Biodegradable bacterial cellulose / high-chlorine imidazolate composite piezoelectric fiber

Through the preparation of bacterial cellulose and perchlorimidazole composite materials, the problem of non-degradable fibers is solved, and biodegradable piezoelectric fibers are realized, with high voltage electrical coefficient and sensitivity, suitable for healthy exercise monitoring.

CN118932567APending Publication Date: 2024-11-12HUBEI UNIV OF SCI & TECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410988189.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The fibers of existing piezoelectric sensor parts are mainly made of non-degradable materials, resulting in environmental pollution and waste of resources, and lack of biodegradable solutions.

Method used

The perchlorimidazole crystal is prepared by dissolving imidazole and perchloric acid, and combined with the bacterial cellulose material, and then mechanically stretching and polarizing treatment to prepare bio-enabled Degraded piezoelectric fibers.

Benefits of technology

The low-cost, degradable piezoelectric fibers are achieved, with high voltage electrical coefficients and sensitivity, reducing resource waste and showing potential applications in health exercise monitoring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932567A_ABST
    Figure CN118932567A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of biodegradable bacterial cellulose / high-chlorine imidazolate composite piezoelectric fibers, which comprises the following steps: S1, dissolving imidazole and perchloric acid in distilled water, and uniformly stirring to obtain a mixed solution; s2, putting the mixed solution into a drying oven, and obtaining a high-chlorine imidazolate crystal along with evaporation of the liquid; s3, dissolving the high-chlorine imidazolate crystal in distilled water to obtain a high-chlorine imidazolate solution; s4, the strip-shaped BC bacterial fiber membrane element material is soaked in a high-chlorine imidazolate solution, the material is placed in a drying oven after shaking table oscillation, and after the solution is evaporated, a BC / ImClO4 compound is obtained; and S5, mechanically stretching the BC / ImClO4 compound, twisting the BC / ImClO4 compound into a linear shape, and shaping the BC / ImClO4 compound in a stretched state to obtain the BC / ImClO4 composite piezoelectric fiber. The BC / ImClO4 composite piezoelectric fiber provided by the invention is simple in preparation process and low in cost, and the composite piezoelectric fiber has good flexibility, biodegradability, rich ImClO4 crystal content and excellent piezoelectric property, and is of great significance to development of green and degradable flexible sensing fabrics.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of piezoelectric sensor devices and functional fabrics, and in particular relates to a biodegradable bacterial cellulose / perchloroimidazole salt composite piezoelectric fiber. Background Art

[0002] With the development of society and the advent of the era of the Internet of Everything, functional sensing fabrics have become the focus of research in the field of wearable devices due to their good flexibility, high comfort and fast heat dissipation. Fibers, as the smallest component of fabrics, have naturally become a research hotspot for their functional preparation. Among them, sensing fabrics for monitoring human mechanical signals have been studied most extensively and maturely. These sensing fabrics include resistive strain sensing fabrics, capacitive sensing fabrics, piezoelectric fabrics, triboelectric fabrics, magnetoelectric fabrics, etc. Among them, piezoelectric fabrics have the characteristics of high sensitivity and fast response speed, and are widely used in monitoring human mechanical movement, heart rate and heartbeat, sleep and breathing.

[0003] However, the fibers currently used to make piezoelectric sensing fabrics are mainly composed of non-degradable polymers and piezoelectric ceramics or polyvinylidene fluoride composites. The functional piezoelectric materials are also non-degradable and non-recyclable, which will produce plastic waste, causing environmental pollution and natural waste.

[0004] Therefore, it is of great significance to prepare a biodegradable bacterial cellulose / perchloroimidazole composite piezoelectric fiber. Summary of the invention

[0005] In order to solve the defects of the prior art, the present invention provides a biodegradable bacterial cellulose / perchloroimidazole salt composite piezoelectric fiber.

[0006] In order to solve the above technical problems, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing biodegradable bacterial cellulose / perchloridized imidazolate composite piezoelectric fiber, comprising the following steps:

[0008] S1, dissolving imidazole and perchloric acid in distilled water, and stirring to obtain a mixed solution;

[0009] S2, placing the mixed solution obtained in step S1 in an oven, and obtaining high-chloride imidazolate crystals (ImClO4) as the liquid evaporates;

[0010] S3, dissolving the high-chloride imidazolate crystals obtained in step S2 in distilled water to obtain a high-chloride imidazolate solution;

[0011] S4, soaking the strip-shaped BC bacterial cellulose material in the high-chloride imidazolate solution obtained in step S3, shaking on a shaker, and placing it in an oven, and after the solution evaporates, obtaining a BC / ImClO4 complex;

[0012] S5, mechanically stretching and twisting the BC / ImClO4 composite obtained in step S4 into a linear shape, and shaping it in the stretched state to obtain a BC / ImClO4 composite piezoelectric fiber.

[0013] Preferably, the concentration range of imidazole in step S1 is 0.05-0.5 mol / L; the concentration range of perchloric acid in step S1 is 0.05-0.5 mol / L.

[0014] Preferably, the temperature range of the oven in step S2 is 40 to 80° C., and the liquid evaporation time is 72 to 120 hours.

[0015] Preferably, the concentration of the high-chloride imidazolate solution in step S3 is 0.01-0.2 mol / L.

[0016] Preferably, the strip-shaped BC bacterial cellulose membrane material in step S4 is prepared by the following steps: cutting semi-dehydrated BC bacterial cellulose membrane into strips, soaking in distilled water to swell and remove impurities, and removing part of the water by mechanical compression to obtain a strip-shaped BC bacterial cellulose membrane material, and the weight loss rate of the bacterial cellulose hydrogel after mechanical compression is 50-90%.

[0017] Preferably, the strip-shaped BC bacterial cellulose material has a thickness of 1 to 3 mm, a width of 4 to 8 mm, and a crystallinity of 85 to 95%.

[0018] Preferably, the shaking speed of the shaking table is 100-150 rpm, and the shaking time is 30 to 120 minutes.

[0019] Preferably, the length of the product after stretching in step S5 changes to 110-120% of the original length, and the length of the twisted fiber changes to 85-95% of the original length.

[0020] Preferably, the tension range for maintaining the stretched state in step S5 is 0.2 to 2N, the drying temperature is 25 to 80°C, and the drying and setting time is 1 to 2 hours.

[0021] Compared with the prior art, the present invention has the following beneficial effects:

[0022] (1) The BC / ImClO4 composite piezoelectric fiber provided by the present invention has a simple preparation process and low cost.

[0023] (2) The present invention utilizes renewable and degradable BC bacterial cellulose membrane material as a matrix material, and the prepared composite piezoelectric fiber has degradable properties.

[0024] (3) The present invention utilizes molecular ferroelectrics that can be dissolved and recrystallized as piezoelectric functional materials. The functional materials have the property of being recyclable, thus reducing the waste of materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 This is a physical picture of the BC / ImClO4 composite piezoelectric fiber obtained in Example 3.

[0026] Figure 2 2a and 2b are scanning electron microscope photographs of the surface of the BC / ImClO4 composite piezoelectric fiber obtained in Example 3 at 400 μm and 4 μm.

[0027] Figure 3 3a and 3b are scanning electron microscope photographs of the surface and cross section of the BC / ImClO4 composite piezoelectric fiber obtained in Example 3 at 500 μm.

[0028] Figure 4 This is a photo of the enzymatic degradation process of the BC / ImClO4 composite piezoelectric fiber prepared in Example 3.

[0029] Figure 5 This is a piezoelectric fabric prepared from the BC / ImClO4 composite piezoelectric fiber prepared in Example 3.

[0030] Figure 6 It is the voltage output signal of the piezoelectric fabric prepared by using the BC / ImClO4 composite piezoelectric fiber prepared in Example 3 when an external force is applied.

[0031] Figure 7 a is a voltage signal generated when monitoring human walking on a piezoelectric fabric nested sock prepared using the BC / ImClO4 composite piezoelectric fiber prepared in Example 3;

[0032] Figure 7 b is the voltage signal generated when monitoring a human body running on the piezoelectric fabric nested socks prepared by using the BC / ImClO4 composite piezoelectric fiber prepared in Example 3. DETAILED DESCRIPTION

[0033] The preferred embodiments of the present invention are described below in conjunction with the accompanying drawings. It should be understood that the preferred embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.

[0034] Example 1

[0035] The present embodiment provides a bacterial cellulose / perchloric acid imidazolate composite piezoelectric fiber and a preparation method thereof, comprising the following steps: dissolving 13.6 g imidazole and 13.36 mL perchloric acid in 40 mL distilled water, stirring for 15 minutes to obtain a mixed solution; placing the mixed solution in a 70°C oven for 120 hours, and obtaining ImClO4 crystals after the solution evaporates; dissolving the ImClO4 crystals in distilled water to prepare a 0.02 g / mL ImClO4 solution; cutting the semi-dehydrated BC bacterial cellulose membrane into 5 mm wide strips, and soaking them in distilled water for 2 hours to fully Swelling to remove impurities; soaking the BC bacterial cellulose membrane element that has been mechanically compressed to remove part of the water in a 0.1g / mL ImClO4 solution, and shaking it in a shaker for 1 hour to obtain a strip of BC bacterial cellulose membrane element material that is fully swollen and absorbs the ImClO4 solution; placing the strip of BC bacterial cellulose membrane element material containing the ImClO4 solution in a 60°C oven for 2 hours for recrystallization to obtain a BC / ImClO4 complex; treating the complex with a high-voltage polarization device, with a polarization voltage of 4 kilovolts and a polarization time of 10 minutes, to obtain a BC / ImClO4 composite piezoelectric material. Stretch the BC / ImClO4 complex to 110% of its original length; twist the stretched BC / ImClO4 complex to 95% of its original length, and then dry it at 40°C and under a load of 20 grams in a stretched state to obtain a BC / ImClO4 composite piezoelectric fiber.

[0036] Example 2

[0037] The present embodiment provides a bacterial cellulose / perchloric acid imidazolate composite piezoelectric fiber and a preparation method thereof, comprising the following steps: dissolving 13.6 g imidazole and 13.36 mL perchloric acid in 40 mL distilled water, stirring for 15 minutes to obtain a mixed solution; placing the mixed solution in a 70° C. oven for 120 hours, and obtaining ImClO4 crystals after the solution evaporates; dissolving the ImClO4 crystals in distilled water to prepare 0.06 g / mL ImClO 4Solution; cut the semi-dehydrated BC bacterial cellulose into strips with a width of 5 mm, and soak it in distilled water for 2 hours to fully swell and remove impurities; soak the BC bacterial cellulose membrane that has been mechanically compressed to remove part of the water in a 0.1 g / mL ImClO4 solution, and shake it in a shaker for 1 hour to obtain a strip of BC bacterial cellulose membrane material that is fully swollen and absorbs the ImClO4 solution; place the strip of BC bacterial cellulose membrane material containing the ImClO4 solution in a 60°C oven for 2 hours to recrystallize to obtain a BC / ImClO4 composite; treat the composite with a high-voltage polarization device, with a polarization voltage of 4 kilovolts and a polarization time of 10 minutes to obtain a BC / ImClO4 composite piezoelectric material. Stretch the BC / ImClO4 composite to 110% of its original length; twist the stretched BC / ImClO4 composite to 95% of its original length, and then dry it at 40°C and under a tensile state with a load of 20 grams to obtain a BC / ImClO4 composite piezoelectric fiber.

[0038] Example 3

[0039] The present embodiment provides a bacterial cellulose / perchloric acid imidazolate composite piezoelectric fiber and a preparation method thereof, comprising the following steps: dissolving 13.6 g imidazole and 13.36 mL perchloric acid in 40 mL distilled water, stirring for 15 minutes to obtain a mixed solution; placing the mixed solution in a 70° C. oven for 120 hours, and obtaining ImClO4 crystals after the solution evaporates; dissolving the ImClO4 crystals in distilled water to prepare 0.1 g / mL ImClO 4 Solution; cut the semi-dehydrated BC bacterial cellulose into strips with a width of 5 mm, and soak it in distilled water for 2 hours to fully swell and remove impurities; soak the BC bacterial cellulose membrane that has been mechanically compressed to remove part of the water in a 0.1 g / mL ImClO4 solution, and shake it in a shaker for 1 hour to obtain a strip of BC bacterial cellulose membrane material that is fully swollen and absorbs the ImClO4 solution; place the strip of BC bacterial cellulose membrane material containing the ImClO4 solution in a 60°C oven for 2 hours to recrystallize to obtain a BC / ImClO4 composite; treat the composite with a high-voltage polarization device, with a polarization voltage of 4 kilovolts and a polarization time of 10 minutes to obtain a BC / ImClO4 composite piezoelectric material. Stretch the BC / ImClO4 composite to 110% of its original length; twist the stretched BC / ImClO4 composite to 95% of its original length, and then dry it at 40°C and under a tensile state with a load of 20 grams to obtain a BC / ImClO4 composite piezoelectric fiber.

[0040] Figure 1 This is a real picture of the BC / ImClO4 composite piezoelectric fiber obtained in Example 3. Figure 1It can be seen that the surface of the BC / ImClO4 composite piezoelectric fiber is attached with ImClO4 crystals and has a certain degree of bendability.

[0041] Figure 2 2a and 2b are scanning electron microscope photos of the surface of the BC / ImClO4 composite piezoelectric fiber obtained in Example 3 at 400 μm and 4 μm. Figure 2 It can be seen that the three-dimensional network structure of bacterial cellulose is filled with ImClO4 crystals.

[0042] Figure 3 3a and 3b are scanning electron microscope photos of the surface and cross section of the BC / ImClO4 composite piezoelectric fiber obtained in Example 3 at 500 μm. Figure 3 It can be seen that the BC / ImClO4 composite piezoelectric fiber has a dense structure, which can ensure strong mechanical strength.

[0043] Figure 4 is a photo of the enzymatic degradation process of the BC / ImClO4 composite piezoelectric fiber prepared in Example 3; Figure 4 It can be seen that the matrix BC in the BC / ImClO4 composite piezoelectric fiber can be completely degraded and the ImClO4 crystals can also be dissolved in the aqueous solution.

[0044] Figure 5 This is a piezoelectric fabric prepared from the BC / ImClO4 composite piezoelectric fiber prepared in Example 3.

[0045] Figure 6 This is the voltage output signal of the piezoelectric fabric prepared using the BC / ImClO4 composite piezoelectric fiber prepared in Example 3 when an external force is applied, indicating that the prepared piezoelectric fabric has sensitive pressure sensing properties.

[0046] Figure 7 7a and 7b are voltage signals generated when a person walks and runs on a piezoelectric fabric nested sock prepared by using the BC / ImClO4 composite piezoelectric fiber prepared in Example 3. This indicates that the prepared BC / ImClO4 composite piezoelectric fiber has potential application prospects in designing smart fabrics for monitoring human activities.

[0047] Example 4

[0048] The present embodiment provides a bacterial cellulose / perchloric acid imidazolate composite piezoelectric fiber and a preparation method thereof, comprising the following steps: dissolving 13.6 g imidazole and 13.36 mL perchloric acid in 40 mL distilled water, stirring for 15 minutes to obtain a mixed solution; placing the mixed solution in a 70° C. oven for 120 hours, and obtaining ImClO4 crystals after the solution evaporates; dissolving the ImClO4 crystals in distilled water to prepare 0.14 g / mL ImClO 4 Solution; cut the semi-dehydrated BC bacterial cellulose into strips with a width of 5 mm, and soak it in distilled water for 2 hours to fully swell and remove impurities; soak the BC bacterial cellulose membrane that has been mechanically compressed to remove part of the water in a 0.1 g / mL ImClO4 solution, and shake it in a shaker for 1 hour to obtain a strip of BC bacterial cellulose membrane material that is fully swollen and absorbs the ImClO4 solution; place the strip of BC bacterial cellulose membrane material containing the ImClO4 solution in a 60°C oven for 2 hours to recrystallize to obtain a BC / ImClO4 composite; treat the composite with a high-voltage polarization device, with a polarization voltage of 4 kilovolts and a polarization time of 10 minutes to obtain a BC / ImClO4 composite piezoelectric material. Stretch the BC / ImClO4 composite to 110% of its original length; twist the stretched BC / ImClO4 composite to 95% of its original length, and then dry it at 40°C and under a tensile state with a load of 20 grams to obtain a BC / ImClO4 composite piezoelectric fiber.

[0049] Example 5

[0050] The present embodiment provides a bacterial cellulose / perchloric acid imidazolate composite piezoelectric fiber and a preparation method thereof, comprising the following steps: dissolving 13.6 g imidazole and 13.36 mL perchloric acid in 40 mL distilled water, stirring for 15 minutes to obtain a mixed solution; placing the mixed solution in a 70° C. oven for 120 hours, and obtaining ImClO4 crystals after the solution evaporates; dissolving the ImClO4 crystals in distilled water to prepare 0.18 g / mL ImClO 4Solution; cut the semi-dehydrated BC bacterial cellulose into strips with a width of 5 mm, and soak it in distilled water for 2 hours to fully swell and remove impurities; soak the BC bacterial cellulose membrane that has been mechanically compressed to remove part of the water in a 0.1 g / mL ImClO4 solution, and shake it in a shaker for 1 hour to obtain a strip of BC bacterial cellulose membrane material that is fully swollen and absorbs the ImClO4 solution; place the strip of BC bacterial cellulose membrane material containing the ImClO4 solution in a 60°C oven for 2 hours to recrystallize to obtain a BC / ImClO4 composite; treat the composite with a high-voltage polarization device, with a polarization voltage of 4 kilovolts and a polarization time of 10 minutes to obtain a BC / ImClO4 composite piezoelectric material. Stretch the BC / ImClO4 composite to 110% of its original length; twist the stretched BC / ImClO4 composite to 95% of its original length, and then dry it at 40°C and under a tensile state with a load of 20 grams to obtain a BC / ImClO4 composite piezoelectric fiber.

[0051] Comparative Example 1

[0052] The present embodiment provides a method for preparing pure BC fiber, comprising the following steps: cutting semi-dehydrated BC bacterial cellulose into strips with a width of 5 mm, and soaking the strips in distilled water for 2 hours to fully swell and remove impurities; stretching the BC strips to 110% of the original length; twisting the stretched BC strips to 95% of the original length, and then drying them at 40°C and under a load of 20 grams in a stretched state to obtain pure BC fiber.

[0053] The properties of the materials prepared in Examples 1-5 and Comparative Example 1 are compared as follows:

[0054]

[0055] The BBC / ImClO4 composite piezoelectric fiber prepared by the present invention has the advantages of high piezoelectric coefficient, high pressure monitoring sensitivity and biodegradability, and has great application potential in wearable smart fabrics such as health and sports monitoring.

[0056] Finally, it should be noted that the above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for preparing biodegradable bacterial cellulose / perchloridized imidazolate composite piezoelectric fiber, characterized in that: The steps include: S1, dissolving imidazole and perchloric acid in distilled water, and stirring to obtain a mixed solution; S2, placing the mixed solution obtained in step S1 in an oven, and obtaining high-chloride imidazolate crystals as the liquid evaporates; S3, dissolving the high-chloride imidazolate crystals obtained in step S2 in distilled water to obtain a high-chloride imidazolate solution; S4, soaking the strip-shaped BC bacterial cellulose material in the high-chloride imidazolate solution obtained in step S3, shaking on a shaker, and placing it in an oven, and after the solution evaporates, obtaining a BC / ImClO4 complex; S5, mechanically stretching and twisting the BC / ImClO4 composite obtained in step S4 into a linear shape, and shaping it in the stretched state to obtain a BC / ImClO4 composite piezoelectric fiber.

2. The method for preparing a biodegradable bacterial cellulose / perchloroimidazole salt composite piezoelectric fiber according to claim 1, characterized in that: The concentration range of imidazole in step S1 is 0.05-0.5 mol / L; the concentration range of perchloric acid in step S1 is 0.05-0.5 mol / L.

3. The method for preparing a biodegradable bacterial cellulose / perchloroimidazole salt composite piezoelectric fiber according to claim 1, characterized in that: The temperature range of the oven in step S2 is 40 to 80° C., and the liquid evaporation time is 72 to 120 hours.

4. The method for preparing a biodegradable bacterial cellulose / perchloroimidazole salt composite piezoelectric fiber according to claim 1, characterized in that: The concentration of the high-chloride imidazolate solution in step S3 is 0.01-0.2 mol / L.

5. The method for preparing a biodegradable bacterial cellulose / perchloroimidazole salt composite piezoelectric fiber according to claim 1, characterized in that: The strip-shaped BC bacterial cellulose membrane material in step S4 is prepared by the following steps: cutting semi-dehydrated BC bacterial cellulose membrane into strips, soaking in distilled water to swell and remove impurities, and removing part of the water by mechanical compression to obtain the strip-shaped BC bacterial cellulose membrane material. The weight loss rate of the bacterial cellulose hydrogel after mechanical compression is 50-90%.

6. The method for preparing a biodegradable bacterial cellulose / perchloroimidazole salt composite piezoelectric fiber according to claim 5, characterized in that: The strip-shaped BC bacterial fibrous membrane material has a thickness of 1 to 3 mm, a width of 4 to 8 mm, and a crystallinity of 85 to 95%.

7. The method for preparing a biodegradable bacterial cellulose / perchloridized imidazolate composite piezoelectric fiber according to claim 1, characterized in that: The shaking speed of the shaking table is 100-150 rpm, and the shaking time is 30-120 minutes.

8. The method for preparing a biodegradable bacterial cellulose / perchloroimidazole salt composite piezoelectric fiber according to claim 1, characterized in that: The length of the product after stretching in step S5 changes to 110-120% of the original length, and the length of the twisted fiber changes to 85-95% of the original length.

9. The method for preparing a biodegradable bacterial cellulose / perchloroimidazole salt composite piezoelectric fiber according to claim 1, characterized in that: The tension range of maintaining the stretched state in step S5 is 0.2 to 2N, the drying temperature is 25 to 80°C, and the drying and setting time is 1 to 2 hours.

Citation Information

Patent Citations

  • Liquid crystal spinning method for regeneration bacterium cellulose fiber

    CN102776593A

  • Nano microcrystalline cellulose piezoelectric material and preparation method thereof

    CN111205499A

  • Integrated flexible stretchable tactile sensor based on super-capacitor sensing principle

    CN111504520A

  • High-orientation and high-strength bacterial cellulose composite membrane as well as preparation and application thereof

    CN113082282A