Preparation method of double-sided anti-cracking printed composite fabric
By using trimethylallyl ammonium chloride and pectinase pretreatment and microwave curing of silica resin in alkaline environment, the problem of blurred patterns of double-sided printed fabrics after friction is solved, and crack resistance is achieved and improve the anti-friction color fastness.
Patent Information
- Application Number
- CN202411426150.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-14
- Publication Date
- 2024-11-12
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing double-sided printed fabrics are prone to friction during wear and cleaning, resulting in blurred and unsightly patterns and lack crack resistance.
Pretreatment of cotton fabrics using trimethylallyl ammonium chloride and pectinase in alkaline environments to enhance the puffing and hydrophilicity of cellulose fibers and coat dioxide with double-sided digital inkjet printing Silicone is microwave-cured to form a crack-resistant printed composite fabric.
Improves the anti-friction fastness and crack resistance of printed fabrics, and maintains the freshness and durability of the pattern.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of multi-layer fabrics, in particular to a method for preparing a double-sided anti-cracking printed composite fabric. Background Art
[0002] With the development of economy and the continuous improvement of people's living standards, people's pursuit of beauty, fashion and personalization is getting higher and higher. The diversity, personalization and integration of textiles in expression form have become an important development trend in today's era. Printing, as a key part of improving textile quality, increasing textile added value and enriching textile expression forms, has attracted more and more attention. From the emergence and development of double-sided printing and the comparison with traditional single-sided printing, process flow and application in material field, it can be seen that the emergence and development of double-sided digital printing is based on the advantages of other printings to innovate and use technology to maximize the value of fabrics. The emergence of double-sided printing technology reflects that the public is no longer satisfied with the current printing and needs more innovative and distinctive product presentations, but the general printed patterns will be rubbed and blurred and unsightly with the number of wears and washings. Therefore, it is particularly necessary to invent a double-sided anti-cracking printed composite fabric. Summary of the invention
[0003] The purpose of the present invention is to provide a method for preparing a double-sided anti-cracking printed composite fabric to solve the problems existing in the prior art.
[0004] In order to solve the above technical problems, the present invention provides the following technical solutions: a double-sided anti-cracking printed composite fabric, wherein the preparation method of the double-sided anti-cracking printed composite fabric comprises the following preparation steps: (1) Trimethylallyl ammonium chloride, pectinase and deionized water are mixed, stirred at 70-100 rpm for 20-40 min, sodium hydroxide solution is added until the pH value of the solution is 8.5-9.5, then cotton fabric is immersed in the solution, heated to 30-40°C, immersed for 30-60 min, and treated with a padder, baked at 80°C for 5-8 min, then placed in a 6wt% sodium hydroxide aqueous solution, heated to 60°C, left to stand for 30 min, washed with deionized water for 3-5 times, and dried to obtain a pretreated fabric; (2) performing double-sided digital inkjet printing on the pretreated fabric, drying, washing once with deionized water, and baking to obtain a double-sided printed fabric; (3) The silica resin is coated on the double-sided printed fabric with a thickness of 0.04-0.1 mm, and microwave curing is performed to obtain a double-sided anti-cracking printed composite fabric.
[0005] Furthermore, in step (1), the mass ratio of trimethylallyl ammonium chloride, pectinase and deionized water is 1-4:5:100.
[0006] Furthermore, in step (1), the cotton fabric is impregnated at a bath ratio of 1:10-15.
[0007] Furthermore, the rolling margin in step (1) is 60-80%.
[0008] Furthermore, the drying conditions in step (1) are as follows: temperature is 50-70° C. and time is 1 h.
[0009] Furthermore, the area of the printed color block in step (2) is 25 cm×10 cm, and the inkjet volume is 100%.
[0010] Furthermore, the baking conditions in step (2) are: temperature of 80-100° C. and time of 20-50 min.
[0011] Furthermore, the baking conditions in step (2) are as follows: temperature is 120-130° C. and time is 10-20 min.
[0012] Furthermore, the silica resin in step (3) is prepared from silica, acrylic acid, vinyl triethoxysilane, azobisisobutyronitrile, butyl methacrylate and butyl acetate in a mass ratio of 5-10:35-50:1-3:12-30:8-10.
[0013] Furthermore, the process parameters of the microwave treatment in step (3) are: power of 750-1000 W and time of 1-5 min.
[0014] Compared with the prior art, the beneficial effects achieved by the present invention are: The present invention uses allyl ammonium chloride and pectinase to pretreat cotton fabric under an alkaline environment, which can not only make cellulose fibers swell, but also well remove impurities such as lipids, phenols and pectin on the surface of cellulose textiles, so that the alcohol hydroxyl groups on the glucose rings are exposed, and the hydrophilicity and permeation of the fabric are improved, thereby promoting ionic bonding between the cationic groups in the allyl ammonium chloride and the anionic groups of the printing dye to form a lake, which is deposited on the fabric, and the molecular ring structures with similar structures of the two form van der Waals forces, further improving the bonding ability, thereby achieving the anti-friction color fastness of the fabric, and then coating a layer of silicon dioxide resin, and performing microwave treatment and curing treatment, so that the printed fabric can achieve the anti-cracking effect. DETAILED DESCRIPTION
[0015] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0016] Example 1; (1) trimethylallyl ammonium chloride, pectinase and deionized water were mixed, stirred at 70 rpm for 20 min, sodium hydroxide solution was added until the solution pH was 8.5, then cotton fabric was immersed in the solution at a bath ratio of 1:10, heated to 30°C, immersed for 30 min, and treated with a padder after immersion, with a padding rate of 60%, baked at 80°C for 5 min, then placed in a 6wt% sodium hydroxide aqueous solution, heated to 60°C, left to stand for 30 min, washed with deionized water for 3 times, and dried at 50°C for 1 h to obtain a pretreated fabric; the mass ratio of trimethylallyl ammonium chloride, pectinase and deionized water was 1:5:100; (2) Double-sided digital inkjet printing was performed on the pretreated fabric, the area of the printed color block was 25 cm × 10 cm, the inkjet volume was 100%, dried at 80°C for 20 min, washed once with deionized water, and baked at 120°C for 10 min to obtain a double-sided printed fabric; (3) Coating a silica resin on a double-sided printed fabric with a thickness of 0.04 mm, curing it for 1 min under a microwave power of 750 W, and obtaining a double-sided anti-cracking printed composite fabric; the silica resin is prepared from silica, acrylic acid, vinyl triethoxysilane, azobisisobutyronitrile, butyl methacrylate, and butyl acetate in a mass ratio of 5:35:1:12:8.
[0017] Example 2; (1) trimethylallyl ammonium chloride, pectinase and deionized water were mixed, stirred at 80 rpm for 30 min, sodium hydroxide solution was added until the solution pH was 9, then cotton fabric was immersed in the solution at a bath ratio of 1:13, heated to 35°C, immersed for 45 min, and treated with a padder after immersion, with a padding rate of 70%, baked at 80°C for 6 min, then placed in a 6wt% sodium hydroxide aqueous solution, heated to 60°C, left to stand for 30 min, washed with deionized water 4 times, and dried at 60°C for 1 h to obtain a pretreated fabric; the mass ratio of trimethylallyl ammonium chloride, pectinase and deionized water was 2:5:100; (2) Double-sided digital inkjet printing was performed on the pretreated fabric, the area of the printed color block was 25 cm × 10 cm, the inkjet volume was 100%, dried at 90°C for 40 min, washed once with deionized water, and baked at 125°C for 15 min to obtain a double-sided printed fabric; (3) Coating a silica resin on a double-sided printed fabric with a thickness of 0.07 mm, curing it for 3 minutes under a microwave power of 900 W, and obtaining a double-sided anti-cracking printed composite fabric; the silica resin is prepared from silica, acrylic acid, vinyl triethoxysilane, azobisisobutyronitrile, butyl methacrylate, and butyl acetate in a mass ratio of 8:40:2:20:9.
[0018] Example 3; (1) trimethylallyl ammonium chloride, pectinase and deionized water were mixed, stirred at 100 rpm for 40 min, sodium hydroxide solution was added until the solution pH was 9.5, then cotton fabric was immersed in the solution at a bath ratio of 1:15, heated to 40°C, immersed for 60 min, and treated with a padder after immersion, with a padding rate of 80%, baked at 80°C for 8 min, then placed in a 6wt% sodium hydroxide aqueous solution, heated to 60°C, left to stand for 30 min, washed with deionized water for 5 times, and dried at 70°C for 1 h to obtain a pretreated fabric; the mass ratio of trimethylallyl ammonium chloride, pectinase and deionized water was 4:5:100; (2) Double-sided digital inkjet printing was performed on the pretreated fabric, the area of the printed color block was 25 cm × 10 cm, the inkjet volume was 100%, dried at 100°C for 50 min, washed once with deionized water, and baked at 130°C for 20 min to obtain a double-sided printed fabric; (3) Coating a silica resin on a double-sided printed fabric with a thickness of 0.1 mm, curing it for 5 minutes under a microwave power of 1000 W, and obtaining a double-sided anti-cracking printed composite fabric; the silica resin is prepared from silica, acrylic acid, vinyl triethoxysilane, azobisisobutyronitrile, butyl methacrylate, and butyl acetate in a mass ratio of 10:50:3:30:10.
[0019] Comparative Example 1: The difference between Comparative Example 1 and Example 2 is that step (1) is different. Step (1) is changed to: pectinase and deionized water are mixed, stirred at 80 rpm for 30 minutes, sodium hydroxide solution is added until the solution pH is 9, then cotton fabric is immersed in it at a bath ratio of 1:13, heated to 35°C, immersed for 45 minutes, and the immersed cotton fabric is treated with a padder, the padding rate is 70%, baked at 80°C for 6 minutes, then placed in a 6wt% sodium hydroxide aqueous solution, heated to 60°C, left to stand for 30 minutes, washed with deionized water 4 times, and dried at 60°C for 1 hour to obtain a pretreated fabric; the mass ratio of pectinase to deionized water is 5:100; the remaining steps are the same as Example 2.
[0020] Comparative Example 2: The difference between Comparative Example 2 and Example 2 is that step (1) is different. Step (1) is changed to: trimethylallyl ammonium chloride and deionized water are mixed, stirred at 80 rpm for 30 minutes, sodium hydroxide solution is added until the pH of the solution is 9, and then the cotton fabric is immersed in it at a bath ratio of 1:13, the temperature is raised to 35°C, and the soaking is carried out for 45 minutes. The cotton fabric after the immersion is treated with a padder, and the padding rate is 70%. The fabric is baked at 80°C for 6 minutes, and then placed in a 6wt% sodium hydroxide aqueous solution, heated to 60°C, allowed to stand for 30 minutes, washed with deionized water 4 times, and dried at 60°C for 1 hour to obtain a pretreated fabric. The mass ratio of trimethylallyl ammonium chloride to deionized water is 2:100. The remaining steps are the same as those in Example 2.
[0021] Effect example Table 1 below shows the performance analysis results of the double-sided anti-cracking printed composite fabrics using Examples 1 to 3 of the present invention and Comparative Examples 1 to 2.
[0022]
[0023] From the comparison of the experimental data of the embodiment and the comparative example in Table 1, it can be found that the present invention uses allyl ammonium chloride and pectinase to pretreat cotton fabric. Under an alkaline environment, not only can the cellulose fiber be expanded, but also impurities such as lipids, phenols and pectin on the surface of cellulose textiles can be well removed, so that the alcohol hydroxyl groups on the glucose ring are exposed, the hydrophilicity and permeation of the fabric are improved, thereby promoting the ionic bonding of the cationic groups in the allyl ammonium chloride and the anionic groups of the printing dye to form a lake, and the molecular ring structures with similar structures of the two form van der Waals forces, further improving the binding ability, thereby achieving the anti-friction color fastness of the fabric, and then coating a layer of silica resin, and performing microwave curing treatment, so that the printed fabric can achieve the anti-cracking effect.
[0024] It will be apparent to those skilled in the art that the invention is not limited to the details of the exemplary embodiments described above and that the invention can be implemented in other specific forms without departing from the spirit or essential features of the invention. Therefore, the embodiments should be considered in all respects as exemplary and non-limiting, and the scope of the invention is defined by the appended claims rather than the foregoing description, and it is intended that all variations within the meaning and scope of the equivalent elements of the claims be included in the invention. Any marking in a claim should not be considered as limiting the claim to which it relates.
Claims
1. A double-sided anti-cracking printed composite fabric, characterized in that: The preparation method of the double-sided anti-cracking printed composite fabric comprises the following preparation steps: (1) Trimethylallyl ammonium chloride, pectinase and deionized water are mixed, stirred at 70-100 rpm for 20-40 min, sodium hydroxide solution is added until the pH value of the solution is 8.5-9.5, then cotton fabric is immersed in the solution, heated to 30-40°C, immersed for 30-60 min, and treated with a padder, baked at 80°C for 5-8 min, then placed in a 6wt% sodium hydroxide aqueous solution, heated to 60°C, left to stand for 30 min, washed with deionized water for 3-5 times, and dried to obtain a pretreated fabric; (2) performing double-sided digital inkjet printing on the pretreated fabric, drying, washing once with deionized water, and baking to obtain a double-sided printed fabric; (3) The silica resin is coated on the double-sided printed fabric with a thickness of 0.04-0.1 mm, and microwave curing is performed to obtain a double-sided anti-cracking printed composite fabric.
2. A double-sided anti-cracking printed composite fabric according to claim 1, characterized in that: The mass ratio of trimethylallyl ammonium chloride, pectinase and deionized water in step (1) is 1-4:5:
100.
3. The double-sided anti-cracking printed composite fabric according to claim 1, characterized in that: The cotton fabric in step (1) is impregnated at a bath ratio of 1:10-15.
4. The double-sided anti-cracking printed composite fabric according to claim 1, characterized in that: The rolling margin in step (1) is 60-80%.
5. The double-sided anti-cracking printed composite fabric according to claim 1, characterized in that: The drying conditions in step (1) are as follows: temperature is 50-70°C and time is 1 hour.
6. The double-sided anti-cracking printed composite fabric according to claim 1, characterized in that: The area of the printed color block in step (2) is 25 cm×10 cm, and the inkjet amount is 100%.
7. The double-sided anti-cracking printed composite fabric according to claim 1, characterized in that: The drying conditions in step (2) are as follows: temperature of 80-100° C. and time of 20-50 min.
8. The double-sided anti-cracking printed composite fabric according to claim 1, characterized in that: The baking conditions in step (2) are as follows: temperature of 120-130° C. and time of 10-20 min.
9. The double-sided anti-cracking printed composite fabric according to claim 1, characterized in that: The silica resin in step (3) is prepared from silica, acrylic acid, vinyl triethoxysilane, azobisisobutyronitrile, butyl methacrylate and butyl acetate in a mass ratio of 5-10:35-50:1-3:12-30:8-10.
10. The double-sided anti-cracking printed composite fabric according to claim 1, characterized in that: The process parameters of the microwave treatment in step (3) are: power of 750-1000 W and time of 1-5 min.
Citation Information
Patent Citations
Production process of photosensitive color-changing printed fabric
CN102505530A
Multifunctional printed fabric
CN103556472A
Method for improving inkjet printing definition, color yield and vividness of silk fabric
CN106498772A
Digital printing method of home textile fabric
CN106930128A
Water-free, low-energy-consumption and high-quality inkjet printing method for cellulose fabric