Degradable thermal repair CNTs / PBAT composite fiber and preparation method and application thereof

By preparing thermally repaired CNTs/PBAT composite fibers, the problems of non-degradability and poor flexibility of traditional strain sensor materials are solved, and efficient and fast self-repairing effect is achieved, which is suitable for the new generation of wearable devices.

CN118932702AActive Publication Date: 2024-11-12ZHEJIANG SCI-TECH UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411099303.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-12
Publication Date
2024-11-12
Estimated Expiration
2044-08-12

AI Technical Summary

Technical Problem

The matrix materials of existing strain sensors, especially rigid materials, are poor in flexibility and non-degradable, making it difficult to meet the needs of a new generation of wearable devices. Traditional polymer materials have a short service life and are non-degradable, which limits their use in wearable devices. Application.

Method used

Using a degradable thermal repair CNTs/PBAT composite fiber, the polyadipic acid/butylene terephthalate PBAT was premixed with triallyl isocyanurate TAIC and benzophenone BP. The cross-linked PBAT fibers were prepared by melt extrusion and ultraviolet radiation cross-linking, combined with carbon nanotube CNTs, and the CNTs dispersion was prepared by ultrasonic treatment, and the cross-linked PBAT fibers were impregnated to produce thermally repaired CNTs/PBAT composite fibers.

Benefits of technology

It realizes a flexible strain sensor with degradability, thermal repair, light weight, small size and simple manufacturing process. It has excellent sensing performance and durability, extends service life, and has melt-induced shrinkage under constant and stress-free conditions. Quickly repair damaged conductive networks.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932702A_ABST
    Figure CN118932702A_ABST
Patent Text Reader

Abstract

The invention relates to a degradable thermal remediation CNTs / PBAT composite fiber as well as a preparation method and application thereof. The preparation method comprises the following steps: (1) premixing poly (butylene adipate / terephthalate) (PBAT), triallyl isocyanurate (TAIC) and benzophenone (BP), then carrying out melt extrusion, and carrying out ultraviolet radiation crosslinking, so as to obtain a crosslinked PBAT fiber; the preparation method comprises the following steps: dispersing carbon nanotubes (CNTs) and sodium dodecyl sulfate (SDS) in a mixed solution of ethyl acetate and absolute ethyl alcohol, and carrying out ultrasonic treatment to prepare a CNTs dispersion solution; and (2) dipping the cross-linked PBAT fiber in the CNTs dispersion liquid, taking out the cross-linked PBAT fiber, hanging the cross-linked PBAT fiber, and airing the cross-linked PBAT fiber to prepare the thermal repair CNTs / PBAT composite fiber. The CNTs / PBAT composite fiber disclosed by the invention has the advantages of degradability, thermal repair sensing, light weight, small size, simple manufacturing process and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of functional composite materials, and specifically relates to a degradable thermally repairable CNTs / PBAT composite fiber and a preparation method and application thereof. Background Art

[0002] In the context of the rapid development of modern information technology, wearable sensors can be seen everywhere in life. They are like human sensory organs. Their appearance not only provides people with a more convenient lifestyle, but also makes it easier to explore the world. The base materials of strain sensors can be divided into rigid base materials (metal materials, semiconductor materials) and flexible base materials (polymers). Common rigid base materials of strain sensors include metal wires, metal films and silicon wafers. Rigid materials have poor flexibility and small strain range, which makes it difficult to meet the requirements of the new generation of wearable devices. Flexible polymer fiber materials have significant advantages as flexible substrates for wearable strain sensors. They have unique permeability, biocompatibility, light weight and flexibility. They can fit tightly with any curved surface. They can be woven into clothing, attached to the skin surface, clothing or accessories. They can continuously monitor personal physical, chemical and biological signals in a non-invasive, real-time and comfortable way, and have shown great application potential in various fields such as health monitoring, disease diagnosis, rehabilitation medicine and human-computer interaction.

[0003] Traditional polymers such as polyethylene terephthalate, polycarbonate and silicone rubber are common matrix materials for strain sensors. Their non-degradable and short service life limit their application in wearable devices. Polybutylene adipate / terephthalate PBAT is a degradable material that is more in line with the sustainable development strategy than traditional non-degradable polymer materials. Moreover, PBAT is a semi-crystalline copolymer with the characteristics of crystallization-induced elongation and melt-induced expansion, so it has thermal repair performance, fast repair speed and high repair efficiency, which greatly extends the service life of flexible strain sensors.

[0004] The degradable flexible strain sensor prepared by the present invention through a simple and easy-to-operate method is more in line with the sustainable development strategy. The high bonding strength with CNTs makes it have excellent sensing performance, good durability and resistance to harsh environments, which increases its use scenarios and expands its scope of use in the wearable field. Summary of the invention

[0005] Based on the above-mentioned shortcomings and deficiencies in the prior art, one of the objects of the present invention is to at least solve one or more of the above-mentioned problems in the prior art. In other words, one of the objects of the present invention is to provide a degradable thermally repairable CNTs / PBAT composite fiber and a preparation method and application thereof that meet one or more of the aforementioned needs.

[0006] In order to achieve the above-mentioned object of the invention, the present invention adopts the following technical solutions:

[0007] A method for preparing a degradable thermally repairable CNTs / PBAT composite fiber comprises the following steps:

[0008] (1) premixing polybutylene adipate / terephthalate (PBAT), triallyl isocyanurate (TAIC) and benzophenone (BP), then melt-extruding and cross-linking by ultraviolet radiation to obtain cross-linked PBAT fibers;

[0009] Dispersing carbon nanotubes (CNTs) and sodium dodecyl sulfate (SDS) in a mixed solution of ethyl acetate and anhydrous ethanol and subjecting the mixture to ultrasonic treatment to obtain a CNTs dispersion.

[0010] (2) The cross-linked PBAT fiber is immersed in the CNTs dispersion, taken out and hung to dry, thereby obtaining the thermally repaired CNTs / PBAT composite fiber.

[0011] As a preferred embodiment, in the step (1), the mass ratio of PBAT, TAIC and BP is 100:(1-1.5):(1-1.5).

[0012] As a preferred embodiment, in step (1), the time of ultraviolet radiation cross-linking is 0.5 to 2 hours.

[0013] As a preferred embodiment, in step (1), the ratio of CNTs, SDS, ethyl acetate and anhydrous ethanol is (150-204 mg): (100-136 mg): (100 mL): (0-50 mL).

[0014] As a preferred embodiment, in step (1), the ultrasonic treatment time is 15 to 20 minutes.

[0015] As a preferred embodiment, in step (2), the immersion temperature is 69-72°C.

[0016] As a preferred embodiment, in the step (2), the immersion time is 1 to 20 minutes.

[0017] As a preferred embodiment, in step (2), the hanging and drying time is 24 to 36 hours.

[0018] The present invention also provides a degradable thermally repairable CNTs / PBAT composite fiber prepared by the preparation method described in any of the above schemes.

[0019] The present invention also provides the application of the thermally repaired CNTs / PBAT composite fiber as described in the above scheme for strain sensing.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The CNTs / PBAT composite fiber of the present invention not only has the advantages of being degradable, heat-repairable sensing, light weight, small size and simple manufacturing process, but also has the effect of melt-induced shrinkage under constant and stress-free conditions, which provides power for the self-repairing behavior of the flexible strain sensor, so that the CNTs conductive network destroyed by the hysteresis effect can be repaired efficiently and quickly. Therefore, the flexible strain sensor composite fiber with degradable heat-repair is one of the ideal choices for the new generation of wearable devices. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 are SEM images of the cross-section and surface of the PBAT fiber and the CNTs / PBAT composite fiber of Example 1 of the present invention;

[0023] Figure 2 is a resistance comparison diagram of the cross-linked PBAT fibers of Examples 1-4 of the present invention at different ratios of ethyl acetate to anhydrous ethanol;

[0024] Figure 3 is a comparison chart of the sensing performance of the cross-linked PBAT fibers of Examples 1-4 of the present invention at different ratios of ethyl acetate to anhydrous ethanol;

[0025] Figure 4 is a comparison diagram of the sensing performance of CNTs / PBAT fibers obtained by immersing the cross-linked PBAT fibers of Example 1 of the present invention in a suspension of CNTs and ethyl acetate for 10 minutes;

[0026] Figure 5 is a comparison chart of the sensing performance of the CNTs / PBAT fibers of Examples 1, 5 and 6 of the present invention;

[0027] Figure 6 This is a curve chart of 2000 cycles of the CNTs / PBAT composite fiber of Example 1 of the present invention before and after thermal repair. DETAILED DESCRIPTION

[0028] The technical solution of the present invention will be further described below through specific embodiments.

[0029] Embodiment 1:

[0030] The preparation method of the CNTs / PBAT composite fiber of this embodiment specifically includes the following steps:

[0031] (1) PBAT, TAIC and BP were mixed uniformly at a ratio of 100 g: 1 g: 1.5 g, the mixture was melt-extruded by a twin-screw extruder and then spun by a collecting device, and then irradiated with a UV lamp for cross-linking for 60 minutes to obtain cross-linked PBAT fibers.

[0032] (2) 150 mg of CNTs and 100 mg of SDS were dispersed in a mixed solution of 100 mL of ethyl acetate and 10 mL of anhydrous ethanol, and ultrasonicated for 20 min using a probe ultrasonicator to obtain a uniformly dispersed CNTs suspension solution;

[0033] (3) The cross-linked PBAT fibers were placed in a CNTs suspension solution at a temperature of 71°C for swelling and impregnation. The immersion time was 10 min and the hanging and drying time was 24 h to obtain CNTs / PBAT composite fibers.

[0034] like Figure 1 As shown, the CNTs of the CNTs / PBAT composite fiber prepared in this embodiment are evenly distributed on the surface of the PBAT fiber, constructing a perfect conductive network.

[0035] like Figure 2 As shown in the figure, the resistance of the cross-linked PBAT fiber of this embodiment under different ethyl acetate: anhydrous ethanol, with the increase of anhydrous ethanol, the resistance becomes larger and larger until it basically tends to be stable. The smaller the resistance, the greater the swelling layer, and the greater the damage to the fiber matrix. When ethyl acetate: anhydrous ethanol = 10:3, the resistance tends to be stable and has the best resistance stability.

[0036] like Figure 3 The figure shows the sensing performance of the cross-linked PBAT fiber prepared in Example 1 of the present invention under different conditions of ethyl acetate and anhydrous ethanol. Figure 2 Compared with the properties of ethyl acetate and anhydrous ethanol, too much ethyl acetate will destroy the structure of the fiber, and too much anhydrous ethanol will evaporate quickly at high temperature, which will affect the stability of the resistance of CNTs / PBAT composite fibers ( Figure 3 d). When ethyl acetate: anhydrous ethanol = 10:3, the resistance is the most stable and has the highest measurement factor at strains of 2.5%, 7.5% and 12.5%.

[0037] like Figure 4As shown, the cross-linked PBAT fiber prepared in Example 1 of the present invention is immersed in a suspension of CNTs and ethyl acetate for 10 minutes to obtain a CNTs / PBAT composite fiber. Ten sensing tests are performed at a strain of 12.5%. In 5 cycles, the sensing performance is basically the same as that in Example 1. However, since the pure ethyl acetate solution will destroy the internal structure of the PBAT fiber, it can be seen that after 5 cycles, the fiber matrix is ​​damaged and the sensing performance is destroyed.

[0038] like Figure 5 As shown, the thermal sensing performance of the CNTs / PBAT composite fiber of this embodiment at different immersion times. It can be observed that when the immersion time is 3 minutes, its measurement factor is the lowest. This is mainly because the immersion time is too short, which makes its resistance higher and insensitive under small strain. When the immersion time is 5 minutes, its measurement factor at 2.5% and 7.5% is the largest and very stable. When the immersion time is 10 minutes, due to the extension of the immersion time, more CNTs are deposited on the surface of the PBAT fiber, and the CNTs are entangled together, making it insensitive under small strain, but having a higher measurement factor under 12.5% ​​strain.

[0039] like Figure 6 As shown in the figure, the cycle curve of the CNTs / PBAT composite fiber before and after thermal repair of this embodiment. It can be observed that the sensing performance is basically unchanged before and after thermal repair, and the sensing performance of the repaired CNTs / PBAT composite fiber is very stable after 2000 cycles, indicating that the CNTs / PBAT composite fiber has excellent thermal repair function and prolongs the service life of the CNTs / PBAT fiber strain sensor in practical applications.

[0040] Embodiment 2:

[0041] The preparation method of the CNTs / PBAT composite fiber of this embodiment specifically includes the following steps:

[0042] (1) PBAT, TAIC and BP were mixed uniformly at a ratio of 100 g: 1 g: 1.5 g, the mixture was melt-extruded by a twin-screw extruder and then spun by a collecting device, and then irradiated with a UV lamp for cross-linking for 60 minutes to obtain cross-linked PBAT fibers.

[0043] (2) 150 mg of CNTs and 100 mg of SDS were dispersed in a mixed solution of 100 mL of ethyl acetate and 20 mL of anhydrous ethanol, and ultrasonicated for 20 min using a probe ultrasonicator to obtain a uniformly dispersed CNTs suspension solution;

[0044] (3) The cross-linked PBAT fibers were placed in a CNTs suspension solution at a temperature of 71°C for swelling and impregnation. The immersion time was 10 min and the hanging and drying time was 24 h to obtain CNTs / PBAT composite fibers.

[0045] The CNTs / PBAT composite fiber of this embodiment was characterized by the same method as in Example 1. The results showed that the sensing performance of the composite fiber was similar to that of the composite fiber obtained in Example 1, and the sensing performance was more stable.

[0046] Embodiment 3:

[0047] The preparation method of the CNTs / PBAT composite fiber of this embodiment specifically includes the following steps:

[0048] (1) PBAT, TAIC and BP were mixed uniformly at a ratio of 100 g: 1 g: 1.5 g, the mixture was melt-extruded by a twin-screw extruder and then spun by a collecting device, and then irradiated with a UV lamp for cross-linking for 60 minutes to obtain cross-linked PBAT fibers.

[0049] (2) 150 mg of CNTs and 100 mg of SDS were dispersed in a mixed solution of 100 mL of ethyl acetate and 30 mL of anhydrous ethanol, and ultrasonicated for 20 min using a probe ultrasonicator to obtain a uniformly dispersed CNTs suspension solution;

[0050] (3) The cross-linked PBAT fibers were placed in a CNTs suspension solution at a temperature of 71°C for swelling and impregnation. The immersion time was 10 min and the hanging and drying time was 24 h to obtain CNTs / PBAT composite fibers.

[0051] The CNTs / PBAT composite fiber of this embodiment was characterized by the same method as in Example 1, and its sensing performance under small strain was even better.

[0052] Embodiment 4:

[0053] The preparation method of the CNTs / PBAT composite fiber of this embodiment specifically includes the following steps:

[0054] (1) PBAT, TAIC and BP were mixed uniformly at a ratio of 100 g: 1 g: 1.5 g, the mixture was melt-extruded by a twin-screw extruder and then spun by a collecting device, and then irradiated with a UV lamp for cross-linking for 60 minutes to obtain cross-linked PBAT fibers.

[0055] (2) 150 mg of CNTs and 100 mg of SDS were dispersed in a mixed solution of 100 mL of ethyl acetate and 40 mL of anhydrous ethanol, and sonicated for 20 min using a probe sonicator to obtain a uniformly dispersed CNTs suspension solution;

[0056] (3) The cross-linked PBAT fibers were placed in a CNTs suspension solution at a temperature of 71°C for swelling and impregnation. The immersion time was 10 min and the hanging and drying time was 24 h to obtain CNTs / PBAT composite fibers.

[0057] The CNTs / PBAT composite fiber of this example was characterized by the same method as that of Example 1. The results showed that the resistance of the composite fiber was greater than that obtained in Example 1, and the stability of the resistance was also slightly lower than that in Example 1.

[0058] Embodiment 5:

[0059] The preparation method of the CNTs / PBAT composite fiber of this embodiment specifically includes the following steps:

[0060] (1) PBAT, TAIC and BP were mixed uniformly at a ratio of 100 g: 1 g: 1.5 g, the mixture was melt-extruded by a twin-screw extruder and then spun by a collecting device, and then irradiated with a UV lamp for cross-linking for 60 minutes to obtain cross-linked PBAT fibers.

[0061] (2) 150 mg of CNTs and 100 mg of SDS were dispersed in a mixed solution of 100 mL of ethyl acetate and 30 mL of anhydrous ethanol, and ultrasonicated for 20 min using a probe ultrasonicator to obtain a uniformly dispersed CNTs suspension solution;

[0062] (3) The cross-linked PBAT fiber was placed in a CNTs suspension solution at a temperature of 71°C for swelling and impregnation. The immersion time was 3 minutes and the hanging and drying time was 24 hours to obtain CNTs / PBAT composite fibers.

[0063] The CNTs / EVA composite fiber of this embodiment was characterized by the same method as in Example 1, and the results showed that the sensing performance of the composite fiber was less stable and had a smaller measurement factor than the sensing performance of the composite fiber obtained in Example 1. The reason for this was that the CNTs on the surface of the CNTs / PBAT composite fiber were unevenly distributed due to the short immersion time, resulting in higher resistance.

[0064] Embodiment 6:

[0065] The preparation method of the CNTs / PBAT composite fiber of this embodiment specifically includes the following steps:

[0066] (1) PBAT, TAIC and BP were mixed uniformly at a ratio of 100 g: 1 g: 1.5 g, the mixture was melt-extruded by a twin-screw extruder and then spun by a collecting device, and then irradiated with a UV lamp for cross-linking for 60 minutes to obtain cross-linked PBAT fibers.

[0067] (2) 150 mg of CNTs and 100 mg of SDS were dispersed in a mixed solution of 100 mL of ethyl acetate and 30 mL of anhydrous ethanol, and ultrasonicated for 20 min using a probe ultrasonicator to obtain a uniformly dispersed CNTs suspension solution;

[0068] (3) The cross-linked PBAT fiber was placed in a CNTs suspension solution at a temperature of 71°C for swelling and impregnation. The immersion time was 5 minutes and the hanging and drying time was 24 hours to obtain CNTs / PBAT composite fibers.

[0069] The CNTs / PBAT composite fiber of this embodiment was characterized by the same means as in Example 1, and the results showed that the composite fiber had a more stable sensing performance than that of Example 1. Compared with the immersion time of Example 1, the immersion time of this embodiment was more appropriate. The immersion time of Example 1 was too long, 10 min, which caused the CNTs on the surface of the CNTs / PBAT composite fiber to be entangled, making its sensing performance less stable than that of this embodiment.

[0070] Comparative Example 1:

[0071] The preparation method of the CNTs / PBAT composite fiber of this comparative example specifically comprises the following steps:

[0072] (1) PBAT, TAIC and BP were mixed uniformly at a ratio of 100 g: 1 g: 1.5 g, the mixture was melt-extruded by a twin-screw extruder and then spun by a collecting device, and then irradiated with a UV lamp for cross-linking for 60 minutes to obtain cross-linked PBAT fibers.

[0073] (2) 150 mg of CNTs and 100 mg of SDS were dispersed in 100 mL of ethyl acetate and sonicated for 20 min using a probe sonicator to obtain a uniformly dispersed CNTs suspension solution;

[0074] (3) The cross-linked PBAT fibers were placed in a CNTs suspension solution at a temperature of 71°C for swelling and impregnation. The immersion time was 10 min and the hanging and drying time was 24 h to obtain CNTs / PBAT composite fibers.

[0075] The CNTs / PBAT composite fiber of this embodiment was characterized by the same method as in Example 1. The results showed that the sensing performance of the composite fiber was similar to that of the composite fiber obtained in Example 1. However, the cycle durability of this example was extremely poor. After 5 cycles of stretching and relaxing, the fiber matrix was damaged, which was manifested as increased resistance. The low cycle durability greatly limits the application of PBAT composite fibers in flexible strain sensors.

[0076] Comparative Example 2:

[0077] The preparation method of the CNTs / PBAT composite fiber of this comparative example specifically comprises the following steps:

[0078] (1) PBAT, TAIC, BP ​​and CNTs were mixed uniformly at a ratio of 100 g: 1 g: 1.5 g: 150 mg, the mixture was melt-extruded by a twin-screw extruder and then spun by a collecting device, and then irradiated with a UV lamp for cross-linking for 60 minutes to obtain a cross-linked CNTs / PBAT composite fiber.

[0079] The CNTs / PBAT composite fiber of this example was characterized by the same method as that of Example 1. The results showed that the unit resistance of the composite fiber of this comparative example was basically non-conductive compared with the composite fiber obtained in Example 1.

[0080] In the above embodiment and its alternatives, the mass ratio of PBAT, TAIC and BP can also be 100:1:1, 100:1.5:1, 100:1.2:1.2, etc.

[0081] In the above embodiment and its alternatives, the time of UV radiation cross-linking can also be 0.5h, 1.5h, 2h, etc.

[0082] In the above embodiment and its alternatives, the ratio of CNTs, SDS, ethyl acetate and anhydrous ethanol can also be any ratio of (150-204 mg): (100-136 mg): (100 mL): (0-50 mL), which can be determined according to actual application requirements.

[0083] In the above embodiment and its alternatives, the ultrasonic treatment time can also be 15 minutes, 16 minutes, 18 minutes, etc.

[0084] In the above embodiment and its alternatives, the immersion temperature can also be 69° C., 70° C., 72° C., etc., and the immersion time can also be 1 min, 12 min, 15 min, 18 min, 20 min, etc.

[0085] In the above embodiment and its alternatives, the hanging drying time can also be 30 hours, 32 hours, 36 hours, etc.

[0086] In view of the numerous embodiments of the scheme of the present invention, the raw materials and dosage involved can be selected according to actual needs within the limited range, and the experimental data of each embodiment is huge and numerous, which is not suitable for listing and explaining one by one here, but the content required to be verified and the final conclusion obtained in each embodiment are similar. Therefore, the verification content of each embodiment will not be explained one by one here.

[0087] The above description is only a detailed description of the preferred embodiments and principles of the present invention. For ordinary technicians in this field, according to the ideas provided by the present invention, there will be changes in the specific implementation methods, and these changes should also be regarded as the protection scope of the present invention.

Claims

1. A method for preparing a degradable thermally repairable CNTs / PBAT composite fiber, characterized in that: The following steps are involved: (1) premixing polybutylene adipate / terephthalate (PBAT), triallyl isocyanurate (TAIC) and benzophenone (BP), then melt-extruding and cross-linking by ultraviolet radiation to obtain cross-linked PBAT fibers; Dispersing carbon nanotubes (CNTs) and sodium dodecyl sulfate (SDS) in a mixed solution of ethyl acetate and anhydrous ethanol and subjecting the mixture to ultrasonic treatment to obtain a CNTs dispersion. (2) The cross-linked PBAT fiber is immersed in the CNTs dispersion, taken out and hung to dry, thereby obtaining the thermally repaired CNTs / PBAT composite fiber.

2. The preparation method according to claim 1, characterized in that: In the step (1), the mass ratio of PBAT, TAIC and BP is 100:(1-1.5):(1-1.5).

3. The preparation method according to claim 1, characterized in that: In the step (1), the time of ultraviolet radiation cross-linking is 0.5 to 2 hours.

4. The preparation method according to claim 1, characterized in that: In the step (1), the ratio of CNTs, SDS, ethyl acetate and anhydrous ethanol is (150-204 mg): (100-136 mg): (100 mL): (0-50 mL).

5. The preparation method according to claim 1, characterized in that: In the step (1), the ultrasonic treatment time is 15 to 20 minutes.

6. The preparation method according to claim 1, characterized in that: In the step (2), the immersion temperature is 69-72°C.

7. The preparation method according to claim 6, characterized in that: In the step (2), the immersion time is 1 to 20 minutes.

8. The preparation method according to claim 7, characterized in that: In the step (2), the hanging and drying time is 24 to 36 hours.

9. The degradable thermally repairable CNTs / PBAT composite fiber obtained by the preparation method according to any one of claims 1 to 8.

10. The use of the thermal repair CNTs / PBAT composite fiber according to claim 9, characterized in that: Used for strain sensing.

Citation Information

Patent Citations

  • Composite fiber with shape memory performance and strain sensing performance and preparation method thereof

    CN112376266A

  • Hydrophobically modified starch / PBAT composite film and preparation method thereof

    CN114874476A

  • CNT / EVA shape memory composite material and preparation method thereof

    CN115058046A

  • Preparation method of CNTs / MXene-based composite micro-wrinkled fiber strain sensor

    CN118048785A

  • Carbon nanotube composite comprising mechanical ligands

    WO2023001506A1