PBO fiber surface treatment method

By coordinating transition metal ions on the surface of PBO fibers and grafting small dopamine molecules to form polydopamine macromolecular chains, the problem of insufficient anti-ultraviolet aging performance and surface performance of PBO fibers is solved, and its resistance to ultraviolet aging and interface is significantly improved. Adhesion extends service life and expands application areas.

CN118932730APending Publication Date: 2024-11-12SHANDONG NON METALLIC MATERIAL RESEARCH INSTITUTE
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411275677.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The poor anti-ultraviolet aging and surface properties of PBO fibers limit their application in the fields of protective materials and composite materials.

Method used

By coordinating transition metal ions on the surface of PBO fibers and grafting dopamine small molecules as active centers for oxidation and self-polymerization, polydopamine macromolecule chains are formed, enhancing the fiber's UV aging resistance and surfactivity.

Benefits of technology

It significantly improves the UV aging resistance of PBO fiber, extends its service life, and improves the interface adhesion with the resin matrix, expanding its application field.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118932730A_ABST
    Figure CN118932730A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of high-performance materials, and discloses a PBO fiber surface treatment method which comprises the following steps: firstly, coordinating transition metal ions on the surface layer of a PBO fiber, then grafting dopamine micromolecules by taking the transition metal ions as an active center, and carrying out oxidative auto-polymerization under an alkaline condition to form a polydopamine (PDA) macromolecular chain loaded on the surface of the PBO fiber. The ultraviolet-resistant PBO fiber with high surface performance is obtained. According to the treatment method, raw materials are low in price, preparation is easy and convenient, damage to the original mechanical property and thermal stability of the PBO fiber is small, the ultraviolet aging resistance of the PBO fiber can be remarkably enhanced, the service life of the PBO fiber is prolonged, and the application field of the PBO fiber is expanded; a large number of active sites exist, so that the functionalization of the PBO fiber is favorably realized; the surface of the fiber contains a large number of phenolic hydroxyl groups, amino groups and other polar groups, so that the interfacial shear strength of the PBO fiber and a resin matrix can be improved, and the interfacial adhesion of a PBO fiber composite material can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of high-performance materials and discloses a PBO fiber surface treatment method. Background Art

[0002] Poly (p-phenylene benzobisoxazole) (PBO) fiber is currently a high-performance organic fiber with the best overall properties. Its highly symmetrical, rigid, rod-like molecular structure provides excellent properties, such as high thermal stability, mechanical properties, chemical stability, and abrasion resistance. PBO fiber is widely used in fiber-reinforced composites, high-strength protective ropes, tension structures, UV shields, high-voltage electrical work gloves, bulletproof vests, canvas, and aircraft engine debris barriers. It is a high-end fiber material with dual military and civilian applications.

[0003] However, the poor UV aging resistance and surface properties of PBO fibers limit their application in protective materials, composite materials, and other fields. The poor UV resistance is due to the instability of the five-membered oxazole ring in the PBO macromolecular chain, which easily absorbs high-energy UV light in the wavelength range of 300-340nm. This energy is transferred to the macromolecular chain, causing charge transitions between molecules and chain scission degradation, further leading to a sharp decrease in mechanical strength. Secondly, the poor surface properties are due to the fiber's highly symmetrical molecular structure and the highly parallel arrangement of giant fibrils, forming a unique skin-core structure. The surface is smooth, free of additional reactive groups, and chemically inert.

[0004] Therefore, simultaneously improving the UV aging resistance and surface properties of PBO fibers is an urgent problem to be solved by those skilled in the art. Summary of the Invention

[0005] The present invention addresses the numerous shortcomings of existing technologies and provides a method for treating the surface of poly(ethylene glycol) (PBO) fibers. This method involves first coordinating transition metal ions onto the surface of the PBO fiber. Dopamine molecules are then grafted onto the PBO fiber surface using the transition metal ions as active centers. Under alkaline conditions, these molecules undergo oxidative self-polymerization to form polydopamine macromolecular chains, which are then loaded onto the PBO fiber surface. This method results in UV-resistant PBO fibers with high surface properties. This treatment method utilizes low-cost raw materials, is simple to prepare, and minimally impairs the PBO fiber's inherent mechanical and thermal stability properties. The transition metal ions and PDA on the modified PBO fiber surface synergistically enhance the PBO fiber's resistance to UV aging, extending its service life and expanding its application areas. The PDA-loaded layer on the modified PBO fiber surface contains numerous active sites that can be grafted onto other groups or substrates through covalent or non-covalent interactions, facilitating the functionalization of the PBO fiber. The modified PBO fiber surface contains numerous polar groups, such as phenolic hydroxyl groups and amino groups, which enhance the interfacial shear strength between the PBO fiber and the resin matrix, thereby improving the interfacial adhesion of PBO fiber composites.

[0006] The main principles of the present invention are: The PBO fiber molecular chain contains a large number of aromatic heterocycles, namely benzoxazole five-membered rings, in which the C=N and CO functional groups can react with transition metal ions to form a unique donor-ligand coordination structure. Transition metal ions themselves contain multiple highly active unsaturated coordination sites, such as Fe 3+ There are six unsaturated coordination sites, Cu 2+ Containing four unsaturated coordination sites, transition metal ions can serve as active centers in PBO fibers and further bind to other functional nanomaterials. The artificially synthesized "melanin-like" polydopamine, inspired by mussel protein, has the properties of natural melanin and can absorb ultraviolet light. Its structure contains numerous phenolic hydroxyl and amino active groups, which can be further coordinated to the modified PBO-M fibers, transforming the PBO fibers from hydrophobic to hydrophilic, improving their UV resistance and interfacial properties.

[0007] The inventors used metal ion coordination bonds as intermediate bridges between the fiber and the polymer chain. Specifically, the PBO fiber was subjected to a coordination reaction with a transition metal complex salt, which increased the roughness of the fiber surface. Dopamine small molecules were then grafted onto the transition metal ions, which then oxidatively self-polymerized polydopamine chains under alkaline conditions. This resulted in modified PBO fibers with both UV resistance and interfacial properties. This surface modification method offers advantages such as ease of operation, mild reaction conditions, minimal fiber damage, and a short experimental cycle. It also simultaneously improved the PBO fiber's UV resistance and interfacial properties.

[0008] The specific technical solution of the present invention is: A PBO fiber surface treatment method, the specific steps are as follows: (1) Pretreatment of fiber surface: Place the PBO fiber in a Soxhlet extractor and extract with acetone for 24-72 hours, replacing the solvent every 24 hours. The volume ratio of PBO fiber mass to acetone is 1 g: (30-150) ml each time. The PBO fiber after the above treatment is washed with water and ethanol for 3-5 times, and dried in a vacuum oven at 80-120°C for 1-10 hours to obtain the degreasing agent pretreated PBO fiber.

[0009] (2) Transition metal ions coordinated on the fiber surface: Prepare a 0.2-1 mol / L transition metal ion complex salt solution in anhydrous ethanol and deionized water mixture. Cut the pretreated PBO fibers into 5-10 cm short fiber bundles, place them in the transition metal ion complex salt solution, and react in an oil bath at 30-70°C for 4-8 hours. At this time, the C=N in the benzoxazole ring on the PBO molecular chain undergoes a coordination reaction with the transition metal ion to form a donor-ligand structure; after the reaction is completed, the fiber is taken out and washed with ethanol and deionized water 3-5 times in sequence, and dried under vacuum for 1-10 hours; the fiber obtained at this time is PBO-M fiber.

[0010] In the above step (2), the volume ratio of the PBO fiber mass to the transition metal complex salt solution is (0.1-1) g: (50-200) ml, and the volume ratio of anhydrous ethanol to deionized water is 99-95:1-5; The transition metal ion is Fe 3+ ions or Cu 2+ ions or Zn 2+ ions or Co 2+ ion.

[0011] (3) Grafted polydopamine molecular chain: Deionized water was added to dopamine hydrochloride, and ultrasonically dissolved for 5-30 minutes using an ultrasonic cleaning machine at room temperature and an ultrasonic power of 200-360 W to obtain a fully dissolved dopamine hydrochloride solution; An appropriate amount of PBO-M fiber was completely immersed in a dopamine hydrochloride solution. The pH of the dopamine hydrochloride solution was monitored in real time using a pH meter. Tris(hydroxymethyl)aminomethane buffer solution was continuously added. The pH of the solution was buffered to 8-10 using an ultrasonic cleaner at room temperature and an ultrasonic power of 200-360 W. The solution was then placed in a constant temperature shaker for an oscillation reaction for 12-48 hours at room temperature. In the alkaline environment, dopamine molecules were oxidized and self-polymerized to form polydopamine, which was loaded on the surface of the PBO-M fiber. After the reaction, the fiber was washed with deionized water 3-5 times and dried under vacuum for 1-10 hours to obtain UV-resistant PBO-M-PDA fiber with high surface performance.

[0012] The concentration of the dopamine hydrochloride solution used in the above step (3) is 1-3 g / L; the mass ratio of the PBO-M fiber to the dopamine hydrochloride solution is (0.1-1) g: (50-200) ml; and the concentration of the tris(hydroxymethyl)aminomethane solution used is 0.5-1.5 g / L.

[0013] Wherein, in step (1), the preferred volume ratio of the PBO fiber mass to the acetone solution is 1 g: (30-70) ml.

[0014] Preferably, in step (2), the volume ratio of the PBO fiber mass to the transition metal complex salt solution is 0.1 g: (50-100) ml, and the volume ratio of anhydrous ethanol to deionized water is 99-96:1-4.

[0015] Preferably, the transition metal ion complex salt is one or more of ferric chloride hexahydrate (FeCl3•6H2O), copper sulfate pentahydrate (CuSO4•5H2O), zinc acetate ((CH3COO)2Zn), or cobalt acetate ((CH3COO)2Co).

[0016] Preferably, in step (3), the volume ratio of the PBO-M fiber mass to the dopamine hydrochloride solution is 0.1 g: (100-200) ml; and the concentration of the tris(hydroxymethyl)aminomethane solution is 1-1.5 g / L.

[0017] In the above preparation method, the extracted PBO fiber is subjected to a coordination reaction with a transition metal complex salt. The metal ions are coordinated to increase the roughness of the fiber surface. Then, dopamine small molecules are grafted with the transition metal ions as the active center, and oxidative self-polymerization occurs under alkaline conditions. The surface is loaded with polydopamine molecular chains, resulting in a PBO fiber with both UV resistance and surface performance modification. The above modification process causes minimal damage to the original mechanical and thermal properties of the fiber, effectively protecting the fiber's own mechanical strength. The transition metal ions have a fluorescent emission effect and a synergistic effect with the "melanin"-like polydopamine molecular chains to absorb ultraviolet light, improving the PBO fiber's UV resistance and extending its service life. At the same time, the surface activity of the PBO fiber is improved, greatly enhancing the interfacial bonding between the PBO fiber and the resin matrix. The surface dopamine molecular chains contain a large number of active groups such as amino and hydroxyl groups, which can load other functional molecular groups, further broadening the application areas of PBO fiber.

[0018] In summary, the fiber surface treatment method provided by the present invention has mild reaction conditions and is easy to operate. It can significantly enhance the UV aging resistance of PBO fibers; help to achieve the functionalization of PBO fibers; and improve the interfacial shear strength between PBO fibers and the resin matrix, which is beneficial to improving the interfacial adhesion of PBO fiber composites. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 Schematic diagram of the principle of obtaining modified PBO-M-PDA fiber by the PBO fiber surface treatment method of the present invention. DETAILED DESCRIPTION

[0020] In order to better understand the present invention, the content of the present invention is further illustrated below in conjunction with embodiments. The present invention described herein is only used to explain the present invention and is not used to limit the present invention.

[0021] Example 1 A PBO fiber surface treatment technology includes the following steps: To remove the oil and impurities on the surface of PBO fiber, 10 g of PBO fiber was first placed in a Soxhlet extractor with acetone as the solvent. The volume ratio of PBO fiber mass to acetone solution was 1 g:50 ml, and the extraction was carried out for 48 h. The solvent was replaced every 24 h. The PBO fiber after degreasing was washed three times with water and ethanol, and dried in a vacuum oven at 100 °C for 6 h to obtain pretreated PBO fiber.

[0022] The 0.8 mol / LFeCl3·6H2O salt solution was prepared with anhydrous ethanol and deionized water in a volume fraction ratio of 97:3. The cleaned PBO fibers were cut into 10 cm short fiber bundles and added to the above solution. The PBO fiber mass and salt solution volume ratio was 0.1 g:85 ml. The fibers were reacted in a 50 ℃ oil bath for 6 h. At this time, the C=N in the benzoxazole ring on the PBO molecular chain reacted with the transition metal ion Fe 3+ A coordination reaction occurs, forming a donor-ligand structure. After the reaction, the fiber is removed and washed three times with ethanol and deionized water, followed by drying under vacuum for 6 hours. The resulting fiber is PBO-Fe fiber.

[0023] Deionized water was added to dopamine hydrochloride and ultrasonically dissolved in an ultrasonic cleaner at room temperature and 360 W power for 15 minutes to obtain a fully dissolved 2 g / L dopamine hydrochloride solution. 0.5 g of PBO-Fe fiber was completely immersed in the 2 g / L dopamine hydrochloride solution. The volume ratio of the PBO-Fe fiber to the dopamine hydrochloride solution was 0.1 g:100 ml. The pH of the dopamine hydrochloride solution was monitored in real time using a pH meter. 1.2 g / L Tris solution was continuously added to buffer the pH to 8.5. The solution was placed on a thermostatic shaker at room temperature for 24 hours. After the reaction, it was washed with deionized water and dried under vacuum to obtain the PBO-Fe-PDA fiber.

[0024] The UV aging test conditions are as follows: the dried fibers are evenly spread on the sample rack, and the sample rack is placed in the UV light box parallel to the UV lamp tube, with a radiation intensity of 1100 W / m 2 The temperature in the box is 60℃, the humidity is 60%, the fiber is 10cm away from the lamp, and the aging time is 288h.

[0025] Filament Pullout Testing: Filament pullout testing, where a fiber is pulled from a drop of cured epoxy resin, is the fastest and most effective method for evaluating the interfacial shear strength (IFSS) between the fiber and matrix.

[0026] PBO fiber monofilaments, before and after modification, were secured to an aluminum support using double-sided tape. Epoxy droplets were applied to the monofilaments with an embedding length of 50-70 mm using a fine-point applicator. The samples were cured at 75°C for 2 hours, 120°C for 2 hours, and 150°C for 4 hours. After curing, IFSS testing was performed using a composite interface structure analyzer (MODEL HM410, Tohei Sanyon) at a feed rate of 2 mm / min.

[0027] Testing showed that the initial strength of the PBO-Fe-PDA fiber prepared in this example was 4.21 GPa, and the tensile strength retention rate of the PBO-Fe-PDA fiber after 288 hours of UV aging was 67.62%. The interfacial shear strength (IFSS) between the modified PBO-Fe-PDA and the epoxy resin matrix was 58.72 MPa.

[0028] The initial strength of the untreated PBO fiber was 4.47 GPa, and the tensile strength retention rate of the PBO fiber after 288 h of UV aging was 30.87%. The interfacial shear strength (IFSS) between the unmodified PBO and epoxy resin matrix was 36.52 MPa.

[0029] Example 2

[0030] A PBO fiber surface treatment technology includes the following steps: To remove the oil and impurities on the surface of PBO fiber, 10 g of PBO fiber was first placed in a Soxhlet extractor with acetone as the solvent. The volume ratio of PBO fiber mass to acetone solution was 1 g:50 ml, and the extraction was carried out for 48 h. The solvent was replaced every 24 h. The PBO fiber after degreasing was washed three times with water and ethanol, and dried in a vacuum oven at 100 °C for 6 h to obtain pretreated PBO fiber.

[0031] A 0.6 mol / LCuSO4•5H2O salt solution was prepared with anhydrous ethanol and deionized water in a volume fraction ratio of 97:3 as a mixed solvent. The cleaned PBO fibers were cut into 10 cm short fiber bundles and added to the above solution. The PBO fiber mass and salt solution volume ratio was 0.1 g: 60 ml. The fibers were reacted in a 55 °C oil bath for 6 h. At this time, the C=N in the benzoxazole ring on the PBO molecular chain reacted with the transition metal ion Cu 2+ A coordination reaction occurs, forming a donor-ligand structure. After the reaction, the fiber is removed and washed three times with ethanol and deionized water, followed by drying under vacuum for 8 hours. The resulting fiber is PBO-Cu fiber.

[0032] Deionized water was added to dopamine hydrochloride and ultrasonically dissolved in an ultrasonic cleaner at room temperature and 360 W power for 15 minutes to obtain a fully dissolved 1.5 g / L dopamine hydrochloride solution. 0.5 g of PBO-Cu fiber was completely immersed in the 1.5 g / L dopamine hydrochloride solution. The volume ratio of the PBO-Cu fiber to the dopamine hydrochloride solution was 0.1 g:150 ml. The pH of the dopamine hydrochloride solution was monitored in real time using a pH meter. 1 g / L Tris solution was continuously added to buffer the pH to 8.5. The solution was placed on a thermostatic shaker at room temperature for 24 hours. After the reaction, it was washed with deionized water and dried under vacuum to obtain PBO-Cu-PDA fiber.

[0033] The UV aging test and the single-filament pull-out test method are the same as those in Example 1.

[0034] Testing showed that the initial strength of the PBO-Cu-PDA fiber prepared in this example was 4.12 GPa, and the tensile strength retention rate of the PBO-Cu-PDA fiber after 288 hours of UV aging was 76.23%. The interfacial shear strength (IFSS) between the modified PBO-Cu-PDA and the epoxy resin matrix was 54.28 MPa.

[0035] The initial strength of the untreated PBO fiber was 4.47 GPa, and the tensile strength retention of the PBO fiber after 288 h of UV aging was 30.87%. The interfacial shear strength (IFSS) between the unmodified PBO and epoxy resin matrix was 36.52 MPa.

[0036] Example 3 A PBO fiber surface treatment technology includes the following steps: To remove the oil and impurities on the surface of PBO fiber, 10 g of PBO fiber was first placed in a Soxhlet extractor with acetone as the solvent. The volume ratio of PBO fiber mass to acetone solution was 1 g:50 ml, and the extraction was carried out for 48 h. The solvent was replaced every 24 h. The PBO fiber after degreasing was washed three times with water and ethanol, and dried in a vacuum oven at 100 °C for 3 h to obtain pretreated PBO fiber.

[0037] A 0.5 mol / L (CH3COO)2Zn salt solution was prepared with anhydrous ethanol and deionized water in a volume fraction ratio of 97:3 as a mixed solvent. The cleaned PBO fibers were cut into 10 cm short fiber bundles and added to the above solution. The PBO fiber mass and salt solution volume ratio was 0.1 g: 100 ml. The fibers were reacted in an oil bath at 65 °C for 8 h. At this time, the C=N in the benzoxazole ring on the PBO molecular chain reacted with the transition metal ion Zn. 2+A coordination reaction occurs, forming a donor-ligand structure. After the reaction, the fibers are removed and washed three times with ethanol and deionized water, followed by drying under vacuum for 10 hours. The resulting fibers are PBO-Zn fibers.

[0038] Deionized water was added to dopamine hydrochloride and ultrasonically dissolved in an ultrasonic cleaner at room temperature and 360 W power for 15 minutes to obtain a fully dissolved 2 g / L dopamine hydrochloride solution. 0.5 g of PBO-Zn fiber was completely immersed in the 2 g / L dopamine hydrochloride solution. The volume ratio of the PBO-Zn fiber to the dopamine hydrochloride solution was 0.1 g:150 ml. The pH of the dopamine hydrochloride solution was monitored in real time using a pH meter. 1.2 g / L Tris solution was then continuously added to buffer the pH to 9. The solution was placed on a thermostatic shaker at room temperature for 24 hours. After the reaction, it was washed with deionized water and dried under vacuum to obtain the PBO-Zn-PDA fiber.

[0039] The UV aging test and the single-filament pull-out test method are the same as those in Example 1.

[0040] Testing showed that the initial strength of the PBO-Zn-PDA fiber prepared in this example was 3.89 GPa, still meeting performance requirements. Furthermore, after 288 hours of UV aging, the PBO-Zn-PDA fiber retained 74.83% of its tensile strength. The interfacial shear strength (IFSS) between the modified PBO-Zn-PDA and the epoxy resin matrix was 50.26 MPa.

[0041] The initial strength of the untreated PBO fiber was 4.47 GPa, and the tensile strength retention rate of the PBO fiber after 288 h of UV aging was 30.87%. The interfacial shear strength (IFSS) between the unmodified PBO and epoxy resin matrix was 36.52 MPa.

[0042] Comparative Example With reference to the solution of Example 1 described in CN201911121606.X, the inventors designed this comparative example, and the specific steps are as follows: The fibers were ultrasonically dissolved in a cleaning machine for 10 minutes to obtain a dopamine hydrochloride solution, and the PBO fibers were extracted with acetone for 48 hours to obtain extracted fibers. The extracted fibers were immersed in the dopamine hydrochloride solution, and tris(hydroxymethylaminomethane) was added. The fibers were ultrasonically dissolved in an ultrasonic cleaning machine at room temperature and a power of 300 W for 10 minutes to make the pH of the solution 9.0 after the addition of tris(hydroxymethylaminomethane). The fibers were then shaken in a shaking table at room temperature and a frequency of 120 r / min for 24 hours. Finally, the fibers were taken out and washed repeatedly with deionized water twice, and dried in an oven at a temperature of 100°C for 1 hour to obtain pretreated PBO fibers. Methanol was added to Zn(NO3)2, and then ultrasonically dissolved for 10 minutes using an ultrasonic cleaner at room temperature and a power of 300 W to obtain a Zn(NO3)2 solution with a concentration of 100 mg / ml. The pretreated PBO fiber was immersed in the Zn(NO3)2 solution and shaken for 10 minutes in a shaker at room temperature and a frequency of 120 r / min to obtain a fiber-containing Zn(NO3)2 solution. Methanol was added to 2-methylimidazole, and then ultrasonically dissolved for 10 minutes using an ultrasonic cleaner at room temperature and a power of 300 W to obtain a 2-methylimidazole solution. The 2-methylimidazole solution was added to the Zn(NO3)2 solution containing the PBO fiber at a speed of 1 mL / s and shaken for 24 hours in a shaker at room temperature and a frequency of 120 r / min. Finally, the fiber was taken out and washed repeatedly with methanol twice, and dried in an oven at a temperature of 70°C for 2 hours to obtain the PBO fiber loaded with a metal organic framework compound medium. The PBO fiber loaded with a metal organic framework compound medium was immersed in n-hexane to obtain a PBO fiber solution loaded with a metal organic framework compound medium; a transition metal ion solution was prepared using FeCl3•6H2O and methanol, and the transition metal ion solution was added dropwise to the fiber solution loaded with a metal organic framework compound medium at a speed of 10uL / s, and oscillated in a shaker at room temperature and a frequency of 120 r / min for 12 hours. Finally, the fiber was taken out and dried in an oven at a temperature of 70°C for 6 hours to obtain a fiber with transition metal ions loaded on the surface, thereby completing the reinforcement of PBO fiber by loading transition metal ions on the fiber surface.

[0043] Testing showed that the PBO fiber with transition metal ions on its surface, prepared in this comparative example, retained a tensile strength of 2.89 GPa after 240 hours of UV aging, with a retention rate of 64.7%. The unmodified PBO fiber's tensile strength had dropped from 4.60 GPa to 2.33 GPa, a performance loss of nearly 50%.

[0044] By comparison, it can be seen that the tensile strength retention rates of the modified PBO-M-PDA fibers after UV aging for 288 h in Examples 1-3 are much higher than that of the modified PBO fibers in the comparative examples, and the interfacial shear strength between the modified PBO-M-PDA fibers and the epoxy resin matrix in Examples 1-3 are much stronger than that of the unmodified PBO fibers. Therefore, the present invention is beneficial for extending the service life of the PBO fibers, enhancing the interfacial bonding strength between the fibers and the resin, and the reaction conditions are mild. The excellent mechanical properties of the PBO fibers are still maintained after modification, which greatly broadens the application field of the PBO fibers.

[0045] The above embodiments illustrate and describe the basic principles, product features, and advantages of the method of the present invention. The present invention is not limited to the above embodiments. Various changes and improvements may be made to the present invention without departing from the scope of the present invention, all of which are required to be included in the scope of protection.

Claims

1. A PBO fiber surface treatment method, characterized in that: The specific steps are as follows: (1) Pretreatment of fiber surface: Place the PBO fiber in a Soxhlet extractor and extract with acetone as solvent for 24-72 h, changing the solvent every 24 h. The volume ratio of PBO fiber mass to acetone is 1 g: (30-150) ml each time. The PBO fiber after the above treatment is washed with water and ethanol for 3-5 times, and dried in a vacuum oven at 80-120°C for 1-10 h to obtain the degreasing agent pretreated PBO fiber; (2) Transition metal ions coordinated on the fiber surface: Anhydrous ethanol and deionized water are used as a mixed solvent to prepare a 0.2-1 mol / L transition metal ion complex salt solution, the PBO fiber obtained in the previous step is cut into 5-10 cm short fiber bundles, which are placed in the above transition metal ion complex salt solution and reacted in a 30-70 ℃ oil bath for 4-8 h; after the reaction is completed, the fiber is taken out and washed with ethanol and deionized water for 3-5 times in sequence, and dried under vacuum for 1-10 h; the fiber obtained at this time is PBO-M fiber; (3) Grafted polydopamine molecular chain: Add deionized water to dopamine hydrochloride, and dissolve it by ultrasonic cleaning for 5-30 min at room temperature and an ultrasonic power of 200-360 W to obtain a fully dissolved dopamine hydrochloride solution; Take an appropriate amount of PBO-M fiber and completely immerse it in the dopamine hydrochloride solution. Use a pH meter to monitor the pH of the dopamine hydrochloride solution in real time. Continue to add tris(hydroxymethyl)aminomethane buffer solution. Use an ultrasonic cleaner to buffer the solution pH to 8-10 at room temperature and an ultrasonic power of 200-360 W. Place the above solution in a constant temperature shaker at room temperature for oscillation reaction for 12-48 h. In an alkaline environment, dopamine molecules are oxidized and self-polymerized into polydopamine and loaded on the surface of the PBO-M fiber. After the reaction, wash with deionized water for 3-5 times and dry under vacuum for 1-10 h to obtain UV-resistant PBO-M-PDA fiber with high surface performance.

2. The PBO fiber surface treatment method according to claim 1, characterized in that: In step (1), the volume ratio of the PBO fiber mass to the acetone solution is 1 g: (30-70) ml each time.

3. The PBO fiber surface treatment method according to claim 1, characterized in that: In step (2), the volume ratio of the PBO fiber mass to the transition metal complex salt solution is (0.1-1) g: (50-200) ml, and the volume ratio of anhydrous ethanol to deionized water is 99-95: 1-5.

4. The PBO fiber surface treatment method according to claim 3, characterized in that: In step (2), the volume ratio of the PBO fiber mass to the transition metal complex salt solution is 0.1 g: (50-100) ml, and the volume ratio of anhydrous ethanol to deionized water is 99-96: 1-4.

5. The PBO fiber surface treatment method according to claim 1, characterized in that: The transition metal ion in step (2) is Fe 3+ Ion or Cu 2+ Ion or Zn 2+ Ion or Co 2+ ion.

6. The PBO fiber surface treatment method according to claim 1 or 5, characterized in that: The transition metal ion complex salt in step (2) is one or more of ferric chloride hexahydrate, copper sulfate pentahydrate, zinc acetate, or cobalt acetate.

7. The PBO fiber surface treatment method according to claim 1, characterized in that: The concentration of the dopamine hydrochloride solution used in step (3) is 1-3 g / L; the mass ratio of the PBO-M fiber to the volume of the dopamine hydrochloride solution is (0.1-1) g: (50-200) ml.

8. The PBO fiber surface treatment method according to claim 1, characterized in that: The concentration of the tris(hydroxymethyl)aminomethane solution in step (3) is 0.5-1.5 g / L.

9. The PBO fiber surface treatment method according to claims 7 and 8, characterized in that: In step (3), the mass ratio of the PBO-M fiber to the volume of the dopamine hydrochloride solution is 0.1 g: (100-200) ml; the concentration of the tris(hydroxymethyl)aminomethane solution is 1-1.5 g / L.

Citation Information

Cited By

  • Full-process recovery method of fiber reinforced composite material

    CN121930545A