Falling ball impact test method and device for light physical glass in heating state

By conducting multiple ball-falling impact tests on lightweight physically chemical glass under heating, the problem that the existing technology cannot truly simulate the impact resistance of photovoltaic modules at high temperatures is solved, and a comprehensive evaluation of glass performance is achieved and the testing is improved. accuracy and reliability.

CN118937117APending Publication Date: 2024-11-12QINGHAI HUANGHE HYDROPOWER DEV CO LTD XINING SOLAR POWER BRANCH +3
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411076257.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing photovoltaic module testing methods cannot truly simulate and evaluate the impact resistance of glass in high temperature and hot spots, and traditional testing methods cannot comprehensively evaluate the performance of glass under different impact conditions.

Method used

The ball impact test method of lightweight physical glass in heating state is used, and spaced ball impact is performed by setting temperature programs and multiple test positions to simulate the actual application environment of photovoltaic modules at high temperatures and evaluate the structural strength and reliability of the glass.

Benefits of technology

A comprehensive test of light physical glass of photovoltaic modules under high temperature and multiple impact conditions is achieved, providing a more realistic performance evaluation, improving the accuracy and reliability of the test, and being able to more comprehensively evaluate the components in the actual working environment. performance in.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118937117A_ABST
    Figure CN118937117A_ABST
Patent Text Reader

Abstract

The invention relates to a falling ball impact test method and device for light physical glass in a heating state, and belongs to the technical field of reliability test of photovoltaic modules. The method comprises the following steps: setting temperature programs of a heating stage, a constant temperature stage, a testing stage and a cooling stage; at the beginning of the test stage, carrying out an interval falling ball impact test on a plurality of test positions on the smooth surface of the light physical glass at the same time; and when the cooling stage is started, the interval falling ball impact test is ended. According to the invention, a plurality of positions of the light physical glass are subjected to multiple falling ball impact tests after being heated under a temperature program, so that the comprehensive test conditions of multiple impact and multiple height impact on multiple positions of the single glass in a heated and high-temperature state are realized; the condition of severe weather such as hail or sand storm when the light physical glass in the photovoltaic module has hot spots is simulated to the maximum extent, and the performance of the glass under different impact conditions can be comprehensively evaluated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photovoltaic component reliability testing, and in particular relates to a falling ball impact testing method and device for lightweight physical and chemical glass in a heated state. Background Art

[0002] In recent years, the photovoltaic industry has continued to pursue high efficiency, reliability and cost-effectiveness. The thickness of tempered glass used to encapsulate double-glass modules has been tending to be thinner, from 3.2mm to 2.5mm, 2.0mm, and 1.6mm. At the same time, in order to improve the power generation efficiency of the modules, a new product of glazed grid lightweight physical and chemical glass has been launched. This product is a one or more layers of white glaze printed on the surface of the back glass to form a grid pattern. The glaze layer usually contains TiO2, which can significantly enhance the utilization rate of the module light, thereby increasing the module power. However, the glaze layer of photovoltaic glazed glass has a different expansion coefficient from the glass body. Even after special processing, the glaze layer will still produce a certain stress on the glass, thereby increasing the risk of self-explosion of the glass due to uneven internal stress and reducing its ability to withstand impact.

[0003] At present, the impact resistance of glass is tested according to the standard GB / T 41314-2022 for coated glass for building photovoltaic modules. For lightweight physical and chemical glass with a thickness of 2.0 mm to 3.2 mm, a 227±2g steel ball is used. For glass with a thickness of ≥3.2 mm, a 1040g steel ball is used to fall freely from a height of 1 meter from the sample surface without breaking. For the front glass, the impact point is within 25 mm from the center of the sample. For the back glass, the impact point is the middle position between the edge of the glass and the edge of the opening. Each piece of glass is impacted only at one position and the number of impacts is 1.

[0004] With the rapid development of the photovoltaic industry, the reliability and durability of photovoltaic modules have become the focus of attention. In practical applications, photovoltaic modules often face various environmental challenges, among which the hot spot phenomenon is a key issue. The hot spot phenomenon can cause local overheating of photovoltaic modules. Some experts have observed that the outdoor hot spot temperature has reached more than 190°C, thus affecting the performance and life of the module. Therefore, it is necessary to develop a new test method to more realistically simulate and evaluate the impact resistance of photovoltaic modules under high temperature and hot spot conditions. Summary of the invention

[0005] In view of the above problems, the present invention provides a falling ball impact test method and device for lightweight physical and chemical glass under a heated state. On the one hand, performing falling ball impact under a high temperature state can be closer to the actual simulated fracture condition; on the other hand, applying the same impact force at different positions of the same piece of glass can evaluate the stress distribution of the glass when subjected to external force, thereby more comprehensively assessing its structural strength.

[0006] The first object of the present invention is to provide a drop ball impact test method for lightweight physical and chemical glass in a heated state, comprising:

[0007] Set the temperature program for heating stage, constant temperature stage, test stage and cooling stage;

[0008] At the beginning of the test phase, a spaced drop ball impact test is performed simultaneously on a plurality of test locations on the light surface of the lightweight physical and chemical glass;

[0009] When the cooling phase begins, the interval drop ball impact test ends.

[0010] Furthermore, when the lightweight physical and chemical glass is a front plate lightweight physical and chemical glass, the test positions include a first position, a second position and a third position;

[0011] The first position is distributed within 25 mm of the center position of the light surface of the front panel lightweight physical and chemical glass;

[0012] The second position is distributed within a range of 25 mm from the intersection of a tangent line of 1 / 4 of a long side and a midline of a short side in the front plate lightweight physical and chemical glass;

[0013] The third position is distributed within 10mm of the center position of the corner battery half-piece of the front panel lightweight physical and chemical glass;

[0014] The second position and the third position are located on both sides of the midline of the long side of the lightweight physical and chemical glass of the front plate.

[0015] Further, the falling ball height at the first position is 1±0.05m;

[0016] The ball drop height at the second position is 0.7±0.05m;

[0017] The ball falling height at the third position is 0.5±0.05m.

[0018] Furthermore, when the lightweight physical and chemical glass is a back panel lightweight physical and chemical glass, the test position includes a fourth position and a fifth position;

[0019] The fourth position is distributed within a 10mm range between any two holes on the light surface of the back panel lightweight physical and chemical glass;

[0020] The fifth position is distributed within a range of 5 mm from the intersection of a tangent line of 1 / 4 of a long side of the back panel lightweight physical and chemical glass and a midline of a short side.

[0021] Furthermore, the ball falling height at the fourth position is 0.5±0.05m; and the ball falling height at the fifth position is 0.7±0.05m.

[0022] Furthermore, in the interval drop ball impact test, the interval time is 2-3 minutes.

[0023] Furthermore, the heating rate in the heating stage is 7-10°C / min, and the insulation time in the constant temperature stage is 15-25min.

[0024] Furthermore, the temperature of the test stage is 190-210°C, the test time of the test stage is 10-15min, the cooling rate of the cooling stage is 13-18°C / min; the mass of the steel ball used in the ball impact test is 227±2g.

[0025] Furthermore, the falling ball impact test method further comprises:

[0026] The reliability of the lightweight physical and chemical glass as the lightweight physical and chemical glass in the photovoltaic module is judged based on the results of several interval drop ball impact tests.

[0027] The second object of the present invention is to provide a drop ball impact test device for lightweight physical and chemical glass in a heated state, comprising:

[0028] Temperature control device: used to set the temperature program of heating stage, constant temperature stage, test stage and cooling stage; also used to end the interval drop ball impact test at the beginning of the cooling stage

[0029] Drop ball steel tube: used to perform interval drop ball impact tests on several test positions on the smooth surface of lightweight physical and chemical glass at the beginning of the test phase;

[0030] Several brackets: used to support lightweight physical and chemical glass;

[0031] The ball-dropping steel pipe is embedded in a hole arranged on a side wall of the temperature control device, and a plurality of the brackets are placed in the temperature control device.

[0032] Beneficial effects of the present invention:

[0033] The present invention provides a drop ball impact test method for lightweight physical and chemical glass in a heated state. By performing multiple drop ball impact tests on several positions of the lightweight physical and chemical glass after being heated under a temperature program, the comprehensive test conditions of a single piece of glass in a heated and high-temperature state, multiple impacts, and multiple height impacts at multiple positions are achieved. The method maximizes the simulation of severe weather conditions such as hail or sandstorms (Gobi Desert) when hot spots appear on the lightweight physical and chemical glass in photovoltaic modules. First, it helps to comprehensively evaluate the performance of glass under different impact conditions. Second, it provides temperature conditions when hot spots occur in modules. By comprehensively evaluating the performance of photovoltaic modules under the dual effects of hot spot effect and physical impact, the problem that traditional test methods cannot truly reflect the performance of modules in actual working environments is solved.

[0034] The falling ball impact method provided by the present invention has the advantages of simple operation and rapid and accurate evaluation;

[0035] And the reliability and stability of the lightweight physical and chemical glass in the photovoltaic module in actual application are evaluated according to the results of the impact test method of the present invention, and the evaluation result is reliable.

[0036] Other features and advantages of the present invention will be described in the following description, and partly become apparent from the description, or understood by practicing the present invention. The purpose and other advantages of the present invention can be realized and obtained by the structures pointed out in the description, claims and drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0038] Figure 1 A flow chart showing a method for testing a falling ball impact of lightweight physical and chemical glass in a heated state according to an embodiment of the present invention is shown;

[0039] Figure 2 shows a temperature program diagram according to an embodiment of the present invention;

[0040] Figure 3 A schematic diagram showing a test position in a front plate lightweight physical and chemical glass according to an embodiment of the present invention;

[0041] Figure 4 A schematic diagram showing the test positions in the back panel lightweight physical and chemical glass according to an embodiment of the present invention. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] like Figure 1 As shown, a drop ball impact test method for lightweight physical and chemical glass in a heated state according to an embodiment of the present invention comprises:

[0044] Step 1: Set the temperature program for the heating stage, constant temperature stage, test stage and cooling stage;

[0045] Step 2: At the beginning of the test phase, a drop ball impact test is performed on several test positions on the light surface of the lightweight physical and chemical glass at intervals;

[0046] Step 3: When the cooling stage begins, the interval drop ball impact test ends.

[0047] In the temperature program of step 1, the heating rate of the heating stage is 7-10°C / min, the holding time of the constant temperature stage is 15-25min, the temperature of the test stage is 190-210°C, the test time of the test stage is 10-15min, and the cooling rate of the cooling stage is 13-18°C / min. In the embodiment of the present invention, for example, the temperature program is as follows Figure 2 As shown, in this embodiment, the heating rate of the heating stage is 8°C / min, the temperature of the test stage is 200°C, the insulation time of the constant temperature stage is 20min, the test time of the test stage is 10min, and the cooling rate of the cooling stage is 15°C / min.

[0048] The lightweight glass in the photovoltaic module is a rectangular glass plate, including a long side and a short side. The lightweight glass includes a front panel lightweight glass and a back panel lightweight glass. The front panel lightweight glass includes an embossed surface and a smooth surface (the smooth surface is a coated surface). The embossed surface is used as a contact surface with one side of the photovoltaic module, and the smooth surface of the front panel lightweight glass is in contact with the air; the back panel lightweight glass includes a glazed surface and a smooth surface. The glazed surface (a grid is printed on this surface) is used as a contact surface with the other side of the photovoltaic module.

[0049] When assembling solar cells, the glazed surface of the lightweight physical and chemical glass on the back panel is bonded to one side of the double-sided cell sheet through the adhesive film in the photovoltaic module, and the other side of the double-sided cell sheet is bonded to the embossed surface of the lightweight physical and chemical glass on the front panel through the adhesive film to assemble into a solar cell.

[0050] Therefore, in step 2 of the embodiment of the present invention, the design of several test positions needs to fully consider the difference between the front plate and the back plate in the lightweight physical and chemical glass in the photovoltaic module. The difference between the two is that the front plate is more susceptible to outdoor hot spots due to direct contact with sunlight, and the back plate lightweight physical and chemical glass needs to be punched for the connection of the battery cell and the junction box in the photovoltaic module. The glass sheet within the area of ​​the hole also needs to be tested. Therefore, in the embodiment of the present invention, several of the test positions are designed as follows:

[0051] When the lightweight physical and chemical glass is a front plate lightweight physical and chemical glass, the test positions include a first position, a second position and a third position;

[0052] The first position is distributed within 25 mm of the center position of the light surface of the front panel lightweight physical and chemical glass;

[0053] The second position is distributed within a range of 25 mm from the intersection of a tangent line of 1 / 4 of a long side and a midline of a short side in the front plate lightweight physical and chemical glass;

[0054] The third position is distributed within 10mm of the center position of the corner battery half-piece of the front panel lightweight physical and chemical glass;

[0055] The second position and the third position are located on both sides of the midline of the long side of the lightweight physical and chemical glass of the front panel;

[0056] In an embodiment of the present invention, the first position is Figure 3 The position marked in 1, the second position is as Figure 3 The position marked by 2, the third position is as follows Figure 3 At the position marked with 3, Figure 3 The area enclosed by the dotted line and rectangular edges represents the corner cell half-cell.

[0057] In step 2, when the lightweight physical and chemical glass is a back panel lightweight physical and chemical glass, the test positions include a fourth position and a fifth position;

[0058] The fourth position is distributed within a 10mm range between any two holes on the light surface of the back panel lightweight physical and chemical glass;

[0059] The fifth position is distributed within a range of 5 mm from the intersection of a tangent line of 1 / 4 of a long side of the back panel lightweight physical and chemical glass and a midline of a short side;

[0060] In the embodiment of the present invention, illustratively, the fourth position is as follows Figure 4 The position marked by 4, the fifth position is as Figure 4 The position marked by 5, wherein the fourth position can also be Figure 4 The other two holes mark the positions of Figure 4 There are 3 holes in it (the holes are designed to facilitate the connection between the battery cell and the junction box in the photovoltaic module), and the holes are located at the intersection of the 1 / 6 line, 3 / 6 line, 5 / 6 line of the short side and the midline of the long side.

[0061] Step two, in the interval drop ball impact test, the drop ball height at the first position is 1±0.05m; the drop ball height at the second position is 0.7±0.05m; the drop ball height at the third position is 0.5±0.05m, the drop ball height at the fourth position is 0.5±0.05m; the drop ball height at the fifth position is 0.7±0.05m.

[0062] Step 2: In the interval drop ball impact test, the interval time is 2-3 minutes.

[0063] Step 2: The mass of the steel ball used in the interval drop ball impact test is 227±2g.

[0064] In some embodiments of the present invention, the falling ball impact test method further includes:

[0065] The reliability of the lightweight physical and chemical glass as the lightweight physical and chemical glass in the photovoltaic module is judged based on the results of the several interval drop ball impact tests.

[0066] Example 1

[0067] The reliability of the lightweight physical and chemical glass in the photovoltaic module is evaluated according to the method provided in the above embodiment:

[0068] Sample preparation: Take the finished product as the sample, randomly select 3 pieces of front panel lightweight physical and chemical glass and 3 pieces of back panel lightweight physical and chemical glass, among which each piece of back panel glass is impacted at 2 positions; each piece of front panel glass is impacted at 3 positions.

[0069] Test equipment (temperature control device): The equipment has a temperature control program that can achieve a temperature condition of 200±5℃. At the same time, the equipment is equipped with a refrigeration and cooling system. After completing a test, the temperature is quickly reduced through the refrigeration system. Four holes are set on the top of the equipment corresponding to the glass impact point. The holes are set with steel pipes for steel balls. The height of the steel pipe can be adjusted at will according to the height of the falling ball, and the opening and closing of the bottom cover of the steel pipe can be controlled by the device button.

[0070] The bracket is a steel bracket with a steel frame height of 150mm. Two 600mm*600mm steel support frames are placed in the length direction of the glass. The outer sides of the steel brackets are 100mm away from the edge of the glass. Two 600mm*200mm steel support frames are placed in the width direction. The outer sides of the steel brackets are 100mm away from the edge of the glass. The contact surface between the steel frame and the glass is lined with a high temperature resistant 250°C silicone rubber pad with a thickness of 3mm, a width of 10mm and a hardness of Shore A50.

[0071] Among them, the temperature control program in the temperature control device and the refrigeration and cooling system are common knowledge in the technical field, and the embodiments of the present invention will not be repeated here; at the same time, the control of opening and closing the bottom cover of the steel pipe is well known in the technical field, and the embodiments of the present invention will not be repeated here.

[0072] Testing process:

[0073] 1) Front panel lightweight physical and chemical glass drop ball impact test

[0074] a. Place the front glass sample on the steel bracket inside the equipment box, with the glossy surface of the front glass sample facing upward (front side facing downward), and the outer side of the steel bracket 100 mm away from the edge of the glass.

[0075] b. Place three steel balls with a mass of 227±2g in the steel tubes respectively, and the steel tubes are placed directly above the three positions of the impact glass. Among them, position 1 is within 25㎜ of the center position of the light surface of the front panel lightweight physical and chemical glass, position 2 is within 25㎜ of the intersection position of the tangent line of 1 / 4 of a long side of the front panel lightweight physical and chemical glass and the midline of the short side, and position 3 is the third position distributed within 10㎜ of the center position of the corner battery half of the front panel lightweight physical and chemical glass; the second position and the third position are located on both sides of the midline of the long side of the front panel lightweight physical and chemical glass. Then adjust the height of the steel tube, and the height of the bottom of the three steel tubes from the glass surface are: the drop height of the test position 1 is 1m, the drop height of the test position 2 is 0.7m, and the drop height of the test position 3 is 0.5m.

[0076] c. Turn on the power of the equipment, click the temperature program to run, the temperature reaches 200℃ within 25 minutes, keep the temperature constant for 30 minutes, turn on the drop ball impact button of test position 1, test position 2, and test position 3 respectively, and the interval between each impact is 2-3 minutes. After the impact is completed, the equipment will cool to room temperature within 20 minutes and take out the glass.

[0077] d. After testing the three front glass panels, turn off the power of the device.

[0078] 2) Back panel lightweight physical and chemical glass drop ball impact test

[0079] a. Place the back glass sample on the steel bracket inside the equipment box, with the glossy surface of the back glass sample facing upward (glazed surface facing downward), and the outer side of the steel bracket 100 mm away from the edge of the glass.

[0080] b. Place two steel balls with a mass of 227±2g in the steel tubes respectively, and the steel tubes are placed directly above the two positions of the impact glass. Among them, test position 1 is within 10mm of the middle position of the two holes on the smooth surface, and test position 2 is within 5mm of the intersection of the tangent of 1 / 4 of the long side and the midline of the short side (that is, within 5mm of the grid point of the intersection of the tangent of 1 / 4 of the long side and the midline of the short side). Then adjust the height of the steel tubes, and the height of the bottom of the two steel tubes from the glass surface is: the drop height of the ball at test position 1 is 0.5m, and the drop height of the ball at test position 2 is 0.7m.

[0081] c. Turn on the power of the equipment, click the temperature program to run, the temperature reaches 200℃ within 25 minutes, keep the temperature constant for 30 minutes, turn on the drop ball impact button of test position 1 and test position 2 respectively, and the interval between each impact is 2-3 minutes. After the impact is completed, the equipment will cool to room temperature within 20 minutes and take out the glass.

[0082] d. After testing the three back glass panels, turn off the power of the device.

[0083] The reliability of lightweight physical and chemical glass as lightweight physical and chemical glass in photovoltaic modules is judged based on the test results of the above three front panels, specifically, including the following situations:

[0084] If the three front panel samples are intact and not broken, the batch of front panel samples is judged to be lightweight physical and chemical glass with high reliability in photovoltaic modules, and the batch of front panel samples is judged to be qualified;

[0085] If two of the three front panel samples are broken, the reliability of the batch of front panel samples is judged to be low for the lightweight physical and chemical glass in the photovoltaic module, and the batch of front panels is judged to be unqualified;

[0086] If one of the three front panel samples is broken, in order to improve the accuracy of judgment, three more front panel samples are taken for re-interval drop ball impact test. If the three additional front panel samples are all intact, it is judged that the batch of front panel samples is of medium reliability of lightweight physical and chemical glass in photovoltaic modules, and the batch of front panel samples is qualified; if one of the three additional front panel samples is broken, it is judged that the batch of front panel samples is of low reliability of lightweight physical and chemical glass in photovoltaic modules, and the batch of front panels is unqualified.

[0087] Judging the reliability of the lightweight physical and chemical glass as the lightweight physical and chemical glass in the photovoltaic module based on the test results of the above three back panels is equivalent to the judgment process of the above front panel, and will not be repeated in this embodiment of the present invention.

[0088] The embodiment of the present invention only exemplarily shows the process of "judging the reliability of lightweight physical and chemical glass as lightweight physical and chemical glass in photovoltaic modules based on the results of the several times of interval drop ball impact tests", where the several times is 3 times, and the present invention does not make any specific limitation on this number. At the same time, the judgment of the reliability level can also be flexibly set according to the specific results of the several times of interval drop ball impact tests, and the present invention does not make any specific limitation on it.

[0089] Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent substitutions for some of the technical features therein; and these modifications or substitutions do not make the essence of the corresponding technical solutions deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A drop ball impact test method for lightweight physical and chemical glass in a heated state, characterized in that: include: Set the temperature program for heating stage, constant temperature stage, test stage and cooling stage; At the beginning of the test phase, a spaced drop ball impact test is performed simultaneously on a plurality of test locations on the light surface of the lightweight physical and chemical glass; When the cooling phase begins, the interval drop ball impact test ends.

2. The method for testing the falling ball impact of lightweight physical and chemical glass in a heated state according to claim 1, characterized in that: When the lightweight physical and chemical glass is a front plate lightweight physical and chemical glass, the test positions include a first position, a second position and a third position; The first position is distributed within 25 mm of the center position of the light surface of the front panel lightweight physical and chemical glass; The second position is distributed within a range of 25 mm from the intersection of a tangent line of 1 / 4 of a long side and a midline of a short side in the front plate lightweight physical and chemical glass; The third position is distributed within 10mm of the center position of the corner battery half-piece of the front panel lightweight physical and chemical glass; The second position and the third position are located on both sides of the midline of the long side of the lightweight physical and chemical glass of the front plate.

3. The method for testing the falling ball impact of lightweight physical and chemical glass in a heated state according to claim 2, characterized in that: The height of the ball falling at the first position is 1±0.05m; The ball drop height at the second position is 0.7±0.05m; The ball falling height at the third position is 0.5±0.05m.

4. The method for testing the falling ball impact of lightweight physical and chemical glass in a heated state according to claim 1, characterized in that: When the lightweight physical and chemical glass is a back panel lightweight physical and chemical glass, the test positions include a fourth position and a fifth position; The fourth position is distributed within a 10mm range between any two holes on the light surface of the back panel lightweight physical and chemical glass; The fifth position is distributed within a range of 5 mm from the intersection of a tangent line of 1 / 4 of a long side of the back panel lightweight physical and chemical glass and a midline of a short side.

5. The method for testing the falling ball impact of lightweight physical and chemical glass in a heated state according to claim 4, characterized in that: The ball falling height at the fourth position is 0.5±0.05m; the ball falling height at the fifth position is 0.7±0.05m.

6. The method for testing the falling ball impact of lightweight physical and chemical glass in a heated state according to claim 1, characterized in that: In the interval drop ball impact test, the interval time is 2-3 minutes.

7. The method for testing the falling ball impact of lightweight physical and chemical glass in a heated state according to claim 1, characterized in that: The heating rate in the heating stage is 7-10°C / min, and the insulation time in the constant temperature stage is 15-25min.

8. The method for testing the falling ball impact of lightweight physical and chemical glass in a heated state according to claim 1, characterized in that: The temperature of the test stage is 190-210° C., the test time of the test stage is 10-15 min, the cooling rate of the cooling stage is 13-18° C. / min; the mass of the steel ball used in the ball impact test is 227±2 g.

9. A drop ball impact test method for lightweight physical and chemical glass in a heated state according to claims 1-8, characterized in that: Also includes: The reliability of the lightweight physical and chemical glass as the lightweight physical and chemical glass in the photovoltaic module is judged based on the results of several interval drop ball impact tests.

10. A falling ball impact test device for lightweight physical and chemical glass in a heated state, characterized in that: include: Temperature control device: used to set the temperature program of heating stage, constant temperature stage, test stage and cooling stage; also used to end the interval drop ball impact test at the beginning of the cooling stage Drop ball steel tube: used to perform interval drop ball impact tests on several test positions on the smooth surface of lightweight physical and chemical glass at the beginning of the test phase; Several brackets: used to support lightweight physical and chemical glass; The ball-dropping steel pipe is embedded in a hole arranged on a side wall of the temperature control device, and a plurality of the brackets are placed in the temperature control device.