Method for detecting internal defects of composite material carbon felt-carbon fiber bonding structure
Through the delay law and multi-sound beam processing technology of phased array ultrasonic system, the simultaneous detection of layered defects and debonding defects of composite carbon felt-carbon fiber adhesive structures is achieved, and multiple scans and inspections in the prior art are solved. The problem of defect missed detection provides flexible detection methods and quantitative characterization capabilities.
Patent Information
- Application Number
- CN202411217659.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-11-12
AI Technical Summary
The existing ultrasonic detection technology is difficult to simultaneously detect layered defects and debonding defects in the composite carbon felt-carbon fiber adhesive structure, especially when the inclination angle changes of the carbon felt-carbon fiber prepreg adhesive interface, it is necessary to perform multiple times. Scan and replace the acoustic inclined wedge block, resulting in an increased risk of defect missed detection.
The detection method based on phased array ultrasonic system is adopted to realize the deflection of the ultrasonic sound beam through the delay law, and two groups of sound beams at different angles are stimulated simultaneously, so as to detect stratified defects and debonded defects in one scan, and adapt to a certain inclination range. Carbon felt-carbon fiber prepreg adhesive interface.
It realizes convenient, intuitive and visual inspection of composite carbon felt-carbon fiber adhesive structures, avoids multiple detections and defect missed detection, and can flexibly adapt to structures at different angles for qualitative and quantitative characterization.
Smart Images

Figure CN118937490A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nondestructive testing, and in particular to a method for detecting internal defects of a composite material carbon felt-carbon fiber adhesive bonding structure. Background Art
[0002] In order to meet the use and maintenance requirements of aircraft, composite panels are usually provided with openings of different shapes and sizes. In order to avoid stress concentration at the openings and thus reduce the structural strength, the panel openings must be reinforced. The commonly used method of intercalation reinforcement is used in engineering, and the following methods are used: Figure 1 The triangular cross-section carbon felt-inserted carbon fiber prepreg bonding structure shown ensures structural integrity and structural rigidity. The design requires non-destructive testing of the structure to detect delamination defects between carbon fiber prepreg plies and debonding defects between carbon felt and prepreg.
[0003] When using ultrasonic testing technology to detect parts, the main consideration is the location and orientation of the defects to be detected. The principle of selection is to obtain the maximum possible display of defects. "Shi Yiwei et al., "Ultrasonic Testing", Machinery Industry Press, Section 3.3 "Direct Beam Method and Oblique Beam Method." In engineering, the vertical incidence method of ultrasonic longitudinal waves is often used to detect composite parts. The delamination defects are distributed along the prepreg plies, and their main reflection surface is perpendicular to the axis of the ultrasonic beam. The defect echo amplitude received by the probe is the largest, and the defect display is the most obvious. The bonding interface of carbon felt-carbon fiber prepreg has a certain inclination angle. The main reflection surface of the debonding defect is not perpendicular to the axis of the ultrasonic beam. When the inclination angle reaches a certain angle, the probe cannot receive the defect echo or the echo signal is very weak, which can easily cause the debonding defect to be missed.
[0004] "Shi Yiwei et al., Ultrasonic Testing, Machinery Industry Press, Section 3.3.2 "Oblique Beam Method"" Installing a sound-transmitting oblique wedge at the front end of the ultrasonic probe can make the ultrasonic beam enter the carbon felt-carbon fiber prepreg bonding interface at a certain inclination angle, thereby obtaining the maximum display of debonding defects. However, the disadvantages of this method are: 1) The parts need to be scanned twice at vertical incidence and oblique incidence to detect delamination defects and debonding defects; 2) When the angle of the carbon felt-carbon fiber prepreg bonding interface changes, the oblique wedge needs to be replaced to change the incident angle of the sound beam. A composite wall panel often has multiple carbon felt-carbon fiber prepreg bonding structures, and their inclination angles are inconsistent.
[0005] In order to solve the above problems, the present invention proposes a detection method based on a phased array ultrasonic system, which realizes the deflection of the ultrasonic sound beam through the delay law, and simultaneously excites two sets of sound beams at different angles, so that detection can be achieved with one scan. Figure 1 The delamination defect and debonding defect of the structure can be eliminated, and it can adapt to the bonding interface of carbon felt-carbon fiber prepreg within a certain inclination range, without the need to carry and replace a large number of sound-transmitting oblique wedges. Summary of the invention
[0006] The present invention mainly solves the problem of detecting internal defects of the reinforcement structure at the opening of composite material wall panel parts, proposes a convenient, intuitive and visual detection method, and adopts ultrasonic beam processing technology combined with multiple methods in a fully digital phased array ultrasonic imaging system.
[0007] The technical solution of the present invention is as follows: a method for detecting internal defects of a composite carbon felt-carbon fiber bonding structure, which realizes the deflection of an ultrasonic sound beam through a delay law, and simultaneously excites two groups of sound beams at different angles, so as to realize a single scan to detect the delamination defects and debonding defects of a bonding structure of a triangular cross-section carbon felt-intercalated carbon fiber prepreg.
[0008] The method for detecting internal defects of the composite material carbon felt-carbon fiber adhesive bonding structure specifically comprises the following steps:
[0009] Step 1: Set the parameters related to the focal law;
[0010] Step 2: Set imaging display related parameters;
[0011] Step 3: Qualitative and quantitative analysis of defects.
[0012] The parameters related to setting the focal law are specifically:
[0013] Phased array ultrasonic technology is used, two groups of delayed focusing laws are set, and two groups of sound beams are detected simultaneously. The first group is a linear sound beam 6 with a deflection of 0°, and the second group is a linear sound beam 7 with a deflection angle of θ; there are delamination defects 8 between carbon fiber prepreg plies, and there are debonding defects 9 at the bonding interface of carbon felt-carbon fiber prepreg; the θ of the linear sound beam 7 with a deflection angle of θ meets equations 1) to 2);
[0014]
[0015] θ=θ0 2)
[0016] Among them, λ is the longitudinal wave wavelength of the ultrasonic wave in the part, and e is the width of a single chip in the phased array probe.
[0017] The imaging display related parameters are specifically set as follows:
[0018] Set the display mode to L view. The L views corresponding to the two sets of linear beams are recorded as L0 and L θ ; The horizontal axis of the L view is the linear acoustic beam electronic scanning sequence L N , the vertical axis is the signal depth, where N = 1, 2, 3...N max , N max is the maximum beam sequence of a linear beam.
[0019] The imaging shows the following:
[0020] The linear sound beam 6 incident at 0° is incident perpendicularly to the carbon fiber prepreg structure, and the propagation direction of the sound beam is perpendicular to the carbon fiber prepreg ply. When there is no delamination defect inside the carbon fiber prepreg, the sound beam propagates inside the carbon fiber prepreg to the bottom surface, is reflected on the bottom surface, and the reflected sound beam is received by the probe. When there is a delamination defect 8 between the layers inside the carbon fiber prepreg, at the delamination defect-prepreg ply interface, the sound energy is almost completely reflected, and the reflected sound beam is received by the probe 4.
[0021] The linear sound beam 7 with a deflection angle of θ° is perpendicular to the carbon felt 2 structure, and the propagation direction of the sound beam is perpendicular to the carbon felt 2; when there is no debonding defect 9 at the carbon felt-carbon fiber prepreg bonding interface, the amplitude of the reflected signal of the sound beam at the interface is low, most of the sound energy is transmitted into the carbon felt 2 and continues to propagate, and the probe does not receive an obvious reflected signal; when there is a debonding defect 9 at the bonding interface, the sound energy of the sound beam at the defect is almost completely reflected and the reflected sound beam is received by the probe.
[0022] The third step is specifically as follows: judging whether there is a delamination defect 8 by a linear sound beam 6 with an incident angle of 0°; judging whether there is a debonding defect 9 by a linear sound beam 7 with a deflection angle of θ°; obtaining an ultrasonic signal in the time domain range of the linear array phased array probe 4, with the aid of the fixed position relationship of each chip in the probe, and based on the time delay focusing law, obtaining the sound beam sequence and spatial correspondence of the linear sound beam 6 with an incident angle of 0° and the linear sound beam 7 with a deflection angle of θ°, and quantifying the defects accordingly.
[0023] The linear acoustic beam 6 incident at 0°: when the depth of the time domain signal received by the probe 4 is equivalent to the thickness of the carbon fiber prepreg ply 1, there is no defect; when the depth of the time domain signal is different from the thickness of the carbon fiber prepreg ply 1, there is a delamination defect 8.
[0024] The linear acoustic beam 7 with the deflection angle θ°: when the probe 4 cannot receive the ultrasonic signal, there is no defect; when the probe 4 receives the ultrasonic signal, there is a debonding defect 9.
[0025] The defect quantification is specifically as follows:
[0026] The width of the delamination defect is:
[0027] L 分 =L0 2 -L0 1 3)
[0028] Among them, L0 1 , L0 2 It is the acoustic beam electronic scanning sequence corresponding to the two ends of the delamination defect in the L0 view;
[0029] The depth of the delamination defect is:
[0030] H 分 =(H0 1 +H0 2 )÷2 4)
[0031] Among them, H0 1 、H0 2 L0 1 and L0 2 Depth of defect signal in ;
[0032] The width of the debonding defect is:
[0033]
[0034] Among them, L θ 1 , L θ 2 YesL θ The electronic scanning sequence of the acoustic beam corresponding to the two ends of the debonding defect in the view;
[0035] The depth of the debonding defect is:
[0036] H 脱 =H θ 1 +(H θ 1 +H θ 2 )÷2 6)
[0037] Among them, H θ 1 , H θ 2 L θ 1 and L θ 2 The depth of defect signal in .
[0038] Beneficial effects of the present invention:
[0039] 1) The present invention proposes a method for detecting internal defects of a composite carbon felt-carbon fiber adhesive structure, which uses a phased array multi-beam ultrasonic detection method to achieve simultaneous visual detection of debonding defects and prepreg delamination defects of a carbon felt-carbon fiber prepreg structure, thereby avoiding multiple detections and preventing defects from being missed;
[0040] 2) The deflection angle of the phased array linear acoustic beam can be flexibly set to adapt to carbon felt-carbon fiber prepreg parts with a certain inclination range;
[0041] 3) The delamination defects between carbon fiber prepreg plies and the debonding defects at the carbon felt-carbon fiber prepreg bonding interface can be qualitatively and quantitatively characterized to facilitate part acceptance / rejection. BRIEF DESCRIPTION OF THE DRAWINGS
[0042] Figure 1 It is a bonding structure of triangular cross-section carbon felt-intercalated carbon fiber prepreg.
[0043] 1 is the carbon fiber prepreg ply, 2 is the carbon felt, 3 is the bonding interface angle of carbon felt-carbon fiber prepreg, 4 is the linear array phased array probe, and 5 is the opposite side of the carbon felt. 6 is the linear sound beam with 0° incidence, and 7 is the linear sound beam with a deflection angle of θ°. 8 is the delamination defect, and 9 is the debonding defect. DETAILED DESCRIPTION
[0044] The innovation of the present invention lies in: 1) using phased array electronic scanning to form a deflected ultrasonic sound beam with oblique incidence at a certain angle, the propagation direction of the deflected ultrasonic sound beam is perpendicular to the bonding interface, and is used to detect the debonding defects of the carbon felt-carbon fiber prepreg structure; 2) the deflection angle can be flexibly set to adapt to a certain inclination range of part structures; 3) 2 groups of different ultrasonic sound beams are excited at the same time, and the debonding defect detection of non-parallel surfaces and the delamination defect detection of parallel surfaces in the structure are realized at the same time; 4) the two types of defects can be located and quantitatively characterized.
[0045] Carbon felt-carbon fiber prepreg bonding structure Figure 1 As shown, it includes a carbon fiber prepreg ply 1, a carbon felt 2, a carbon felt-carbon fiber prepreg bonding interface angle 3 of θ0, and a linear array phased array probe 4 is placed at a position 5 on the opposite side of the carbon felt 2.
[0046] Step 1: Set the focal law parameters
[0047] Phased array ultrasonic technology is used to set two groups of delayed focusing laws to achieve simultaneous detection of two groups of sound beams. The first group is a linear sound beam 6 with a deflection angle of 0°, and the second group is a linear sound beam 7 with a deflection angle of θ. There are delamination defects 8 between carbon fiber prepreg plies, and there are debonding defects 9 at the bonding interface of carbon felt-carbon fiber prepreg. The θ of the linear sound beam (7) with a deflection angle of θ meets formulas (1) to (2).
[0048]
[0049] θ=θ0 Formula (2)
[0050] Where λ is the longitudinal wavelength of the ultrasonic wave in the part, and e is the width of a single element in the phased array probe.
[0051] Step 2: Set imaging display related parameters
[0052] Set the display mode to L view. The L views corresponding to the two sets of linear beams are recorded as L0 and L θ The horizontal axis of the L view is the linear acoustic beam electronic scanning sequence L N, the vertical axis is the signal depth (measured by part depth), where N = 1, 2, 3...N max , N max is the maximum beam sequence of a linear beam.
[0053] Detection principle:
[0054] The linear sound beam 6 incident at 0° is incident perpendicularly to the carbon fiber prepreg structure, and the propagation direction of the sound beam is perpendicular to the carbon fiber prepreg ply. When there is no delamination defect inside the prepreg, the sound beam propagates inside the prepreg to the bottom surface, reflects on the bottom surface, and the reflected sound beam is received by the probe; when there is a delamination defect 8 between the layers inside the prepreg, due to the large difference in acoustic impedance between the delamination defect 8 and the carbon fiber prepreg ply 1, at the delamination defect-prepreg ply interface, the sound energy is almost completely reflected and the reflected sound beam is received by the linear array phased array probe 4.
[0055] The linear sound beam 7 with a deflection angle of θ° vertically enters the carbon felt 2 structure, and the propagation direction of the sound beam is perpendicular to the carbon felt 2. When there is no debonding defect 9 at the carbon felt-carbon fiber prepreg bonding interface, since the difference in acoustic impedance between the carbon felt 2 and the carbon fiber prepreg ply 1 is small, the amplitude of the reflected signal of the sound beam at the interface is low, and most of the sound energy is transmitted into the carbon felt 2 and continues to propagate, and the probe does not receive an obvious reflected signal; when there is a debonding defect 9 at the bonding interface, the acoustic impedance of the debonding defect 9 is significantly different from that of the carbon fiber prepreg ply 1, and the acoustic energy of the sound beam at the defect is almost completely reflected and the reflected sound beam is received by the probe.
[0056] Step 3: Defect qualitative and quantitative methods
[0057] Linear acoustic beam 6 with 0° incidence: When the depth of the time domain signal received by the linear array phased array probe 4 is equivalent to the thickness of the carbon fiber prepreg ply 1, there is no defect; when the depth of the time domain signal is different from the thickness of the carbon fiber prepreg ply 1, there is a delamination defect 8.
[0058] Linear acoustic beam 7 with a deflection angle of θ°: when the linear array phased array probe 4 cannot receive the ultrasonic signal, there is no defect; when the linear array phased array probe 4 receives the ultrasonic signal, there is a debonding defect 9.
[0059] Based on the ultrasonic signal in the time domain obtained by the linear array phased array probe 4, with the help of the fixed position relationship of each chip in the probe, based on the time delay focusing law, the beam sequence and spatial correspondence of the linear sound beam 6 with 0° incidence and the linear sound beam 7 with a deflection angle of θ° are obtained, and the defect quantification is performed accordingly according to formulas 3 to 6.
[0060] The width of the delamination defect is: L 分 =L0 2 -L0 1 3)
[0061] Among them, L0 1 , L0 2 It is the acoustic beam electronic scanning sequence corresponding to the two ends of the delamination defect in the L0 view;
[0062] The depth of the delamination defect is: H 分 =(H0 1 +H0 2 )÷2 4)
[0063] Among them, H0 1 、H0 2 L0 1 and L0 2 Depth of defect signal in ;
[0064] The width of the debonding defect is:
[0065] Among them, L θ 1 , L θ 2 YesL θ The electronic scanning sequence of the acoustic beam corresponding to the two ends of the debonding defect in the view;
[0066] The depth of the debonding defect is: H 脱 =H θ 1 +(H θ 1 +H θ 2 )÷2 6)
[0067] Among them, H θ 1 , H θ 2 L θ 1 and L θ 2 The depth of defect signal in .
[0068] A 5MHz, 64-crystal linear array phased array probe was used to detect the outer wing wall panel of a carbon fiber composite material. The opening of the wall panel was reinforced and supplemented with a carbon felt structure. The angle between the carbon felt and the carbon fiber laminate was 20°, and the thickness of the carbon fiber laminate was 20mm. It was required to detect the Φ5mm delamination defect within the depth range of 2-3 layers on the upper surface of the carbon fiber laminate to 2-3 layers on the lower surface, and the Φ6mm debonding defect at the bonding interface of the carbon felt-carbon fiber laminate.
[0069] The focal law for phased array ultrasonic testing is set as:
[0070] The first group of sound beams: 30 chips are excited at one time, the deflection angle is 0°, and the electronic linear scanning of the synthetic sound beam is performed. The electronic linear scanning step is 2 chips, and the focusing depth is 20mm of the sound path.
[0071] The second group of sound beams: 30 chips are excited at one time, the deflection angle is 20°, and the electronic linear scanning of the synthetic sound beam is performed. The electronic linear scanning step is 2 chips, and the focusing depth is 30mm of the sound path.
[0072] Two sets of sound beams are excited simultaneously, and the part is electronically scanned linearly at the same time.
[0073] like Figure 1 As shown, the probe is placed on the opposite side of the carbon felt triangle structure. The first group of linear sound beams with a deflection angle of 0° is perpendicular to the bottom surface of the edge of the wall panel opening, which is used to detect the delamination defects between the carbon fiber prepreg plies; the second group of linear sound beams with a deflection angle of 20° are obliquely incident, perpendicular to the carbon felt-carbon fiber prepreg bonding interface, and are used to detect the debonding defects in the carbon felt-carbon fiber prepreg bonding interface.
[0074] Open the L-scan view of the two groups of acoustic beams, observe the ultrasonic imaging display, and quantitatively and positionally characterize the delamination defects and debonding defects according to formulas (3) to (6).
[0075] Application results show that this method can intuitively discover two defects at different angles - the delamination defect between carbon fiber prepreg plies and the debonding defect at the bonding interface of carbon felt-carbon fiber prepreg, and can quantify and determine the depth of the defects.
Claims
1. A method for detecting internal defects of a composite material carbon felt-carbon fiber bonding structure, characterized in that: The ultrasonic beam is deflected by the delay law, and two groups of beams at different angles are excited simultaneously, so that the delamination defects and debonding defects of the bonding structure of triangular cross-section carbon felt-intercalated carbon fiber prepreg can be detected in one scan.
2. The method for detecting internal defects of a composite material carbon felt-carbon fiber adhesive bonding structure according to claim 1, characterized in that: The specific steps are as follows: Step 1: Set the parameters related to the focal law; Step 2: Set imaging display related parameters; Step 3: Qualitative and quantitative analysis of defects.
3. The method for detecting internal defects of a composite material carbon felt-carbon fiber adhesive bonding structure according to claim 2, characterized in that: The parameters related to setting the focal law are specifically: Phased array ultrasonic technology is used, two groups of delayed focusing laws are set, and two groups of sound beams are detected simultaneously, the first group is a linear sound beam with a deflection angle of 0° (6), and the second group is a linear sound beam with a deflection angle of θ (7); there are delamination defects (8) between carbon fiber prepreg plies, and there are debonding defects (9) at the bonding interface of carbon felt-carbon fiber prepreg; θ of the linear sound beam with a deflection angle of θ (7) meets equations 1) to 2); θ=θ0 2) Among them, λ is the longitudinal wave wavelength of the ultrasonic wave in the part, and e is the width of a single chip in the phased array probe.
4. The method for detecting internal defects of a composite material carbon felt-carbon fiber adhesive structure according to claim 2, characterized in that: The imaging display related parameters are specifically set as follows: Set the display mode to L view. The L views corresponding to the two sets of linear beams are recorded as L0 and L θ ; The horizontal axis of the L view is the linear acoustic beam electronic scanning sequence L N , the vertical axis is the signal depth, where N = 1, 2, 3...N max , N max is the maximum beam sequence of a linear beam.
5. The method for detecting internal defects of a composite material carbon felt-carbon fiber adhesive bonding structure according to claim 4, characterized in that: The imaging shows the following: A linear acoustic beam (6) incident at 0° is incident perpendicularly on the carbon fiber prepreg structure, and the propagation direction of the acoustic beam is perpendicular to the carbon fiber prepreg ply; when there is no delamination defect inside the carbon fiber prepreg, the acoustic beam propagates inside the carbon fiber prepreg to the bottom surface, is reflected on the bottom surface, and the reflected acoustic beam is received by the probe; when there is a delamination defect (8) between layers inside the carbon fiber prepreg, at the delamination defect-prepreg ply interface, the acoustic energy is almost completely reflected, and the reflected acoustic beam is received by the linear array phased array probe (4); A linear sound beam (7) with a deflection angle of θ° is incident perpendicularly on the carbon felt (2) structure, and the propagation direction of the sound beam is perpendicular to the carbon felt (2); when there is no debonding defect (9) at the bonding interface between the carbon felt and the carbon fiber prepreg, the amplitude of the reflected signal of the sound beam at the interface is low, and most of the sound energy is transmitted into the carbon felt (2) and continues to propagate, and the probe does not receive an obvious reflected signal; when there is a debonding defect (9) at the bonding interface, the sound energy of the sound beam at the defect is almost completely reflected and the reflected sound beam is received by the probe.
6. The method for detecting internal defects of a composite material carbon felt-carbon fiber adhesive bonding structure according to claim 2, characterized in that: The third step specifically comprises: judging whether a delamination defect (8) exists through a linear sound beam (6) with an incidence of 0°; judging whether a debonding defect (9) exists through a linear sound beam (7) with a deflection angle of θ°; obtaining a sound beam sequence and a spatial correspondence between the linear sound beam (6) with an incidence of 0° and the linear sound beam (7) with a deflection angle of θ° and the spatial correspondence based on the ultrasonic signal in the time domain range obtained by the linear array phased array probe (4) with the aid of the fixed position relationship of each chip in the probe and the time-delay focusing law, and performing defect quantification accordingly.
7. The method for detecting internal defects of a composite material carbon felt-carbon fiber adhesive structure according to claim 6, characterized in that: The linear acoustic beam (6) incident at 0°: when the depth of the time domain signal received by the linear array phased array probe (4) is equal to the thickness of the carbon fiber prepreg ply (1), there is no defect; when the depth of the time domain signal is different from the thickness of the carbon fiber prepreg ply (1), there is a delamination defect (8).
8. The method for detecting internal defects of a composite material carbon felt-carbon fiber adhesive structure according to claim 6, characterized in that: The linear sound beam (7) with a deflection angle of θ° has no defect when the linear array phased array probe (4) cannot receive an ultrasonic signal; and has a debonding defect (9) when the linear array phased array probe (4) receives an ultrasonic signal.
9. The method for detecting internal defects of a composite carbon felt-carbon fiber adhesive structure according to any one of claims 6 to 8, characterized in that: The defect quantification is specifically as follows: The width of the delamination defect is: L 分 =L0 2 -L0 1 3) Among them, L0 1 , L0 2 It is the acoustic beam electronic scanning sequence corresponding to the two ends of the delamination defect in the L0 view; The depth of the delamination defect is: <h2 style=";text-align:left;direction:ltr">H<h2 style=";text-align:left;direction:ltr"> 分 <h2 style=";text-align:left;direction:ltr"> (H0)<h2 style=";text-align:left;direction:ltr"> 1 <h2 style=";text-align:left;direction:ltr"> +H0<h2 style=";text-align:left;direction:ltr"> 2 <h2 style=";text-align:left;direction:ltr"> )÷2 4) Among them, H0 1 、H0 2 L0 1 and L0 2 Depth of defect signal in ; The width of the debonding defect is: Among them, L θ 1 , L θ 2 YesL θ The acoustic beam electronic scanning sequence corresponding to the two ends of the debonding defect in the view; the depth of the debonding defect is: H 脱 =H θ 1 +(H θ 1 +H θ 2 )÷2 6) Among them, H θ 1 , H θ 2 L θ 1 and L θ 2 The depth of defect signal in .