Double-color composite packaging paper and production process thereof

By mixing bleached coniferous wood pulp and reed pulp in the packaging paper and adding antibacterial agents and other ingredients, the problems of poor antibacterial properties and insufficient mechanical properties of existing packaging paper are solved, and a two-color composite packaging paper with excellent performance is prepared, suitable for Food packaging and other fields.

CN118932786APending Publication Date: 2024-11-12ZHEJIANG YISHU PAPER GRP CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202410997658.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The antibacterial properties of existing packaging paper are poor and the mechanical properties are insufficient, which affects its quality and quality.

Method used

Using the two-color composite wrapping paper production process, by mixing bleaching coniferous wood pulp and reed pulp, adding antibacterial agent, nanotitanium dioxide, nanozirconium phosphate and other components, combining cationic starch and PAE wet strength agent, passing through a multi-layer slurry box and long net Paper machine processing to prepare two-color composite wrapping paper with excellent antibacterial and mechanical properties.

Benefits of technology

It significantly improves the antibacterial and mechanical properties of two-color composite wrapping paper, ensures its quality and quality, and is suitable for food packaging and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004960697980000111
    Figure BDA0004960697980000111
  • Figure BDA0004960697980000121
    Figure BDA0004960697980000121
Patent Text Reader

Abstract

The invention relates to the technical field of papermaking, in particular to double-color composite packaging paper and a production process thereof. Under the'bridge 'action of glycerol diglycidyl ether, dodecyl triphenyl phosphonium bromide is effectively'grafted' on the surface of the pretreated nano zinc oxide; the obtained solid product is ultrasonically dispersed in a tetradecyl dimethyl benzyl ammonium chloride aqueous solution, so that tetradecyl dimethyl benzyl ammonium chloride can be uniformly adsorbed and detained on the surface of the pretreated nano-zinc oxide, and finally the antibacterial agent is prepared; the obtained antibacterial agent has an excellent antibacterial performance function under the synergistic cooperation of the nano zinc oxide, the dodecyl triphenyl phosphonium bromide and the tetradecyl dimethyl benzyl ammonium chloride; the antibacterial agent and the nano zirconium phosphate are matched with each other, so that the antibacterial property of the double-color composite packaging paper can be further improved; in addition, the prepared double-color composite packaging paper also has excellent mechanical properties, and the quality of the double-color composite packaging paper is effectively ensured.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of papermaking, in particular to a two-color composite packaging paper and a production process thereof. Background Art

[0002] Wrapping paper refers to the paper used for packaging, which has high strength, low moisture content, low air permeability, no corrosion, certain water resistance and is beautiful to use. At the same time, the paper used for food packaging also requires hygiene, sterility, and no contamination and impurities. Wrapping paper can be divided into ordinary wrapping paper, special wrapping paper, trademark paper, oil-proof wrapping paper and moisture-proof wrapping paper. It usually has high strength and toughness. Various types of wrapping paper have different properties and uses. For example, special fruit wrapping paper is thin and soft. Photosensitive protective paper is not light-transmissive. Oil-proof wrapping paper has the property of preventing grease penetration. Moisture-proof wrapping paper has moisture-proof properties. Trademark paper is used for packaging after printing. Ordinary wrapping paper is mostly used for general commodity packaging, and the quality requirements are not strict.

[0003] A method for producing wrapping paper is disclosed in a patent document with application number "CN201510449094.5" and titled "A method for producing wrapping paper". The technical solution provided in this patent document has the advantages of being simple in method, and the produced wrapping paper can be naturally degraded, has no pollution to the environment, is non-toxic in itself, and has a wide range of applications. However, its antibacterial properties are relatively poor, which affects its quality to a certain extent. At the same time, its mechanical properties are relatively insufficient and still need to be further improved or enhanced. Based on this, the present invention provides a two-color composite wrapping paper and its production process! Summary of the invention

[0004] The purpose of the present invention is to provide a two-color composite packaging paper and a production process thereof. The produced two-color composite packaging paper not only has good antibacterial properties, but also has excellent mechanical properties, effectively ensuring its quality.

[0005] To achieve the above object, the present invention provides the following technical solutions:

[0006] In a first aspect, the present invention provides a production process for a two-color composite packaging paper, comprising the following steps:

[0007] Step 1, mixing and pulping bleached conifer pulp and reed pulp in a weight ratio of 1:0.5-2.5, mixing and stirring the obtained composite pulp evenly after pulping and pulping, and pumping the obtained first mixed pulp into a first pulping tank for storage and standby;

[0008] Step 2: The unbleached bamboo pulp is subjected to pulping treatment, and then the pulp is pumped into a pulp preparation tank after being screened by a fiber classification screen, and then cationic starch and PAE wet strength agent are added thereto, and after mixing and stirring evenly, the obtained second mixed pulp is pumped into a second pulping tank for storage and standby use;

[0009] Step 3, adding the antibacterial agent into clean water to prepare an antibacterial agent dispersion with a concentration of 15-20wt%, and then adding 10-15% sodium carboxymethyl cellulose, 8-12% nano titanium dioxide, and 10-20% nano zirconium phosphate by weight of the antibacterial agent respectively, and after ultrasonic mixing, the obtained third mixed slurry is stored and used for standby;

[0010] Step 4: The first mixed slurry and the second mixed slurry are concentrated and filtered to remove residues, and then a retention aid is added. After screening, the first mixed component is introduced into the lower layer / upper layer of the multi-layer headbox, and the second mixed component is introduced into the upper layer / lower layer of the multi-layer headbox; then the third mixed slurry is introduced into the middle layer of the multi-layer headbox, and then processed through the papermaking process of the fourdrinier paper machine to obtain a finished two-color composite packaging paper.

[0011] Furthermore, cationic starch and PAE wet strength agent are added to the composite pulp in sequence during the pulping process in step one; wherein the amount of cationic starch is 0.2-0.5% of the total dry mass of the bleached coniferous pulp and reed pulp, and the amount of PAE wet strength agent is 0.3-0.5% of the total dry mass of the bleached coniferous pulp and reed pulp.

[0012] Furthermore, the fiber length of the bleached coniferous pulp is 5 to 10 mm, and the fiber length of the reed pulp is 2 to 4 mm; the beating concentration of the bleached coniferous pulp is 4 to 5%, the beating degree is 22 to 25°SR, and the wet weight is 10 to 12 g.

[0013] Furthermore, the step three also includes a surface sizing process, and the amount of sizing is 2 to 5 g / m 2 The surface sizing agent used is prepared by uniformly mixing 5-8wt% cationic starch aqueous solution and AKD neutral sizing agent with a mass of 10-20% of cationic starch.

[0014] Furthermore, the reed pulp and unbleached bamboo pulp have a pulping concentration of 5.5-6.0%, a beating degree of 42-45°SR, and a wet weight of 1.5-1.8 g.

[0015] Furthermore, the preparation method of the antibacterial agent is as follows: add dodecyl triphenylphosphonium bromide with a mass of 20-40% of the pretreated nano zinc oxide to a pretreated nano zinc oxide aqueous dispersion with a concentration of 0.02-0.05 g / mL, stir and mix evenly, and then stir and react at a temperature of 70-85° C. for 3-6 hours. After the reaction is completed, filter, wash and dry the reaction product in sequence; after drying, add the obtained solid material in a dosage ratio of 0.05-0.08 g / mL into a 0.05-0.2 g / mL tetradecyl dimethyl benzyl ammonium chloride aqueous solution, ultrasonically disperse it evenly, centrifuge it, discard the supernatant, and then dry the obtained solid substrate to obtain the antibacterial agent.

[0016] Furthermore, the preparation method of the pretreated nano zinc oxide is: adding nano zinc oxide into deionized water at a solid-liquid ratio of 0.01 to 0.03 g / mL, and then adding glycerol diglycidyl ether with a mass of 0.3 to 0.6 times that of the nano zinc oxide, mixing and stirring evenly, and then keeping warm and stirring at a temperature of 60 to 80° C. for 5 to 8 hours. After the reaction is completed, the obtained product components are separated into solid and liquid, the filter cake is first washed with deionized water for 2 to 3 times, and then washed with acetone for 2 to 3 times. After washing, it is vacuum dried, and the final product is the pretreated nano zinc oxide.

[0017] Furthermore, in the step 2, the amount of cationic starch used is 0.3-0.4% of the absolute dry mass of the unbleached bamboo pulp, and the amount of PAE wet strength agent used is 0.2-0.35% of the absolute dry mass of the unbleached bamboo pulp.

[0018] Furthermore, the retention aid is polyacrylamide, and the amount of the retention aid is 2-4% and 3-4% of the first mixed slurry and the second mixed slurry respectively.

[0019] In a second aspect, the present invention provides a two-color composite packaging paper, which is produced by the production process described above.

[0020] Compared with the prior art, the present invention has the following beneficial effects:

[0021] The invention puts nano zinc oxide into deionized water and adds glycerol diglycidyl ether, and then performs heat preservation reaction to make the two chemically react and bond, and then performs solid-liquid separation, washing and vacuum drying on the resultant components in sequence to obtain pretreated nano zinc oxide. Then the pretreated nano zinc oxide is made into a pretreated nano zinc oxide aqueous phase dispersion, and dodecyl triphenyl phosphonium bromide is added thereto, mixed and stirred evenly, and then heat-insulated to react, and finally dodecyl triphenyl phosphonium bromide is effectively "grafted" on the surface of the pretreated nano zinc oxide under the "bridge" effect of glycerol diglycidyl ether. The obtained solid product is ultrasonically dispersed in a tetradecyl dimethyl benzyl ammonium chloride aqueous solution so that the tetradecyl dimethyl benzyl ammonium chloride can be uniformly adsorbed and retained on the surface of the pretreated nano zinc oxide, and finally an antibacterial agent is prepared. The obtained antibacterial agent has excellent antibacterial performance function under the synergistic cooperation of nano zinc oxide, dodecyl triphenyl phosphonium bromide and tetradecyl dimethyl benzyl ammonium chloride. In addition, the antibacterial agent and nano zirconium phosphate cooperate with each other, which can further improve the antibacterial performance of the two-color composite packaging paper. In addition, the two-color composite packaging paper prepared by the present invention also has excellent mechanical properties, effectively ensuring its quality.

[0022] In summary, the two-color composite packaging paper produced by the present invention not only has good antibacterial properties, but also has excellent mechanical properties, which effectively guarantees its quality. DETAILED DESCRIPTION

[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] A production process for two-color composite packaging paper comprises the following steps:

[0026] Step 1, bleached conifer pulp and reed pulp are mixed and pulped in a weight ratio of 1:0.5, the obtained composite pulp is pulped and mixed and stirred evenly, and the obtained first mixed pulp is pumped into the first pulping tank for storage and standby;

[0027] Step 2, the unbleached bamboo pulp is subjected to pulping treatment, and then the unbleached bamboo pulp is screened by a fiber classification screen and then pumped into a pulp preparation tank, and then cationic starch and PAE wet strength agent are added thereto, and after mixing and stirring evenly, the obtained second mixed pulp is pumped into a second pulping tank for storage and standby; wherein the amount of cationic starch is 0.3% of the absolute dry mass of the unbleached bamboo pulp, and the amount of PAE wet strength agent is 0.2% of the absolute dry mass of the unbleached bamboo pulp;

[0028] Step 3, adding the antibacterial agent into clean water to prepare an antibacterial agent dispersion with a concentration of 15wt%, and then adding 10% sodium carboxymethyl cellulose, 8% nano titanium dioxide, and 10% nano zirconium phosphate by weight of the antibacterial agent respectively, and after ultrasonic mixing, the obtained third mixed slurry is stored and used for standby;

[0029] Step 4: The first mixed slurry and the second mixed slurry are sequentially concentrated and filtered to remove residues, and then a retention aid is added. After screening, the first mixed component is introduced into the lower layer / upper layer of the multi-layer headbox, and the second mixed component is introduced into the upper layer / lower layer of the multi-layer headbox; then the third mixed slurry is introduced into the middle layer of the multi-layer headbox, and then processed in the papermaking process of the fourdrinier paper machine to obtain a finished two-color composite packaging paper;

[0030] The retention aid is polyacrylamide, and the amount of the retention aid is 2% and 3% of the first mixed slurry and the second mixed slurry respectively.

[0031] During the pulping process of step one, cationic starch and PAE wet strength agent are added to the composite pulp in sequence; wherein, the amount of cationic starch is 0.2% of the total dry mass of bleached coniferous pulp and reed pulp, and the amount of PAE wet strength agent is 0.3% of the total dry mass of bleached coniferous pulp and reed pulp.

[0032] The fiber length in bleached coniferous pulp is 5 mm, and the fiber length in reed pulp is 2 mm; the pulping concentration of bleached coniferous pulp is 4%, the beating degree is 22°SR, and the wet weight is 10 g; the pulping concentration of reed pulp and unbleached bamboo pulp is 5.5%, the beating degree is 42°SR, and the wet weight is 1.5 g.

[0033] Step 3 also includes a surface sizing process, and the amount of glue applied is 2g / m 2 The surface sizing agent used is prepared by uniformly mixing a 5wt% cationic starch aqueous solution and an AKD neutral sizing agent with a mass percentage of 10% of the cationic starch.

[0034] The preparation method of the antibacterial agent comprises the following steps: adding dodecyl triphenylphosphonium bromide whose mass is 20% of the pretreated nano zinc oxide to a pretreated nano zinc oxide aqueous phase dispersion liquid with a concentration of 0.02 g / mL, stirring and mixing evenly, and then reacting at a temperature of 70°C with heat preservation and stirring for 3 hours; after the reaction is completed, filtering, washing and drying the reaction product in sequence; after drying, adding the obtained solid material into a 0.05 g / mL tetradecyl dimethyl benzyl ammonium chloride aqueous solution at a dosage ratio of 0.05 g / mL, ultrasonically dispersing the obtained solid material evenly, centrifuging the obtained solid material, discarding the supernatant, and then drying the obtained solid substrate to obtain the antibacterial agent.

[0035] The preparation method of pretreated nano zinc oxide is as follows: nano zinc oxide is put into deionized water at a solid-liquid ratio of 0.01 g / mL, and then glycerol diglycidyl ether with a mass that is 0.3 times that of nano zinc oxide is added thereto, and after mixing and stirring evenly, the mixture is kept stirred and reacted at a temperature of 60°C for 5 hours. After the reaction is completed, the obtained product components are separated into solid and liquid, and the filter cake is first washed twice with deionized water and then washed twice with acetone. After washing, it is vacuum dried to obtain the pretreated nano zinc oxide.

[0036] Example 2

[0037] A production process for two-color composite packaging paper comprises the following steps:

[0038] Step 1, bleached conifer pulp and reed pulp are mixed and pulped in a weight ratio of 1:2, the obtained composite pulp is pulped and mixed and stirred evenly, and the obtained first mixed pulp is pumped into the first pulping tank for storage and standby;

[0039] Step 2, the unbleached bamboo pulp is subjected to pulping treatment, and then the unbleached bamboo pulp is screened by a fiber classification screen and then pumped into a pulp preparation tank, and then cationic starch and PAE wet strength agent are added thereto, and after mixing and stirring evenly, the obtained second mixed pulp is pumped into a second pulping tank for storage and standby; wherein the amount of cationic starch is 0.35% of the absolute dry mass of the unbleached bamboo pulp, and the amount of PAE wet strength agent is 0.3% of the absolute dry mass of the unbleached bamboo pulp;

[0040] Step 3, adding the antibacterial agent into clean water to prepare an antibacterial agent dispersion with a concentration of 15wt%, and then adding 12% sodium carboxymethyl cellulose, 10% nano titanium dioxide, and 15% nano zirconium phosphate by weight of the antibacterial agent respectively, and after ultrasonic mixing, the obtained third mixed slurry is stored and used for standby;

[0041] Step 4: The first mixed slurry and the second mixed slurry are concentrated and filtered to remove residues, and then a retention aid is added. After screening, the first mixed component is introduced into the lower layer / upper layer of the multi-layer headbox, and the second mixed component is introduced into the upper layer / lower layer of the multi-layer headbox; then the third mixed slurry is introduced into the middle layer of the multi-layer headbox, and then processed by the papermaking process of the fourdrinier paper machine to obtain a two-color composite packaging paper product; wherein, the retention aid is polyacrylamide, and the amount of the retention aid is 3% and 3.5% of the first mixed slurry and the second mixed slurry, respectively.

[0042] During the pulping process of step one, cationic starch and PAE wet strength agent are added to the composite pulp in sequence; wherein, the amount of cationic starch is 0.3% of the total dry mass of bleached coniferous pulp and reed pulp, and the amount of PAE wet strength agent is 0.4% of the total dry mass of bleached coniferous pulp and reed pulp.

[0043] The fiber length in bleached coniferous pulp is 8 mm, and the fiber length in reed pulp is 3 mm; the pulping concentration of bleached coniferous pulp is 4%, the beating degree is 23°SR, and the wet weight is 10 g; the pulping concentration of reed pulp and unbleached bamboo pulp is 5.5%, the beating degree is 43°SR, and the wet weight is 1.6 g.

[0044] Step 3 also includes a surface sizing process, and the amount of glue applied is 3g / m 2 The surface sizing agent used is prepared by uniformly mixing a 6wt% cationic starch aqueous solution and an AKD neutral sizing agent with a mass percentage of 15% of the cationic starch.

[0045] The preparation method of the antibacterial agent comprises the following steps: adding dodecyl triphenylphosphonium bromide whose mass is 30% of the pretreated nano zinc oxide to a pretreated nano zinc oxide aqueous phase dispersion liquid with a concentration of 0.03 g / mL, stirring and mixing evenly, and then reacting at a temperature of 80°C with heat preservation and stirring for 5 hours; after the reaction is completed, filtering, washing and drying the reaction product in sequence; after drying, adding the obtained solid material into a 0.1 g / mL tetradecyl dimethyl benzyl ammonium chloride aqueous solution at a dosage ratio of 0.06 g / mL, ultrasonically dispersing the obtained solid material evenly, centrifuging the obtained solid material, discarding the supernatant, and then drying the obtained solid substrate to obtain the antibacterial agent.

[0046] The preparation method of pretreated nano zinc oxide is as follows: nano zinc oxide is put into deionized water at a solid-liquid ratio of 0.02 g / mL, and then glycerol diglycidyl ether with a mass that is 0.5 times that of nano zinc oxide is added thereto, and after mixing and stirring evenly, the mixture is kept stirred and reacted at a temperature of 70°C for 6 hours. After the reaction is completed, the obtained product components are separated into solid and liquid, and the filter cake is first washed twice with deionized water and then washed three times with acetone. After washing, it is vacuum dried to obtain the pretreated nano zinc oxide.

[0047] Example 3

[0048] A production process for two-color composite packaging paper comprises the following steps:

[0049] Step 1, bleached conifer pulp and reed pulp are mixed and pulped in a weight ratio of 1:2.5, the obtained composite pulp is pulped and mixed and stirred evenly, and the obtained first mixed pulp is pumped into the first pulping tank for storage and standby;

[0050] Step 2, the unbleached bamboo pulp is subjected to pulping treatment, and then the unbleached bamboo pulp is screened by a fiber classification screen and then pumped into a pulp preparation tank, and then cationic starch and PAE wet strength agent are added thereto, and after mixing and stirring evenly, the obtained second mixed pulp is pumped into a second pulping tank for storage and standby; wherein the amount of cationic starch is 0.4% of the absolute dry mass of the unbleached bamboo pulp, and the amount of PAE wet strength agent is 0.35% of the absolute dry mass of the unbleached bamboo pulp;

[0051] Step 3, adding the antibacterial agent into clean water to prepare an antibacterial agent dispersion with a concentration of 20wt%, and then adding 15% sodium carboxymethyl cellulose, 12% nano titanium dioxide, and 20% nano zirconium phosphate by weight of the antibacterial agent respectively, and after ultrasonic mixing, the obtained third mixed slurry is stored and used for standby;

[0052] Step 4: The first mixed slurry and the second mixed slurry are concentrated and filtered to remove residues, and then a retention aid is added. After screening, the first mixed component is introduced into the lower layer / upper layer of the multi-layer headbox, and the second mixed component is introduced into the upper layer / lower layer of the multi-layer headbox; then the third mixed slurry is introduced into the middle layer of the multi-layer headbox, and then processed through the papermaking process of the fourdrinier paper machine to obtain a two-color composite packaging paper product; wherein, the retention aid is polyacrylamide, and the amount of the retention aid is 4% and 4% of the first mixed slurry and the second mixed slurry, respectively.

[0053] During the pulping process of step one, cationic starch and PAE wet strength agent are added to the composite pulp in sequence; wherein the amount of cationic starch is 0.5% of the total dry mass of bleached coniferous pulp and reed pulp, and the amount of PAE wet strength agent is 0.5% of the total dry mass of bleached coniferous pulp and reed pulp.

[0054] The fiber length in bleached coniferous pulp is 10 mm, and the fiber length in reed pulp is 4 mm; the pulping concentration of bleached coniferous pulp is 5%, the beating degree is 25°SR, and the wet weight is 12 g; the pulping concentration of reed pulp and unbleached bamboo pulp is 6.0%, the beating degree is 45°SR, and the wet weight is 1.8 g.

[0055] Step 3 also includes a surface sizing process, and the amount of glue applied is 5g / m 2 The surface sizing agent used is prepared by uniformly mixing 8 wt % of cationic starch aqueous solution and AKD neutral sizing agent with a mass of 20 wt % of cationic starch.

[0056] The preparation method of the antibacterial agent comprises the following steps: adding dodecyl triphenylphosphonium bromide whose mass is 40% of the pretreated nano zinc oxide to a pretreated nano zinc oxide aqueous phase dispersion liquid with a concentration of 0.05 g / mL, stirring and mixing evenly, and then reacting at a temperature of 85°C with heat preservation and stirring for 6 hours; after the reaction is completed, filtering, washing and drying the reaction product in sequence; after drying, adding the obtained solid material into a 0.2 g / mL tetradecyl dimethyl benzyl ammonium chloride aqueous solution at a dosage ratio of 0.08 g / mL, ultrasonically dispersing the obtained solid material evenly, centrifuging the obtained solid material, discarding the supernatant, and then drying the obtained solid substrate to obtain the antibacterial agent.

[0057] The preparation method of pretreated nano zinc oxide is as follows: nano zinc oxide is put into deionized water at a solid-liquid ratio of 0.03 g / mL, and then glycerol diglycidyl ether with a mass 0.6 times that of nano zinc oxide is added thereto, and after mixing and stirring evenly, the mixture is kept stirred and reacted at a temperature of 80°C for 8 hours. After the reaction is completed, the obtained product components are separated into solid and liquid, and the filter cake is first washed 3 times with deionized water and then washed 3 times with acetone. After washing, it is vacuum dried to obtain the pretreated nano zinc oxide.

[0058] Comparative Example 1: The difference between this embodiment and embodiment 1 is that an equal amount of nano zinc oxide is used to replace the antibacterial agent in this embodiment.

[0059] Comparative Example 2: The difference between this embodiment and embodiment 1 is that nano zirconium phosphate is not used in this embodiment.

[0060] Comparative Example 3: The difference between this example and Example 1 is that: in this example, tetradecyl dimethyl benzyl ammonium chloride aqueous solution is not used.

[0061] Performance test: The relevant properties of the two-color composite packaging paper samples provided in Examples 1 to 3 and Comparative Examples 1 to 3 were tested respectively, and the obtained test data were recorded in the following table:

[0062]

[0063]

[0064] By comparing and analyzing the relevant data in the table, it can be seen that the produced two-color composite packaging paper not only has good antibacterial properties, but also has excellent mechanical properties, effectively ensuring its quality. This shows that the two-color composite packaging paper and its production process provided by the present invention have a broader market prospect and are more suitable for promotion.

[0065] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0066] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.

Claims

1. A production process for two-color composite packaging paper, characterized in that: The following steps are involved: Step 1, mixing and pulping bleached conifer pulp and reed pulp in a weight ratio of 1:0.5-2.5, mixing and stirring the obtained composite pulp evenly after pulping and pulping, and pumping the obtained first mixed pulp into a first pulping tank for storage and standby; Step 2: The unbleached bamboo pulp is subjected to pulping treatment, and then the pulp is pumped into a pulp preparation tank after being screened by a fiber classification screen, and then cationic starch and PAE wet strength agent are added thereto, and after mixing and stirring evenly, the obtained second mixed pulp is pumped into a second pulping tank for storage and standby use; Step 3, adding the antibacterial agent into clean water to prepare an antibacterial agent dispersion with a concentration of 15-20wt%, and then adding 10-15% sodium carboxymethyl cellulose, 8-12% nano titanium dioxide, and 10-20% nano zirconium phosphate by weight of the antibacterial agent respectively, and after ultrasonic mixing, the obtained third mixed slurry is stored and used for standby; Step 4: The first mixed slurry and the second mixed slurry are concentrated and filtered to remove residues, and then a retention aid is added. After screening, the first mixed component is introduced into the lower layer / upper layer of the multi-layer headbox, and the second mixed component is introduced into the upper layer / lower layer of the multi-layer headbox; then the third mixed slurry is introduced into the middle layer of the multi-layer headbox, and then processed through the papermaking process of the fourdrinier paper machine to obtain a finished two-color composite packaging paper.

2. The two-color composite packaging paper and process according to claim 1, characterized in that: During the pulping process of step one, cationic starch and PAE wet strength agent are added to the composite pulp in sequence; wherein, the amount of cationic starch is 0.2-0.5% of the total dry mass of bleached coniferous pulp and reed pulp, and the amount of PAE wet strength agent is 0.3-0.5% of the total dry mass of bleached coniferous pulp and reed pulp.

3. The two-color composite packaging paper and process according to claim 1, characterized in that: The fiber length of the bleached coniferous pulp is 5-10 mm, and the fiber length of the reed pulp is 2-4 mm; the beating concentration of the bleached coniferous pulp is 4-5%, the beating degree is 22-25°SR, and the wet weight is 10-12 g.

4. The two-color composite packaging paper and process according to claim 1, characterized in that: The step 3 also includes a surface sizing process, and the amount of sizing is 2 to 5 g / m 2 The surface sizing agent used is prepared by uniformly mixing 5-8wt% cationic starch aqueous solution and AKD neutral sizing agent with a mass of 10-20% of cationic starch.

5. The two-color composite packaging paper and process according to claim 1, characterized in that: The reed pulp and unbleached bamboo pulp have a pulping concentration of 5.5-6.0%, a beating degree of 42-45°SR, and a wet weight of 1.5-1.8g.

6. The two-color composite packaging paper and process thereof according to claim 1, characterized in that: The preparation method of the antibacterial agent comprises the following steps: adding dodecyl triphenylphosphonium bromide whose mass is 20-40% of the pretreated nano zinc oxide to a pretreated nano zinc oxide aqueous phase dispersion liquid with a concentration of 0.02-0.05 g / mL, stirring and mixing evenly, and then reacting at a temperature of 70-85° C. with heat preservation and stirring for 3-6 hours; after the reaction is completed, filtering, washing and drying the reaction product in sequence; after drying, adding the obtained solid material into a 0.05-0.2 g / mL tetradecyl dimethyl benzyl ammonium chloride aqueous solution at a dosage ratio of 0.05-0.08 g / mL, ultrasonically dispersing evenly, centrifuging, discarding the supernatant, and then drying the obtained solid substrate to obtain the antibacterial agent.

7. The two-color composite packaging paper and process according to claim 6, characterized in that: The preparation method of the pretreated nano zinc oxide is as follows: adding nano zinc oxide into deionized water at a solid-liquid ratio of 0.01-0.03 g / mL, then adding glycerol diglycidyl ether in an amount 0.3-0.6 times the mass of the nano zinc oxide, mixing and stirring evenly, and then reacting at a temperature of 60-80° C. with stirring for 5-8 hours, after the reaction is completed, performing solid-liquid separation on the obtained product components, washing the filter cake with deionized water for 2-3 times, and then washing with acetone for 2-3 times, and after washing is completed, vacuum drying the filter cake, and finally obtaining the pretreated nano zinc oxide.

8. The two-color composite packaging paper and process according to claim 1, characterized in that: In the step 2, the amount of cationic starch used is 0.3-0.4% of the absolute dry mass of the unbleached bamboo pulp, and the amount of PAE wet strength agent used is 0.2-0.35% of the absolute dry mass of the unbleached bamboo pulp.

9. The two-color composite packaging paper and process according to claim 1, characterized in that: The retention aid is polyacrylamide, and the dosage of the retention aid is 2-4% and 3-4% of the first mixed slurry and the second mixed slurry respectively.

10. A two-color composite packaging paper, characterized in that: The double-color composite packaging paper is prepared by the production process of the double-color composite packaging paper described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • Antibacterial packaging paper

    CN105113332A

  • Natural-color liquid packaging paper and production process thereof

    CN106245459A

  • Antibacterial glaze material

    CN106348608A

  • Preparation method for antibacterial finishing agent used for textile fabric

    CN106468021A

  • Paper made fromcarboxymethyl cellulose modified nano titanium dioxide

    CN107237207A