Polymer conductive fiber membrane as well as preparation method and application thereof

Polymer conductive fiber membranes with a core-sheath structure were prepared by electrospinning and oxidant-induced polymerization, which solved the problems of low conductivity, poor flexibility and poor stability of traditional conductive fibers, and improved conductivity stability and flexibility.

CN118932606APending Publication Date: 2024-11-12QIANFAN INTELLIGENT TECHNOLOGY (TIANJIN) CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411268969.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Traditional conductive fibers suffer from low conductivity, poor flexibility, and poor stability when conductive media are added. In particular, powdered conductive media cannot be added in large quantities, and the stability and flexibility of coating methods are insufficient.

Method used

Polymer conductive fiber membranes with a core-shell structure consisting of a fiber-forming polymer as the sheath and polypyrrole as the core were prepared using electrospinning technology. Pyrrole was polymerized in the core through electrospinning and oxidant-induced polymerization to form a stable conductive network.

Benefits of technology

It improves the conductivity stability and flexibility of conductive fiber membranes, avoids the polymerization and shedding of pyrrole on the surface, and has a simple process and low cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932606A_ABST
    Figure CN118932606A_ABST
Patent Text Reader

Abstract

The invention discloses a polymer conductive fiber membrane as well as a preparation method and application thereof, and belongs to the technical field of conductive materials. The conductive fiber membrane with a skin-core structure is prepared by taking the fiber-forming polymer as a skin layer and polypyrrole as a core layer, and the conductive polypyrrole is taken as the core layer, so that the shedding phenomenon of pyrrole in surface polymerization is improved, meanwhile, the polymerization of pyrrole occurs in the core part, the conductive stability of the conductive fiber membrane is improved, and in addition, the conductive fiber membrane has a good application prospect. The surface layer of the conductive fiber membrane is still in the natural color of the fiber-forming polymer, and subsequent dyeing, after-finishing and other procedures of the fiber membrane are not affected. According to the preparation method, the skin-core structure nanofiber membrane with the pyrrole monomer as the core layer is prepared through the electrostatic spinning technology, then polymerization of the pyrrole monomer is induced through the oxidizing agent, the polymer conductive fiber membrane with polypyrrole as the core layer is obtained, the process is simple, and the cost is low.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of conductive materials, and in particular relates to a polymer conductive fiber membrane and a preparation method and application thereof. Background Art

[0002] Polymer conductive fiber is a conductive fiber prepared by mixing a conductive medium into a polymer through mixed spinning, composite spinning, coating and other methods. The conductive medium is usually metal powder, carbon black, graphite, metal oxide or intrinsic conductive polymer, etc. It can be widely used in special work clothes for electrostatic shielding, protective clothing, wearable sensors, heat protection and other fields.

[0003] The biggest problem faced by traditional powder conductive media in imparting conductivity to fibers through spinning is that it is impossible to add a large amount of conductive media. As the content of the conductive media increases, the performance of the fiber decreases, while if the conductive media is too little, the conductivity cannot meet the requirements. Therefore, for additive conductive fibers, the spinning bottleneck has not been broken through over the years.

[0004] Another method for preparing conductive fibers is coating. This method can obtain a continuous conductive particle network with lower conductivity, simple preparation, and little damage to the fiber. However, it will reduce the feel of the fiber surface, reduce the softness of the fiber, and the formed coating is easy to fall off and has poor stability.

[0005] In addition, intrinsic conductive polymers can be used to form a conductive layer on the fiber surface by post-polymerization. Since intrinsic conductive polymers have characteristics such as flexibility, the post-polymerization method can effectively improve the phenomenon of fiber surface hardening, but the flexibility and wear resistance of the original fiber still need to be improved.

[0006] Therefore, how to use intrinsic conductive polymers to prepare conductive fibers with good stability, long-lasting conductivity and softness has become a technical problem that needs to be urgently solved in this field. Summary of the invention

[0007] In order to solve the above technical problems, the present invention proposes a polymer conductive fiber membrane and its preparation method and application. The polymer conductive fiber membrane provided by the present invention solves the problems of difficult processing, low conductivity, poor flexibility and poor stability existing in traditional conductive fibers.

[0008] To achieve the above object, the present invention provides the following technical solutions:

[0009] The invention provides a polymer conductive fiber membrane. The polymer conductive fiber membrane has a skin-core structure with a fiber-forming polymer as a skin layer and polypyrrole as a core layer.

[0010] Preferably, the content of fiber-forming polymer in the polymer conductive fiber membrane is 60-80wt%, and the content of polypyrrole is 20-40wt%.

[0011] Preferably, the fiber-forming polymer includes one or more of polyvinyl alcohol, polyvinyl pyrrolidone, polyacrylamide, polyethylene oxide, water-soluble cellulose derivatives, polyacrylic acid, and polyacrylic acid salts.

[0012] The present invention provides a method for preparing the polymer conductive fiber membrane described in the above technical scheme, comprising the following steps: using a fiber-forming polymer as a skin layer and a pyrrole monomer as a core layer to obtain a fiber-forming polymer / pyrrole monomer nanofiber membrane through electrostatic spinning; crosslinking and oxidant-induced polymerization of the fiber-forming polymer / pyrrole monomer nanofiber membrane to obtain a polymer conductive fiber membrane with a fiber-forming polymer as a skin layer and polypyrrole as a core layer.

[0013] Preferably, the voltage of the electrospinning is 20-40 kV, the receiving distance of the winding roller is 15-20 cm, the spinning speed is 3-5 μL / min, the speed of the receiving roller is 1000-1500 r / min; and the electrospinning time is 7-12 h.

[0014] Preferably, the electrospinning skin layer spinning solution is formed by mixing a fiber-forming polymer and water, and the core layer spinning solution is formed by mixing a pyrrole monomer, water and a surfactant.

[0015] Preferably, the concentration of the fiber-forming polymer in the skin layer spinning solution is 60-90wt%; the content of the pyrrole monomer in the core layer spinning solution is 10-40wt% of the amount of water used, and the content of the surfactant is 0.5-2.5wt% of the amount of water used.

[0016] Preferably, the cross-linking temperature is 20-60° C., the cross-linking time is 0.5-2 h, and the cross-linking agent used for cross-linking includes one or more of glutaraldehyde, boric acid, formaldehyde, glyoxal, and dihydroxymethylurea.

[0017] Preferably, the temperature of the oxidant-induced polymerization is -20 to 40°C, and the time of the oxidant-induced polymerization is 1 to 4 hours.

[0018] The present invention also provides applications of the polymer conductive fiber film described in the above technical solution in the fields of electromagnetic shielding, sensors, and intelligent touch conduction.

[0019] Compared with the prior art, the present invention has the following advantages and technical effects:

[0020] The present invention uses a fiber-forming polymer as a skin layer and polypyrrole as a core layer to prepare a conductive fiber membrane with a skin-core structure. The conductive polypyrrole is used as the core layer, which improves the shedding phenomenon of pyrrole polymerization on the surface. At the same time, the polymerization of pyrrole occurs in the core, which improves the conductive stability of the conductive fiber membrane. In addition, the surface layer of the conductive fiber membrane is still the original color of the fiber-forming polymer, which does not affect the subsequent dyeing, post-finishing and other processes of the fiber membrane.

[0021] The present invention firstly prepares a skin-core structure nanofiber membrane with pyrrole monomer as the core layer by electrospinning technology, and then induces polymerization of pyrrole monomer by an oxidant to obtain a polymer conductive fiber membrane with polypyrrole as the core layer. The preparation method provided by the present invention can improve the shedding phenomenon of pyrrole in surface polymerization, and at the same time, the polymerization of pyrrole occurs in the core, thereby improving the conductive stability of the conductive fiber membrane, and the finally obtained polymer conductive fiber membrane has excellent conductive properties and soft properties. In addition, the preparation method of the present invention has a simple process and low cost. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:

[0023] Figure 1 is a schematic diagram of the structure of the polymer conductive fiber membrane in Example 1;

[0024] Figure 2 This is an electron microscope image of the core layer spinning solution in Example 1;

[0025] Figure 3 is an electron microscope image of the nanofiber membrane in Example 1;

[0026] Figure 4 is an electron microscope image of the polymer conductive fiber membrane in Example 1;

[0027] Figure 5 The resistance bar graphs of polypyrrole (PPy) cotton fabric, polypyrrole (PPy) aramid and the polymer conductive fiber film (PPy conductive fiber) prepared in Example 1. DETAILED DESCRIPTION

[0028] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.

[0030] An embodiment of the present invention provides a polymer conductive fiber membrane having a skin-core structure with a fiber-forming polymer as a skin layer and polypyrrole as a core layer.

[0031] The present invention uses a fiber-forming polymer as a skin layer and polypyrrole as a core layer to prepare a conductive fiber membrane with a skin-core structure. The conductive polypyrrole is used as the core layer, which improves the shedding phenomenon of pyrrole polymerization on the surface. At the same time, the polymerization of pyrrole occurs in the core, which improves the conductive stability of the conductive fiber membrane. In addition, the surface layer of the conductive fiber membrane is still the original color of the fiber-forming polymer, which does not affect the subsequent dyeing, post-finishing and other processes of the fiber membrane.

[0032] In a preferred embodiment, the content of fiber-forming polymer in the polymer conductive fiber membrane is 60-80wt%, and the content of polypyrrole is 20-40wt%. The present invention controls the content of polypyrrole in the polymer conductive fiber membrane within the above range, which not only ensures conductivity but also avoids the problem of molecular chain agglomeration caused by excessive polypyrrole content.

[0033] In a preferred embodiment, the fiber-forming polymer includes one or more of polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), polyacrylamide (PAM), polyethylene oxide (PEO), water-soluble cellulose derivatives, polyacrylic acid (PAA), and polyacrylates, and more preferably one or more of polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), polyethylene oxide (PEO), and water-soluble cellulose derivatives; the water-soluble cellulose derivative includes hydroxyethyl cellulose. The present invention uses the above-mentioned types of polymers as fiber-forming polymers, which have the advantages of being cheap and having good biocompatibility.

[0034] The present invention provides a method for preparing the polymer conductive fiber membrane described in the above technical scheme, comprising the following steps: using a fiber-forming polymer as a skin layer and a pyrrole monomer as a core layer to obtain a fiber-forming polymer / pyrrole monomer nanofiber membrane through electrostatic spinning; crosslinking and oxidant-induced polymerization of the fiber-forming polymer / pyrrole monomer nanofiber membrane to obtain a polymer conductive fiber membrane with a fiber-forming polymer as a skin layer and polypyrrole as a core layer.

[0035] The present invention firstly prepares a skin-core structure nanofiber membrane with pyrrole monomer as the core layer by electrospinning technology, and then induces polymerization of pyrrole monomer by an oxidant to obtain a polymer conductive fiber membrane with polypyrrole as the core layer. The preparation method provided by the present invention can improve the shedding phenomenon of pyrrole in surface polymerization, and at the same time, the polymerization of pyrrole occurs in the core, thereby improving the conductive stability of the conductive fiber membrane, and the finally obtained polymer conductive fiber membrane has excellent conductive properties and soft properties. In addition, the preparation method of the present invention has a simple process and low cost.

[0036] In a preferred embodiment, the voltage of the electrospinning is 20-40 kV, the receiving distance of the winding roller is 15-20 cm, the spinning speed is 3-5 μL / min, the speed of the receiving roller is 1000-1500 r / min, and the electrospinning time is 7-12 h. The present invention controls the process parameters of electrospinning within the above range, and the obtained fibers are more uniform and better oriented.

[0037] In a preferred embodiment, the volume ratio of the electrospinning skin layer spinning solution to the core layer spinning solution is (2-5):(1-3).

[0038] In a preferred embodiment, the electrospinning cortex spinning solution is a mixture of a fiber-forming polymer and water; the concentration of the fiber-forming polymer in the cortex spinning solution is 60-90wt%, more preferably 70-85wt%. The present invention controls the concentration of the fiber-forming polymer in the cortex spinning solution within the above range, thereby ensuring the smooth progress of electrospinning.

[0039] In a preferred embodiment, the electrospinning core layer spinning solution is a mixture of pyrrole monomer, water and surfactant; the preparation process of the core layer spinning solution includes: adding surfactant to water, then dropping pyrrole monomer, and homogenizing to obtain the core layer spinning solution.

[0040] In a preferred embodiment, the dripping speed is 30-200 drops / min, more preferably 90-200 drops / min.

[0041] In a preferred embodiment, the temperature of the dropping is -20 to 40°C, more preferably 0 to 40°C; the dropping is performed under stirring; the stirring speed is 100-200 rpm, more preferably 150-200 rpm.

[0042] In a preferred embodiment, the rotation speed of the homogenizer is 5000-20000 rpm, and the homogenization time is 5-30 min. The present invention obtains a uniform spinning solution by homogenization.

[0043] In a preferred embodiment, the content of pyrrole monomer in the core layer spinning solution is 10-40wt% of the water dosage, and more preferably 15-35wt%. The present invention controls the content of pyrrole monomer in the core layer spinning solution within the above range, and the obtained skin-core structure is more complete. Too little content of pyrrole monomer cannot ensure the conductivity of the conductive fiber membrane, and too much content of pyrrole monomer will cause the molecular chain to agglomerate after polymerization.

[0044] In a preferred embodiment, the content of the surfactant in the core layer spinning solution is 0.5-2.5wt% of the amount of water; the surfactant includes sodium dodecylbenzene sulfonate or sodium dodecyl sulfate. The addition of the surfactant in the present invention helps to obtain a stable and uniform core layer spinning solution.

[0045] In a preferred embodiment, the cross-linking temperature is 20-60°C, more preferably 40-60°C; the cross-linking time is 0.5-2h, more preferably 0.5-1h; the cross-linking agent used for the cross-linking includes one or more of glutaraldehyde, boric acid, formaldehyde, glyoxal, and dimethylol urea, more preferably glutaraldehyde; the amount of the cross-linking agent is 0.01-2% of the mass of the fiber-forming polymer. The cross-linking in the present invention can improve the water resistance and water repellency of the fiber membrane.

[0046] In a preferred embodiment, the temperature of the oxidant-induced polymerization is -20 to 40°C, more preferably 0 to 40°C; the time of the oxidant-induced polymerization is 1 to 4 hours. The oxidant-induced polymerization at the above temperature is conducive to obtaining a more ordered molecular chain.

[0047] In a preferred embodiment, the oxidant includes ferric oxide, ammonium persulfate, cupric chloride or hydrogen peroxide, more preferably ferric oxide or hydrogen peroxide; the solvent for dissolving the oxidant includes acetone, methanol, ethylene glycol or dimethyl sulfoxide, more preferably acetone.

[0048] In a preferred embodiment, the mass ratio of the oxidant to the pyrrole monomer is (2-4):(1-4).

[0049] The present invention also provides applications of the polymer conductive fiber film described in the above technical solution in the fields of electromagnetic shielding, sensors, and intelligent touch conduction.

[0050] Unless otherwise specified, the raw materials in the examples of the present invention were purchased from commercial sources.

[0051] The surfactant used in the following examples is sodium dodecylbenzene sulfonate.

[0052] Example 1

[0053] A polymer conductive fiber membrane has a skin-core structure with PVA as a skin layer and polypyrrole as a core layer. The content of PVA in the polymer conductive fiber membrane is 60wt%, and the content of polypyrrole is 40wt%.

[0054] Preparation process of polymer conductive fiber membrane:

[0055] PVA was dissolved in water to obtain a cortex spinning solution with a PVA concentration of 60wt%, which was injected into a syringe with a stainless steel needle (cortex); a surfactant was added to the water (the ratio of surfactant to water was 1:100), and then pyrrole monomer was added at a rate of 90 drops / min at 20°C, and the addition process was accompanied by stirring at a speed of 100 rpm, and then homogenized at a speed of 5000 rpm for 10min to obtain a core spinning solution (the content of pyrrole monomer in the core spinning solution was 25wt% of the amount of water). The core spinning solution was injected into a syringe with a stainless steel needle (core), and electrospun for 8h according to the process parameters of spinning voltage of 20kV, receiving distance of 20cm, receiving roller speed of 1000r / min, and injection pump injection speed of 3μL / min to obtain a nanofiber membrane. Among them, the volume ratio of the cortex spinning solution to the core spinning solution was 3:1.

[0056] The above-mentioned nanofiber membrane is placed in a 20°C closed reactor containing glutaraldehyde (the amount of glutaraldehyde is 2% of the mass of PVA) for cross-linking for 1 hour, and the cross-linked nanofiber membrane is taken out, and placed in an acetone solution of ferric chloride (the mass ratio of ferric chloride to pyrrole monomer is 2:1), dipped, taken out, and placed in a constant temperature and closed oven at 20°C to induce polymerization for 2 hours. After taking out, wash it in distilled water, dry it, and obtain a polymer conductive fiber membrane.

[0057] Figure 1 Schematic diagram of the structure of the polymer conductive fiber membrane in Example 1. Figure 1 It can be seen that the polymer conductive fiber membrane prepared in Example 1 has a skin-core structure.

[0058] Figure 2 This is an electron microscope image of the core layer spinning solution in Example 1. Figure 2 It can be seen that the pyrrole monomer exists in the core spinning solution in a uniform and stable state.

[0059] Figure 3 is an electron microscope image of the nanofiber membrane in Example 1. Figure 3 It can be seen that the nanofiber membrane has a skin-core structure, and the pyrrole monomer is evenly distributed in the core layer of the fiber.

[0060] Figure 4 is an electron microscope image of the polymer conductive fiber membrane in Example 1. Figure 4It can be seen that polypyrrole is uniformly formed in the polymer-based fibers.

[0061] Figure 5 The resistance bar graphs of polypyrrole (PPy) cotton fabric, polypyrrole (PPy) aramid and the polymer conductive fiber film (PPy conductive fiber) prepared in Example 1 are shown in FIG. Figure 5 It can be seen that the resistance of the polymer conductive fiber film prepared in Example 1 of the present invention is only 1032.0Ω, which is greatly reduced compared with the resistance of polypyrrole cotton fabric (1588.0Ω) and the resistance of polypyrrole aramid (1190.3Ω), indicating that the polymer conductive fiber film prepared in Example 1 of the present invention has excellent conductive properties; wherein, polypyrrole cotton fabric comes from the local market, and polypyrrole aramid comes from the local market.

[0062] Example 2

[0063] A polymer conductive fiber membrane has a skin-core structure with PVP as a skin layer and polypyrrole as a core layer. The content of PVP in the polymer conductive fiber membrane is 70wt%, and the content of polypyrrole is 30wt%.

[0064] Preparation process:

[0065] PVP was dissolved in water to obtain a cortex spinning solution with a PVP concentration of 75wt%, which was injected into a syringe with a stainless steel needle (cortex); a surfactant was added to the water (the ratio of surfactant to water was 1:50), and then pyrrole monomer was added at a rate of 100 drops / min at 40°C, and the addition process was accompanied by stirring at a speed of 200 rpm, and then homogenized at a speed of 7500 rpm for 20min to obtain a core spinning solution (the content of pyrrole monomer in the core spinning solution was 20wt% of the amount of water). The core spinning solution was injected into a syringe with a stainless steel needle (core), and electrospun for 7h according to the process parameters of spinning voltage of 30kV, receiving distance of 15cm, receiving roller speed of 1200r / min, and injection pump injection speed of 3μL / min to obtain a nanofiber membrane. Among them, the volume ratio of the cortex spinning solution to the core spinning solution was 2:1.

[0066] The above-mentioned nanofiber membrane was placed in a 60°C closed reactor containing glutaraldehyde (the amount of glutaraldehyde is 0.25% of the mass of PVP) for cross-linking for 0.5h, and then placed in an acetone solution of ferric chloride (the mass ratio of ferric chloride to pyrrole monomer is 4:1), dipped, taken out, and placed in a constant temperature closed oven at 40°C to induce polymerization for 1h. Then, it was taken out and washed in distilled water and dried to obtain a polymer conductive fiber membrane.

[0067] Example 3

[0068] A polymer conductive fiber membrane has a skin-core structure with PEO as a skin layer and polypyrrole as a core layer. The content of PEO in the polymer conductive fiber membrane is 80wt%, and the content of polypyrrole is 20wt%.

[0069] Preparation process:

[0070] PEO was dissolved in water to obtain a cortex spinning solution with a PEO concentration of 80wt%, which was injected into a syringe with a stainless steel needle (cortex); a surfactant was added to the water (the ratio of surfactant to water was 1:150), and then pyrrole monomer was added at a rate of 150 drops / min at 0°C, and the dropping process was accompanied by stirring at a speed of 150 rpm, and then homogenized at a speed of 15000 rpm for 15min to obtain a core spinning solution (the content of pyrrole monomer in the core spinning solution was 20wt% of the amount of water). The core spinning solution was injected into a syringe with a stainless steel needle (core), and electrospun for 10h according to the process parameters of spinning voltage of 40kV, receiving distance of 15cm, receiving roller speed of 1500r / min, and injection pump injection speed of 5μL / min to obtain a nanofiber membrane. Among them, the volume ratio of the cortex spinning solution to the core spinning solution was 3:1.

[0071] The above-mentioned nanofiber membrane is then placed in a 50°C closed reactor containing glutaraldehyde (the amount of glutaraldehyde is 0.3% of the mass of PEO) for cross-linking for 1 hour, and then placed in an acetone solution of ferric chloride (the mass ratio of ferric chloride to pyrrole monomer is 2:1), dipped, taken out, and placed in a constant temperature and closed oven at 0°C to induce polymerization for 4 hours. After taking out, wash it in distilled water and dry it to obtain a polymer conductive fiber membrane.

[0072] Example 4

[0073] A polymer conductive fiber membrane has a skin-core structure with hydroxyethyl cellulose as a skin layer and polypyrrole as a core layer. The content of hydroxyethyl cellulose in the polymer conductive fiber membrane is 80wt%, and the content of polypyrrole is 20wt%.

[0074] Preparation process:

[0075] Hydroxyethyl cellulose is dissolved in water to obtain a cortex spinning solution with a hydroxyethyl cellulose concentration of 85wt%, which is then injected into a syringe with a stainless steel needle (cortex); a surfactant is added to the water (the ratio of surfactant to water is 1:150), and then pyrrole monomer is added dropwise at a rate of 100 drops / min at 10°C, with stirring during the addition process, and the stirring speed is 200 rpm, and then homogenized at a speed of 20000 rpm for 30min to obtain a core spinning solution (the content of pyrrole monomer in the core spinning solution is 30wt% of the amount of water). The core spinning solution is injected into a syringe with a stainless steel needle (core), and electrospun for 12h according to the process parameters of spinning voltage of 20kV, receiving distance of 20cm, receiving roller speed of 1200r / min, and injection pump injection speed of 3μL / min to obtain a nanofiber membrane. Among them, the volume ratio of the cortex spinning solution to the core spinning solution is 3:1.

[0076] The above-mentioned nanofiber membrane was placed in a 40°C closed reactor containing glutaraldehyde (the amount of glutaraldehyde is 0.15% of the mass of hydroxyethyl cellulose) for cross-linking for 2 hours, and then placed in an acetone solution of ferric chloride (the mass ratio of ferric chloride to pyrrole monomer is 3:1), dipped, taken out, and placed in a constant temperature and closed oven at 10°C to induce polymerization for 4 hours. After taking out, wash it in distilled water and dry it to obtain a polymer conductive fiber membrane.

[0077] Comparative Example 1

[0078] PVA was dissolved in water to obtain a cortex spinning solution with a PVA concentration of 10wt%, which was then injected into a syringe with a stainless steel needle (cortex); a surfactant was added to the water (the ratio of surfactant to water was 1:100), and then polypyrrole was added at 20°C, and stirred at a speed of 100 rpm for 5 minutes, and then homogenized at a speed of 5000 rpm for 2 minutes to obtain a core spinning solution (the content of polypyrrole in the core spinning solution was 25wt% of the amount of water). The core spinning solution was injected into a syringe with a stainless steel needle (core), and electrospun for 8 hours according to the process parameters of spinning voltage of 20kV, receiving distance of 20cm, receiving roller speed of 1000r / min, and injection pump injection speed of 3μL / min to obtain a nanofiber membrane. Among them, the volume ratio of the cortex spinning solution to the core spinning solution was 1:1.

[0079] The nanofiber membrane was placed in a 20° C. closed reactor containing glutaraldehyde (the amount of glutaraldehyde was 2% of the mass of PVA) for crosslinking for 1 hour, and then taken out, washed in distilled water, and dried to obtain a polymer conductive fiber membrane.

[0080] Comparative Example 2

[0081] The difference from Example 1 is that electrospinning is carried out for 8 hours according to the process parameters of spinning voltage of 20 kV, receiving distance of 30 cm, receiving roller speed of 1000 r / min, and injection pump injection speed of 8 μL / min, and the remaining steps are the same as Example 1.

[0082] Comparative Example 3

[0083] The difference from Example 1 is that the polymerization is induced in a sealed oven at a constant temperature of 60° C. for 2 h, and the remaining steps are the same as in Example 1.

[0084] The softness of the conductive fiber membranes prepared in Examples 1-4 and Comparative Examples 1-3 was tested according to ISO 9073-7:1995 “Test methods for textile nonwovens - Part 7: Determination of bending length”, and the conductive stability of the conductive fiber membranes was tested according to ISO 3915:1981 “Plastics - Measurement of resistivity of conductive plastics”. The results are shown in Table 1.

[0085] Table 1 Softness and conductive stability of conductive fiber membranes prepared in Examples 1-4 and Comparative Examples 1-3

[0086]

[0087] It can be seen from Table 1 that the polymer conductive fiber membrane prepared in the present invention has excellent conductivity, softness and conductive stability.

[0088] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.

Claims

1. A polymer conductive fiber membrane, It is characterized in that The polymer conductive fiber membrane has a skin-core structure with a fiber-forming polymer as a skin layer and polypyrrole as a core layer.

2. The polymer conductive fiber membrane according to claim 1, It is characterized in that The content of fiber-forming polymer in the polymer conductive fiber membrane is 60-80wt%, and the content of polypyrrole is 20-40wt%.

3. The polymer conductive fiber membrane according to claim 1, It is characterized in that The fiber-forming polymer includes one or more of polyvinyl alcohol, polyvinyl pyrrolidone, polyacrylamide, polyethylene oxide, water-soluble cellulose derivatives, polyacrylic acid, and polyacrylic acid salts.

4. A method for preparing the polymer conductive fiber membrane according to any one of claims 1 to 3, It is characterized in that The following steps are involved: A fiber-forming polymer / pyrrole monomer nanofiber membrane is prepared by electrostatic spinning with a fiber-forming polymer as the skin layer and a pyrrole monomer as the core layer; the fiber-forming polymer / pyrrole monomer nanofiber membrane is cross-linked and polymerized by an oxidant to obtain a polymer conductive fiber membrane with a fiber-forming polymer as the skin layer and polypyrrole as the core layer.

5. The preparation method according to claim 4, It is characterized in that The voltage of the electrostatic spinning is 20-40 kV, the receiving distance of the winding roller is 15-20 cm, the spinning speed is 3-5 μL / min, the speed of the receiving roller is 1000-1500 r / min; and the electrostatic spinning time is 7-12 h.

6. The preparation method according to claim 4, It is characterized in that The electrostatic spinning skin layer spinning solution is formed by mixing a fiber-forming polymer and water, and the core layer spinning solution is formed by mixing a pyrrole monomer, water and a surfactant.

7. The preparation method according to claim 6, It is characterized in that The concentration of the fiber-forming polymer in the skin layer spinning solution is 60-90wt%; the content of the pyrrole monomer in the core layer spinning solution is 10-40wt% of the amount of water used, and the content of the surfactant is 0.5-2.5wt% of the amount of water used.

8. The preparation method according to claim 4, It is characterized in that The cross-linking temperature is 20-60° C., the cross-linking time is 0.5-2 h, and the cross-linking agent used for cross-linking includes one or more of glutaraldehyde, boric acid, formaldehyde, glyoxal, and dihydroxymethyl urea.

9. The preparation method according to claim 4, It is characterized in that The temperature of the oxidant-induced polymerization is -20 to 40° C., and the time of the oxidant-induced polymerization is 1 to 4 hours.

10. Application of the polymer conductive fiber film according to any one of claims 1 to 3 in the fields of electromagnetic shielding, sensors, and smart touch conduction.

Citation Information

Patent Citations

  • Polypyrrole supercapacitor composite electrode material on basis of electrostatic spinning nano-fiber yarn forming technologies and method for preparing polypyrrole supercapacitor composite electrode material

    CN109326453A

  • Cardiac pacemaker connecting wire with degradable conductive macromolecular matrix, and preparation method thereof

    CN111790008A

  • Conductive multi-functional fiber with sheath-core structure and preparation method of conductive multi-functional fiber

    CN112111807A

  • Chitosan-polypyrrole conductive fiber with core-shell structure and preparation method of chitosan-polypyrrole conductive fiber

    CN112779784A

  • Polypyrrole conductive flexible fiber membrane material and preparation method thereof

    CN115323784A