weight of oxidized multi-arm carbon nanotubes are added to deionized water, and ultrasonic dispersion is performed. Then, 3-5 parts of epoxy gemini quaternary ammonium salt intermediate and 25% triethylamine aqueous solution are added thereto, and the mixture is stirred and reacted at 65-75° C. for 24-36 hours. After the reaction is completed, the mixture is filtered, washed with acetone, and dried to obtain gemini quaternary ammonium salt-modified carbon nanotubes.

[0031] (5) According to weight, 100 parts of polylactic acid, 50-100 parts of phosphorus-containing polylactic acid, and 5-20 parts of gemini quaternary ammonium salt-modified carbon nanotubes are added to a twin-screw melt extruder at 180°C for extrusion granulation, and then added to a spinning machine for spinning, and finally cooled, oiled, stretched, and wound, wherein the temperature of the spinning machine is 200-240°C, the spinning speed is 800-1000m / min, and the stretching temperature is 80°C, to obtain a composite fiber material for decorative materials.

[0032] Below, the present invention will be described in detail in conjunction with specific embodiments. Before describing, it should be understood that the terms used in this specification and the attached claims should not be interpreted as being limited to the general meaning and dictionary meaning, but should be interpreted according to the meaning and concept corresponding to the technical aspects of the present invention on the basis of the principle that the inventor is allowed to appropriately define the terms for the best interpretation. Therefore, the descriptions presented here are only preferred examples for illustrative purposes and are not intended to limit the scope of the present invention, so that it should be understood that other equivalents or improvements can be obtained therefrom without departing from the spirit and scope of the present invention.

[0033] Example 1

[0034] (1) Under a nitrogen atmosphere, the temperature was controlled at -5°C. 12 parts by weight of 1-allylpiperazine were added to an acetone solvent and stirred to dissolve. Then, 10 parts of phenylphosphoryl dichloride and 12 parts of triethylamine were added thereto. The mixture was stirred for 40 minutes. The temperature was raised to 25°C and the reaction was continued for 4 hours. After the reaction was completed, the mixture was washed with deionized water, allowed to stand, the lower layer of liquid was separated, concentrated, and dried to obtain (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))bisethylene.

[0035] (2) 4 parts of maleic anhydride and 0.5 parts of diisopropylbenzene peroxide were dissolved in acetone solvent by weight, 100 parts of polylactic acid were added thereto, the mixture was stirred and mixed evenly, dried, and transferred to a torque rheometer at a speed of 50 r / min, 1 part of (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))ethylene was added thereto, and melt grafting reaction was carried out at 180°C for 10 minutes. After the reaction was completed, chloroform was refluxed for purification, ethanol was precipitated, filtered, washed, and dried to obtain phosphorus-containing polylactic acid.

[0036] (3) Under a nitrogen atmosphere, 10 parts by weight of 1,2-bis(diethylamino)ethane and 10 parts of epichlorohydrin are added to an ethanol solvent, stirred and dispersed, and stirred and reacted at 40° C. for 5 hours. After the reaction is completed, the mixture is distilled under reduced pressure, cooled, filtered, and dried to obtain an epoxy gemini quaternary ammonium salt intermediate.

[0037] (4) Under a nitrogen atmosphere, 10 parts by weight of oxidized multi-arm carbon nanotubes were added to deionized water and ultrasonically dispersed, and then 3 parts of epoxy gemini quaternary ammonium salt intermediate and 25% triethylamine aqueous solution were added thereto. The reaction was stirred at 70° C. for 32 hours. After the reaction was completed, the mixture was filtered, washed with acetone, and dried to obtain gemini quaternary ammonium salt-modified carbon nanotubes.

[0038] (5) According to weight, 100 parts of polylactic acid, 50 parts of phosphorus-containing polylactic acid, and 5 parts of gemini quaternary ammonium salt-modified carbon nanotubes are added to a twin-screw melt extruder at 180°C for extrusion granulation, and then added to a spinning machine for spinning, and finally cooled, oiled, stretched, and wound. The temperature of the spinning machine is 200°C, the spinning speed is 1000m / min, and the stretching temperature is 80°C to obtain a composite fiber material for decorative materials.

[0039] Example 2

[0040] (1) Under a nitrogen atmosphere, the temperature was controlled at 0°C. 16 parts by weight of 1-allylpiperazine were added to an acetone solvent and stirred to dissolve. Then, 10 parts of phenylphosphoryl dichloride and 12 parts of triethylamine were added thereto. The mixture was stirred for reaction for 50 minutes. The temperature was raised to 20°C and the reaction was continued for 3 hours. After the reaction was completed, the mixture was washed with deionized water, allowed to stand, the lower layer of liquid was separated, concentrated, and dried to obtain (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))bisethylene.

[0041] (2) Dissolve 5 parts of maleic anhydride and 0.8 parts of dicumyl peroxide in acetone solvent by weight, add 100 parts of polylactic acid thereto, stir and mix evenly, dry, transfer it to a torque rheometer at a speed of 50 r / min, add 4 parts of (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))ethylenediamine, and carry out melt grafting reaction at 180°C for 6 minutes. After the reaction is completed, reflux chloroform for purification, precipitate with ethanol, filter, wash, and dry to obtain phosphorus-containing polylactic acid.

[0042] (3) Under a nitrogen atmosphere, 10 parts by weight of 1,2-bis(diethylamino)ethane and 14 parts of epichlorohydrin are added to an ethanol solvent, stirred and dispersed, and stirred and reacted at 30° C. for 6 hours. After the reaction is completed, the mixture is distilled under reduced pressure, cooled, filtered, and dried to obtain an epoxy gemini quaternary ammonium salt intermediate.

[0043] (4) Under a nitrogen atmosphere, 10 parts by weight of oxidized multi-arm carbon nanotubes were added to deionized water and ultrasonically dispersed, and then 4 parts of epoxy gemini quaternary ammonium salt intermediate and 25% triethylamine aqueous solution were added thereto. The reaction was stirred at 75° C. for 30 hours. After the reaction was completed, the mixture was filtered, washed with acetone, and dried to obtain gemini quaternary ammonium salt-modified carbon nanotubes.

[0044] (5) According to weight, 100 parts of polylactic acid, 75 parts of phosphorus-containing polylactic acid, and 10 parts of gemini quaternary ammonium salt-modified carbon nanotubes are added to a twin-screw melt extruder at 180°C for extrusion granulation, and then added to a spinning machine for spinning, and finally cooled, oiled, stretched, and wound. The temperature of the spinning machine is 220°C, the spinning speed is 800m / min, and the stretching temperature is 80°C to obtain a composite fiber material for decorative materials.

[0045] Example 3

[0046] (1) Under a nitrogen atmosphere, the temperature was controlled at 0°C. 15 parts by weight of 1-allylpiperazine were added to an acetone solvent and stirred to dissolve. Then, 10 parts of phenylphosphoryl dichloride and 10 parts of triethylamine were added thereto. The mixture was stirred for reaction for 20 minutes. The temperature was raised to 30°C and the reaction was continued for 1 hour. After the reaction was completed, the mixture was washed with deionized water, allowed to stand, the lower layer of liquid was separated, concentrated, and dried to obtain (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))bisethylene.

[0047] (2) 4 parts of maleic anhydride and 0.4 parts of dicumyl peroxide were dissolved in acetone solvent by weight, 100 parts of polylactic acid were added thereto, the mixture was stirred and mixed evenly, dried, and transferred to a torque rheometer at a speed of 50 r / min, 6 parts of (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))ethylene were added thereto, and melt grafting reaction was carried out at 170°C for 15 minutes. After the reaction was completed, chloroform was refluxed for purification, ethanol was precipitated, filtered, washed, and dried to obtain phosphorus-containing polylactic acid.

[0048] (3) Under a nitrogen atmosphere, 10 parts by weight of 1,2-bis(diethylamino)ethane and 12 parts of epichlorohydrin are added to an ethanol solvent, stirred and dispersed, and stirred and reacted at 25° C. for 3 hours. After the reaction is completed, the mixture is distilled under reduced pressure, cooled, filtered, and dried to obtain an epoxy gemini quaternary ammonium salt intermediate.

[0049] (4) Under a nitrogen atmosphere, 10 parts by weight of oxidized multi-arm carbon nanotubes were added to deionized water and ultrasonically dispersed, and then 5 parts of epoxy gemini quaternary ammonium salt intermediate and 25% triethylamine aqueous solution were added thereto. The reaction was stirred at 65° C. for 24 hours. After the reaction was completed, the mixture was filtered, washed with acetone, and dried to obtain gemini quaternary ammonium salt-modified carbon nanotubes.

[0050] (5) According to weight, 100 parts of polylactic acid, 85 parts of phosphorus-containing polylactic acid, and 15 parts of gemini quaternary ammonium salt-modified carbon nanotubes are added to a twin-screw melt extruder at 180°C for extrusion granulation, and then added to a spinning machine for spinning, and finally cooled, oiled, stretched, and wound. The temperature of the spinning machine is 240°C, the spinning speed is 900m / min, and the stretching temperature is 80°C to obtain a composite fiber material for decorative materials.

[0051] Example 4

[0052] (1) Under a nitrogen atmosphere, the temperature was controlled at -5°C. 15 parts by weight of 1-allylpiperazine were added to an acetone solvent and stirred to dissolve. Then, 10 parts of phenylphosphoryl dichloride and 12 parts of triethylamine were added thereto. The mixture was stirred for reaction for 50 minutes. The temperature was raised to 25°C and the reaction was continued for 2 hours. After the reaction was completed, the mixture was washed with deionized water, allowed to stand, the lower layer of liquid was separated, concentrated, and dried to obtain (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))bisethylene.

[0053] (2) 2 parts by weight of maleic anhydride and 0.5 parts of dicumyl peroxide were dissolved in acetone solvent, 100 parts of polylactic acid were added thereto, the mixture was stirred and mixed evenly, dried, and transferred to a torque rheometer at a speed of 50 r / min, 10 parts of (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))ethylene were added thereto, and melt grafting reaction was carried out at 175°C for 10 minutes. After the reaction was completed, chloroform was refluxed for purification, ethanol was precipitated, filtered, washed, and dried to obtain phosphorus-containing polylactic acid.

[0054] (3) Under a nitrogen atmosphere, 10 parts by weight of 1,2-bis(diethylamino)ethane and 12 parts of epichlorohydrin are added to an ethanol solvent, stirred and dispersed, and stirred and reacted at 30° C. for 5 hours. After the reaction is completed, the mixture is distilled under reduced pressure, cooled, filtered, and dried to obtain an epoxy gemini quaternary ammonium salt intermediate.

[0055] (4) Under a nitrogen atmosphere, 10 parts by weight of oxidized multi-arm carbon nanotubes were added to deionized water and ultrasonically dispersed, and then 5 parts of epoxy gemini quaternary ammonium salt intermediate and 25% triethylamine aqueous solution were added thereto. The reaction was stirred at 70° C. for 36 hours. After the reaction was completed, the mixture was filtered, washed with acetone, and dried to obtain gemini quaternary ammonium salt-modified carbon nanotubes.

[0056] (5) According to weight, 100 parts of polylactic acid, 100 parts of phosphorus-containing polylactic acid, and 20 parts of gemini quaternary ammonium salt-modified carbon nanotubes are added to a twin-screw melt extruder at 180°C for extrusion granulation, and then added to a spinning machine for spinning, and finally cooled, oiled, stretched, and wound. The temperature of the spinning machine is 220°C, the spinning speed is 1000m / min, and the stretching temperature is 80°C to obtain a composite fiber material for decorative materials.

[0057] Comparative Example 1

[0058] The difference between this comparative example and Example 1 is that in step (5), phosphorus-containing polylactic acid is not contained.

[0059] Comparative Example 2

[0060] The difference between this comparative example and Example 1 is that in step (5), carbon nanotubes are used instead of carbon nanotubes modified by gemini quaternary ammonium salts.

[0061] Mechanical properties test:

[0062] The test was carried out using a chemical fiber filament electronic strength tester with a clamping distance of 200mm.

[0063] Table 1: Mechanical properties test results of various embodiments and comparative examples

[0064] Breaking strength / (cN / dtex) Example 1 1.54 Example 2 1.69 Example 3 1.78 Example 4 1.75 Comparative Example 1 1.48 Comparative Example 2 1.35

[0065] It can be seen from the table that the breaking strength of Examples 1-5 and Comparative Example 1 is greater than that of Comparative Example 2. This is because the carbon nanotubes in Comparative Example 2 are not modified, have large surface energy, and are easy to agglomerate. Therefore, their mechanical properties are not as good as those of Examples 1-5 and Comparative Example 1, and the maximum breaking strength can reach 1.78 cN / dtex.

[0066] Flame retardant performance test:

[0067] Use a vertical burning tester to test the vertical burning level;

[0068] Use a limiting oxygen index meter to test the oxygen index.

[0069] Table 2: Flame retardant performance test results of various embodiments and comparative examples

[0070]

[0071]

[0072] It can be seen from the table that the flame retardant properties of Examples 1-5 and Comparative Example 2 are better than that of Comparative Example 1. Therefore, the composite fiber material prepared in the present invention has better flame retardant properties.

[0073] Antibacterial performance test: The improved shaking flask method was used according to GB15979-2002. The inhibition rate (%) = (average colony count before sample shaking - average colony count after sample shaking) / average colony count before sample shaking × 100%. The test colonies were Staphylococcus aureus and Escherichia coli.

[0074] Table 3: Antibacterial performance test results of various embodiments and comparative examples

[0075]

[0076] It can be seen from the table that the antibacterial properties of Examples 1-5 and Comparative Example 1 are better than those of Comparative Example 2. This is because Examples 1-5 and Comparative Example 1 contain a gemini quaternary ammonium salt structure, which has a good antibacterial effect, and the maximum antibacterial rates for Staphylococcus aureus and Escherichia coli can reach 94.1% and 89.7% respectively.

Claims

1. A composite fiber material for decorative materials, characterized in that: The composite fiber material for decorative materials is prepared from the following raw materials in parts by weight: 100 parts by weight of polylactic acid, 50-100 parts by weight of phosphorus-containing polylactic acid, and 5-20 parts by weight of gemini quaternary ammonium salt-modified carbon nanotubes; The method for preparing the composite fiber material comprises the following steps: Polylactic acid, phosphorus-containing polylactic acid and gemini quaternary ammonium salt-modified carbon nanotubes are added to a twin-screw melt extruder at 180°C for extrusion granulation, then added to a spinning machine for spinning, and finally cooled, oiled, stretched and wound to obtain a composite fiber material for decorative materials.

2. The composite fiber material for decorative materials according to claim 1, characterized in that: The temperature of the spinning machine is 200-240°C, the spinning speed is 800-1000m / min; and the stretching temperature is 80°C.

3. The composite fiber material for decorative materials according to claim 1, characterized in that: The preparation method of the phosphorus-containing polylactic acid is: (1) Under a nitrogen atmosphere, the temperature is controlled at -5 to 0°C, 1-allylpiperazine is added to an acetone solvent, stirred to dissolve, and then phenylphosphoryl dichloride and triethylamine are added thereto, stirred to react for 20-50 minutes, the temperature is raised to 20-30°C, and the reaction is continued for 1-4 hours. After the reaction is completed, the mixture is washed with deionized water, allowed to stand, the lower layer of liquid is separated, concentrated, and dried to obtain (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))bisethylene; (2) maleic anhydride and dicumyl peroxide are dissolved in acetone solvent, polylactic acid is added thereto, the mixture is stirred and mixed evenly, dried, and transferred to a torque rheometer at a speed of 50 r / min, (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))ethylene is added thereto, and melt grafting reaction is carried out at 170-180°C for 6-15 minutes. After the reaction is completed, chloroform is refluxed for purification, ethanol precipitation is performed, filtration is performed, washing is performed, and drying is performed to obtain phosphorus-containing polylactic acid.

4. The composite fiber material for decorative materials according to claim 3, characterized in that: In the above (1), the weight ratio of 1-allylpiperazine, phenylphosphoryl dichloride and triethylamine is (12-16):10:(10-12).

5. The composite fiber material for decorative materials according to claim 3, characterized in that: In the above (2), the weight ratio of maleic anhydride, dicumyl peroxide, polylactic acid, and (4,4'-(phenylphosphoryl)bis(piperazine-4,1-diyl))ethylene is (2-5):(0.4-0.8):100:(1-10).

6. The composite fiber material for decorative materials according to claim 1, characterized in that: The preparation method of the gemini quaternary ammonium salt modified carbon nanotubes is: S1. Under a nitrogen atmosphere, 1,2-bis(diethylamino)ethane and epichlorohydrin are added to an ethanol solvent, stirred and dispersed, and stirred and reacted at 25-40° C. for 3-6 hours. After the reaction is completed, vacuum distillation is performed, cooling, suction filtration, and drying to obtain an epoxy gemini quaternary ammonium salt intermediate; S2. Under a nitrogen atmosphere, add the oxidized multi-arm carbon nanotubes to deionized water, disperse them ultrasonically, add the epoxy gemini quaternary ammonium salt intermediate and triethylamine aqueous solution, stir and react at 65-75°C for 24-36 hours. After the reaction is completed, filter, wash with acetone, and dry to obtain gemini quaternary ammonium salt modified carbon nanotubes.

7. The composite fiber material for decorative materials according to claim 6, characterized in that: In the S1, the weight ratio of 1,2-bis(diethylamino)ethane to epichlorohydrin is 100:(100-140).

8. The composite fiber material for decorative materials according to claim 6, characterized in that: In the S2, the weight ratio of the oxidized multi-arm carbon nanotubes to the epoxy gemini quaternary ammonium salt intermediate is 100:(30-50).

9. The composite fiber material for decorative materials according to claim 6, characterized in that: In the S2, the mass fraction of the triethylamine aqueous solution is 25%.

Citation Information

Patent Citations

  • Functionalized carbon nanotube flame-retardant polylactic acid and preparation method thereof

    CN102329487A

  • Double-reaction-active-group double-cationic-group cation modifier, and preparation method and application thereof

    CN104086511A

  • Phosphorus ionomer copolymerized flame-retardant polylactic acid fiber and preparation method thereof

    CN105754082A

  • Carbon-nanotube-containing high-toughness flame-retardant polylactic acid composite material and preparation method thereof

    CN108659488A

  • Modified cationic compound and preparation method thereof, and solid phase chemical cleaning agent for drilling fluids

    CN109912545A