Ultra-wideband interlayer waveguide light beam splitter and preparation method thereof
By using silicon wafer substrates and organic polymer materials in three-dimensional photonic integrated chips, the problem of small bandwidth and difficult integration in the prior art is solved, and efficient beam splitting of signal light is achieved and robust, suitable for mass production.
Patent Information
- Application Number
- CN202411323150.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-23
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-23
AI Technical Summary
In the prior art, the interlayer waveguide beam splitter in the three-dimensional photonic integrated chip has a small bandwidth and is not easy to integrate, making it difficult to achieve information interaction between signal light between waveguides of different layers.
Using silicon wafers as substrates, using organic polymer materials with different refractive indexes as different cladding and core layers of interlayer waveguides, combined with spin coating and photolithography processes, an ultra-wideband interlayer waveguide light beam splitter was designed to utilize space The thermal insulation principle realizes the beam splitting of signal light.
It realizes efficient inter-layer beam splitting of signal light, is robust, has simple processing technology, is compatible with semiconductor technology, is suitable for large-scale production, and expands the application of polymer-based integrated optoelectronic devices.
Smart Images

Figure CN118938393A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of interlayer waveguide optical beam splitters and preparation thereof, and specifically relates to an ultra-wideband interlayer waveguide optical beam splitter using a silicon wafer as a substrate and organic polymer materials with different refractive indices as a lower cladding, an intermediate cladding, an upper cladding, a lower core layer and an upper core layer of the interlayer waveguide optical beam splitter, and a preparation method thereof. Background Art
[0002] With the development of new technologies such as big data and artificial intelligence, the data transmission capacity required by communication systems is growing rapidly. Compared with traditional electrical interconnection, optical interconnection is considered to be an effective technology that can achieve larger capacity and higher transmission speed, and has become the main means of digital communication. Optical communication is an important part of modern communication systems and plays a very important role in all areas of the national economy. In recent years, as photonic chips need to process more and more information, on-chip complexity and crosstalk are getting higher and higher, and chip size is getting larger and larger, three-dimensional photonic integrated chips have become a new way to achieve miniaturization and integration of photonic chips. Three-dimensional photonic integrated chips can integrate multiple layers of devices on a chip to achieve flexible design and high-density integration. At present, they have become a frontier and hot research topic in the field of optical communications.
[0003] Optical beam splitters are used to split and combine signal light. They are an important component of optical switches and optical modulators, and are also one of the most important devices in optical communication systems. As an important branch of optical beam splitters, optical waveguide optical beam splitters have developed rapidly in recent years. They not only have the advantages of optical fiber optical beam splitters, but also have higher stability and reliability, and can work in more complex and harsh environments. In addition, there are a variety of materials used to prepare optical waveguide optical beam splitters, mainly including inorganic materials and organic polymer materials. Compared with inorganic materials, organic polymer materials are of various types, low cost, simple preparation process, compatible with semiconductor processes, strong anti-interference ability, and preparation process compatible with semiconductor processes, which is conducive to the functional integration and mass production of devices. Organic polymer materials have great development and application prospects. At present, they have become the basic materials for realizing low-cost, high-performance photonic devices, and have been widely used in optical communications and aerospace fields. However, there is a lack of interlayer waveguide optical beam splitters that can be applied to three-dimensional photonic integrated chips, and there are problems such as small bandwidth and difficulty in integration. Summary of the invention
[0004] In order to overcome the deficiencies of the prior art and realize the information interaction between different layers of waveguides of signal light in a three-dimensional photonic integrated chip, the purpose of the present invention is to provide an ultra-wideband interlayer waveguide optical beam splitter that can be applied to a three-dimensional photonic integrated chip and a preparation method thereof. The present invention uses a silicon wafer as a substrate, an organic polymer material as the lower cladding, middle cladding and upper cladding of the waveguide, and an organic polymer material with a large refractive index as the lower core layer and upper core layer of the waveguide, making full use of the advantages of the variety and strong processability of organic polymer materials. At the same time, the preparation process adopted by the present invention is simple, compatible with semiconductor processes, easy to integrate, and suitable for large-scale production, which effectively expands the application of polymer-based integrated optoelectronic devices in three-dimensional photonic integrated chips, and thus has important practical application value.
[0005] The technical solution adopted by the present invention to solve the technical problem is as follows:
[0006] As attached Figure 1 As shown ( Figure 2 The ultra-wideband interlayer waveguide optical beam splitter described in the present invention is prepared based on the principle of spatial adiabatic [Physical Review A73,032319(2006).] This technology has been proven to be very robust to manufacturing errors and wavelength dispersion, and is widely used in waveguide optical couplers and optical communications. The ultra-wideband interlayer waveguide optical splitter consists of, from bottom to top, a silicon substrate 31, a polymer optical waveguide lower cladding 32 prepared on the silicon substrate 31, a strip polymer optical waveguide lower core layer 33 prepared on the polymer optical waveguide lower cladding 32, a polymer optical waveguide intermediate cladding 34 prepared on the polymer optical waveguide lower cladding 32 and the strip polymer optical waveguide lower core layer 33, a strip polymer optical waveguide upper core layer 35 prepared on the polymer optical waveguide intermediate cladding 34, and a polymer optical waveguide upper cladding 36 prepared on the polymer optical waveguide intermediate cladding 34 and the strip polymer optical waveguide upper core layer 35, wherein the strip polymer optical waveguide lower core layer 33 is coated in the polymer optical waveguide intermediate cladding 34, and the strip polymer optical waveguide upper core layer 35 is coated in the polymer optical waveguide upper cladding 36.
[0007] As attached Figure 2 As shown, the strip polymer optical waveguide lower core layer 33 is composed of a discrete lower output waveguide 1, a lower left straight waveguide 2, a lower input straight waveguide 3 and a lower right straight waveguide 4, and the strip polymer optical waveguide upper core layer 35 is composed of an upper output straight waveguide 5; the lower left straight waveguide 2 and the lower right straight waveguide 4 are symmetrically arranged with respect to the lower input straight waveguide 3, and the upper output straight waveguide 5 is arranged in parallel with the lower input straight waveguide 3; the projection length of the lower output waveguide 1, the lower left straight waveguide 2 and the lower right straight waveguide 4 along the direction of the lower input straight waveguide 3 (i.e., the z-axis direction) is equal to the length of the lower input straight waveguide 3 and the upper output straight waveguide 5, which is L.1 =100~10000μm, width is equal to W 1 = 1 ~ 20μm; at the input end, the gap between the lower left straight waveguide 2 and the lower input straight waveguide 3, and the gap between the lower right straight waveguide 4 and the lower input straight waveguide 3 are equal to G 1 =2~30μm; at the output end, the gap between the lower left straight waveguide 2 and the lower input straight waveguide 3, and the gap between the lower right straight waveguide 4 and the lower input straight waveguide 3 are equal to G 2 =0.5~12μm, and G 1 >G 2 At the input end, the upper output straight waveguide 5 is located directly above the lower right straight waveguide 4, and the gap G 3 =0.5~12μm; the position of the lower output waveguide 1 should make the "coupling coefficient between the lower output waveguide 1 and the lower left straight waveguide 2" the same as the "coupling coefficient between the lower right straight waveguide 4 and the upper output straight waveguide 5"; the refractive index of the strip polymer optical waveguide lower core layer 33 and the strip polymer optical waveguide upper core layer 35 materials is higher than the refractive index of the polymer optical waveguide lower cladding 32, the polymer optical waveguide middle cladding 34 and the polymer optical waveguide upper cladding 36 materials.
[0008] The thickness of the silicon substrate 31 is 0.5 to 2 mm, the thickness of the polymer optical waveguide lower cladding 32 is 3 to 20 μm, the thickness of the strip polymer optical waveguide lower core layer 33 is 3 to 10 μm, the thickness of the polymer optical waveguide intermediate cladding 34 above the strip polymer optical waveguide lower core layer 33 is 0.5 to 12 μm, the thickness of the strip polymer optical waveguide upper core layer 35 is 3 to 10 μm, and the thickness of the polymer optical waveguide upper cladding 36 above the strip polymer optical waveguide upper core layer 35 is 3 to 20 μm.
[0009] Light is input from the lower input straight waveguide 3, and is coupled to the lower output waveguide 1 and the upper output straight waveguide 5 respectively through the lower left straight waveguide 2 and the lower right straight waveguide 4 (between two waveguides that are close to each other, due to the overlap of latent vector waves in the waveguide mode, light energy exchange occurs, so the signal light is coupled from the lower input straight waveguide 3 into the lower left straight waveguide 2 and the lower right straight waveguide 4), and is output from the lower output waveguide 1 and the upper output straight waveguide 5.
[0010] The method for preparing an ultra-wideband interlayer waveguide optical beam splitter according to the present invention has a preparation process as follows: Figure 3 As shown, the specific steps are as follows:
[0011] A: Cleaning of silicon substrate 31
[0012] The silicon substrate 31 is wiped with cotton balls soaked in acetone and ethanol respectively, then rinsed with deionized water, and then blown dry with nitrogen gas;
[0013] B: Preparation of polymer optical waveguide lower cladding 32
[0014] The polymer optical waveguide lower cladding material (the polymer optical waveguide lower cladding material is a series of organic polymer materials with good transparency including polymethyl methacrylate (PMMA), polycarbonate (PC), polyimide (PI), polyethylene (PE), polyester (PET), polystyrene (PS), EpoClad, etc.) is spin-coated on the cleaned silicon substrate 31 by a spin coating process, the spin coating speed is 1000-5000 rpm, and then heated at 110-150° C. for 2-20 minutes, and the whole is exposed to ultraviolet light with a wavelength of 350-400 nm for 2-20 seconds, and then heated at 110-150° C. for 20-70 minutes, and the thickness of the obtained polymer optical waveguide lower cladding 32 is 3-20 μm;
[0015] C: Preparation of the lower core layer 33 of the strip polymer optical waveguide
[0016] The polymer optical waveguide lower core layer material (the polymer optical waveguide lower core layer material includes EpoCore, SU-8 2002, SU-8 2005, a series of wet-etchable ultraviolet negative photoresist materials, the refractive index of the polymer optical waveguide lower core layer material is higher than the refractive index of the polymer optical waveguide lower cladding material, the polymer optical waveguide intermediate cladding material and the polymer optical waveguide upper cladding material) is spin-coated on the polymer optical waveguide lower cladding 32 to form a thin film, the rotation speed is 600 to 5000 rpm, and the thickness of the polymer optical waveguide lower core layer film 33' is 3 to 10 μm; then the spin-coated polymer optical waveguide lower core layer film 33' is pre-baked, that is, the step-by-step heating method is used to heat it at 40 to 80° C. for 2 to 20 minutes, and then heated at 70 to 120° C. for 2 to 40 minutes; the polymer optical waveguide lower core layer film 33' is photolithographically processed, that is, the plate is photolithographically processed under ultraviolet light with a wavelength of 350 to 400 nm, and the waveguide mask is complementary to the polymer optical waveguide lower core layer structure to be prepared (such as Figure 2As shown), the exposure time is 3 to 20 seconds, so that the polymer optical waveguide lower core layer material of the lower output waveguide 1, the lower left straight waveguide 2, the lower input straight waveguide 3 and the lower right straight waveguide 4 of the device to be prepared is exposed to ultraviolet light; after the photolithography is completed, it is taken out from the photolithography machine for intermediate baking, that is, heating at 40 to 80° C. for 2 to 20 minutes, and then heating at 80 to 120° C. for 2 to 40 minutes, and cooling at room temperature for 1 to 2 hours after the heating is completed; after the cooling is completed, it is developed, first wet etching in the developer corresponding to the polymer optical waveguide lower core layer material 5 to 80 seconds, remove the unexposed non-polymer optical waveguide lower core layer structure, then put it into isopropanol solution to wash away the polymer optical waveguide lower core layer material and developer remaining on the surface of the silicon substrate, and then rinse it repeatedly with deionized water (rinsing should be done along the waveguide direction to prevent the waveguide from being damaged) to remove the isopropanol, and then blow it dry with nitrogen; finally, post-bake the film, that is, heat it at 110 to 150° C. for 20 to 70 minutes, and cool it down at room temperature for 1 to 2 hours after heating, so that a strip-shaped polymer optical waveguide lower core layer 33 is prepared on the polymer optical waveguide lower cladding;
[0017] D: Preparation of polymer optical waveguide intermediate cladding 34
[0018] The polymer optical waveguide intermediate cladding material (the polymer intermediate cladding material is a series of organic polymer materials with good transparency including polymethyl methacrylate (PMMA), polycarbonate (PC), polyimide (PI), polyethylene (PE), polyester (PET), polystyrene (PS), EpoClad, etc., and the same polymer optical waveguide lower cladding material, polymer optical waveguide intermediate cladding material and polymer optical waveguide upper cladding material are used in the same device for the best effect) is spin-coated on the polymer optical waveguide lower cladding 32 and the polymer optical waveguide lower core layer 33, the spin-coating speed is 1500-6000 rpm, and then heated at 110-150° C. for 2-20 minutes, exposed to ultraviolet light with a wavelength of 350-400 nm for 2-20 seconds, and then heated at 110-150° C. for 20-70 minutes, and the thickness of the obtained polymer optical waveguide intermediate cladding 34 is 0.5-12 μm;
[0019] E: Preparation of the core layer 35 on the strip polymer optical waveguide
[0020] The polymer optical waveguide upper core layer material (the polymer optical waveguide upper core layer material is a series of wet-etchable ultraviolet negative photoresist materials including EpoCore, SU-8 2002, and SU-8 2005, the refractive index of the polymer optical waveguide upper core layer material is higher than the refractive index of the polymer optical waveguide lower cladding material, the polymer optical waveguide middle cladding material, and the polymer optical waveguide upper cladding material. In the same device, using the same polymer optical waveguide lower core layer material and polymer optical waveguide upper core layer material is the best effect) is spin-coated on the polymer optical waveguide middle cladding 34 to form a thin film, the rotation speed is 600 to 5000 rpm, and the polymer optical waveguide is The thickness of the core layer film 35' on the waveguide is 3 to 10 μm; the spin-coated polymer optical waveguide core layer film 35' is then pre-baked, that is, heated at 40 to 80° C. for 2 to 20 minutes by a step-by-step heating method, and then heated at 70 to 120° C. for 2 to 40 minutes; the polymer optical waveguide core layer film 35' is photolithographically processed, that is, the plate is photolithographically processed under ultraviolet light with a wavelength of 350 to 400 nm, and the waveguide mask is complementary to the polymer optical waveguide core layer structure to be prepared (such as Figure 2 As shown), the exposure time is 3 to 20 seconds, so that the polymer optical waveguide upper core layer material of the upper output straight waveguide 5 area of the device to be prepared is exposed to ultraviolet light; after the photolithography is completed, it is taken out from the photolithography machine for intermediate baking, heated at 40 to 80°C for 2 to 20 minutes, and then heated at 80 to 120°C for 2 to 40 minutes. After the heating is completed, the temperature is cooled at room temperature for 1 to 2 hours; after the cooling is completed, it is developed, first wet-etched in the developer corresponding to the core layer material of the polymer optical waveguide for 5 to 80 seconds, and the unexposed non-polymer The core layer structure of the optical waveguide is removed, and then the polymer optical waveguide core layer material and developer remaining on the surface of the silicon substrate are washed away in an isopropanol solution, and then the isopropanol is removed by repeated rinsing with deionized water (rinsing should be done along the waveguide direction to prevent the waveguide from being damaged), and then the isopropanol is removed, and then the film is blown dry with nitrogen; finally, the film is post-baked, that is, heated at 110-150° C. for 20-70 minutes, and then cooled at room temperature for 1-2 hours after the heating is completed, so that a strip-shaped polymer optical waveguide core layer 35 is prepared on the polymer optical waveguide intermediate cladding 34;
[0021] F: Preparation of the upper cladding layer 36 of the polymer optical waveguide
[0022] The polymer optical waveguide upper cladding material (the polymer upper cladding material is a series of organic polymer materials with good transparency including polymethyl methacrylate (PMMA), polycarbonate (PC), polyimide (PI), polyethylene (PE), polyester (PET), polystyrene (PS), EpoClad, etc., and the same polymer optical waveguide lower cladding material, polymer optical waveguide middle cladding material and polymer optical waveguide upper cladding material are used for the best effect in the same device) is applied by spin coating process. The polymer optical waveguide intermediate cladding 34 and the strip polymer optical waveguide upper core layer 35 are spin-coated at a speed of 1000 to 5000 rpm, and then heated at 110 to 150° C. for 2 to 20 minutes, and the entire layer is exposed to ultraviolet light with a wavelength of 350 to 400 nm for 2 to 20 seconds, and then heated at 110 to 150° C. for 20 to 70 minutes. The thickness of the obtained polymer optical waveguide upper cladding 36 is 3 to 20 μm, thereby obtaining the ultra-wideband interlayer waveguide optical splitter described in the present invention.
[0023] Compared with the existing device structure and preparation technology, the beneficial effects of the present invention are: the ultra-wideband interlayer waveguide optical beam splitter of the present invention combines the advantages of strong robustness of the spatial insulation structure and flexible processing technology of organic polymer materials, and achieves the purpose of signal light interlayer splitting; in addition, the use of polymer materials makes the preparation process of the device relatively simple, only conventional processes such as spin coating and photolithography are required, and more difficult processes are not required. The production cost is low, the efficiency is high, and large-scale batch production is possible, and it can be applied to the preparation of ultra-wideband interlayer waveguide optical beam splitters in practice. BRIEF DESCRIPTION OF THE DRAWINGS
[0024] Figure 1 : A cross-sectional schematic diagram of the ultra-wideband interlayer waveguide optical beam splitter according to the present invention;
[0025] Figure 2 : A schematic structural diagram of the ultra-wideband interlayer waveguide optical beam splitter of the present invention;
[0026] Figure 3 : A process flow chart of the preparation of the ultra-wideband interlayer waveguide optical beam splitter of the present invention;
[0027] Figure 4 : Position relationship curve between the lower output waveguide 1 and the lower left straight waveguide 2 of the ultra-wideband interlayer waveguide optical beam splitter of the present invention;
[0028] Figure 5 (a): Light field transmission simulation diagram of the ultra-wideband interlayer waveguide optical beam splitter of the present invention;
[0029] Figure 5 (b): Simulated diagram of the light field distribution at the output end of the ultra-wideband interlayer waveguide optical beam splitter according to the present invention;
[0030] Figure 6 : Curves showing the output power of the two output ports of the ultra-wideband interlayer waveguide optical beam splitter according to the present invention changing with wavelength;
[0031] like Figure 1 As shown, a cross-sectional schematic diagram of an ultra-wideband interlayer waveguide optical beam splitter, the names of the components are: silicon substrate 31, polymer optical waveguide lower cladding 32, strip polymer optical waveguide lower core layer 33, polymer optical waveguide middle cladding 34, strip polymer optical waveguide upper core layer 35, polymer optical waveguide upper cladding 36;
[0032] like Figure 2 As shown, a schematic diagram of the structure of an ultra-wideband interlayer waveguide optical beam splitter, the names of the components are: lower layer output waveguide 1, lower layer left straight waveguide 2, lower layer input straight waveguide 3, lower layer right straight waveguide 4, upper layer output straight waveguide 5;
[0033] like Figure 3 As shown, there is a silicon substrate 31, a polymer optical waveguide lower cladding 32 prepared by a spin coating process on the silicon substrate 31, a strip-shaped polymer optical waveguide lower core layer 33 prepared by a spin coating, photolithography, and wet etching process on the polymer optical waveguide lower cladding 32, a polymer optical waveguide intermediate cladding 34 prepared by a spin coating process on the polymer optical waveguide lower cladding 32 and the strip-shaped polymer optical waveguide lower core layer 33, a strip-shaped polymer optical waveguide upper core layer 35 prepared by a spin coating, photolithography, and wet etching process on the polymer optical waveguide intermediate cladding 34, and a polymer optical waveguide upper cladding 36 prepared by a spin coating process on the polymer optical waveguide intermediate cladding 34 and the strip-shaped polymer optical waveguide upper core layer 35;
[0034] like Figure 4 As shown in FIG. 1 , it is a position relationship curve between the lower output waveguide 1 and the lower left straight waveguide 2 of the ultra-wideband interlayer waveguide optical beam splitter of the present invention. The value of the x-axis at the input end of the lower input straight waveguide 3 is set to 0, and the value of the z-axis is set to 0. The position of the lower output waveguide 1 is calculated based on the relationship that the coupling coefficient between the lower output waveguide 1 and the lower left straight waveguide 2 is the same as the coupling coefficient between the lower right straight waveguide 4 and the upper output straight waveguide 5. The position of the lower output waveguide 1 is calculated based on the relationship that the coupling coefficient between the lower output waveguide 1 and the lower left straight waveguide 2 is the same as the coupling coefficient between the lower right straight waveguide 4 and the upper output straight waveguide 5. During the calculation process, 1000 z values are taken to calculate the coupling coefficients of each z value between the lower right straight waveguide 4 and the upper output straight waveguide 5. Then, the corresponding relative position of the lower output waveguide 1 and the lower left straight waveguide 2 is obtained by the same coupling coefficient. Finally, the calculated position is shown in the attached figure. Figure 4As shown, the gaps between the input end and the output end of the lower output waveguide 1 and the input end and the output end of the lower input straight waveguide 3 are 17 μm and 13.5 μm respectively.
[0035] like Figure 5 As shown, (a) is a simulation diagram of the light field transmission in the lower core layer 33 and the upper core layer 35 of the polymer optical waveguide when the ultra-wideband interlayer waveguide optical beam splitter inputs signal light, and (b) is a simulation diagram of the light field distribution at the output end. We use the materials and waveguide dimensions used in Example 1. It can be clearly seen from the two simulation diagrams that the power of the output signal light of the lower output waveguide 1 and the upper output straight waveguide 5 is almost the same;
[0036] like Figure 6 As shown, the output power of the two output ports of the ultra-wideband interlayer waveguide optical beam splitter varies with wavelength. It can be seen that the beam splitter can well realize the 3dB beam splitting function, and the output is insensitive to wavelength changes. DETAILED DESCRIPTION
[0037] Example 1
[0038] The present invention will be further described below in conjunction with the accompanying drawings and embodiments.
[0039] As attached Figure 1 Shown Figure 2 The cross-sectional view at the position A-A' in FIG. 1 shows an ultra-wideband interlayer waveguide optical beam splitter, which is composed of a silicon substrate 31, a polymer optical waveguide lower cladding 32 prepared on the silicon substrate 31, a strip-shaped polymer optical waveguide lower core layer 33 prepared on the polymer optical waveguide lower cladding 32, a polymer optical waveguide intermediate cladding 34 prepared on the polymer optical waveguide lower cladding 32 and the strip-shaped polymer optical waveguide lower core layer 33, a strip-shaped polymer optical waveguide upper core layer 35 prepared on the polymer optical waveguide intermediate cladding 34, and a strip-shaped polymer optical waveguide upper core layer 35 prepared on the polymer optical waveguide intermediate cladding 34. The strip polymer optical waveguide is composed of a polymer optical waveguide upper cladding layer 36 prepared on the strip polymer optical waveguide middle cladding layer 34 and the strip polymer optical waveguide upper core layer 35, and the strip polymer optical waveguide lower core layer 33 is coated in the polymer optical waveguide middle cladding layer 34, and the strip polymer optical waveguide upper core layer 35 is coated in the polymer optical waveguide upper cladding layer 36; the lower output waveguide 1, the lower left straight waveguide 2, the lower input straight waveguide 3 and the lower right straight waveguide 4 together constitute the strip polymer optical waveguide lower core layer 33, and the upper output straight waveguide 5 constitutes the strip polymer optical waveguide upper core layer 35;
[0040] As attached Figure 2 As shown, the lower left straight waveguide 2 and the lower right straight waveguide 4 are symmetrical about the lower input straight waveguide 3, and the upper output straight waveguide 5 is parallel to the lower input straight waveguide 3; the lengths of the lower output waveguide 1, the lower left straight waveguide 2, the lower input straight waveguide 3, the lower right straight waveguide 4, and the upper output straight waveguide 5 are equal to L 1=3000μm, width is equal to W 1 =4.5μm; at the input end, the gap between the lower left straight waveguide 2 and the lower input straight waveguide 3, and the gap between the lower right straight waveguide 4 and the lower input straight waveguide 3 are equal to G 1 =5.8μm; at the output end, the gap between the lower left straight waveguide 2 and the lower input straight waveguide 3, and the gap between the lower right straight waveguide 4 and the lower input straight waveguide 3 are equal to G 2 =1μm; at the input end, the upper output straight waveguide 5 is located directly above the lower right straight waveguide 4, and the gap G 3 The coupling coefficient between the lower output waveguide 1 and the lower left straight waveguide 2 is the same as the coupling coefficient between the lower right straight waveguide 4 and the upper output straight waveguide 5. The position of the lower output waveguide 1 is calculated as shown in the attached figure. Figure 4 shown.
[0041] The thickness of the silicon substrate 31 is 1 mm, the thickness of the polymer optical waveguide lower cladding 32 is 5 μm, the thickness of the strip polymer optical waveguide lower core layer 33 is 4 μm, the thickness of the polymer optical waveguide intermediate cladding 34 above the strip polymer optical waveguide lower core layer 33 is 1 μm, the thickness of the strip polymer optical waveguide upper core layer 35 is 4 μm, and the thickness of the polymer optical waveguide upper cladding 36 above the strip polymer optical waveguide upper core layer 35 is 5 μm.
[0042] Light is input from the lower input straight waveguide 3, coupled to the lower output waveguide 1 and the upper output straight waveguide 5 through the lower left straight waveguide 2 and the lower right straight waveguide 4 respectively, and output from the lower output waveguide 1 and the upper output straight waveguide 5.
[0043] Example 2
[0044] A: Cleaning of silicon substrate 31
[0045] The silicon substrate 31 is wiped with cotton balls soaked in acetone and ethanol respectively, then rinsed with deionized water, blown dry with nitrogen, placed in a clean culture dish and sealed.
[0046] B: Preparation of polymer optical waveguide lower cladding 32
[0047] The polymer optical waveguide lower cladding material EpoClad was spin-coated on the cleaned silicon substrate by a spin coating process at a spin coating speed of 3000 rpm, and then heated at 120° C. for 5 minutes, and exposed to ultraviolet light with a wavelength of 365 nm for 12 seconds, and then heated at 120° C. for 60 minutes. The obtained polymer optical waveguide lower cladding 32 had a thickness of 5 μm.
[0048] C: Preparation of the lower core layer 33 of the strip polymer optical waveguide
[0049] The polymer optical waveguide lower core layer material EpoCore is spin-coated on the polymer optical waveguide lower cladding layer 32 by a spin coating process, the rotation speed is 3100 rpm, and the thickness of the EpoCore film 33' is 4 μm; then the spin-coated EpoCore film 33' is pre-baked, that is, heated at 50° C. for 2 minutes by a step-by-step heating method, and then heated at 90° C. for 20 minutes; the EpoCore film 33' is photolithographically processed, that is, the plate is photolithographically processed under ultraviolet light with a wavelength of 365 nm, and the waveguide mask is complementary to the polymer optical waveguide lower core layer structure to be prepared (such as Figure 2 As shown), the exposure time is 5.8 seconds, so that the EpoCore film in the lower output waveguide 1, the lower left straight waveguide 2, the lower input straight waveguide 3, and the lower right straight waveguide 4 areas of the device to be prepared are exposed to ultraviolet light; after the photolithography is completed, it is taken out from the photolithography machine for intermediate baking, that is, heating at 50°C for 2 minutes, and then heating at 85°C for 20 minutes. After the heating is completed, the temperature is cooled at room temperature for 1 hour; after the cooling is completed, it is developed, first wet-etched in the developer corresponding to EpoCore for 15 seconds, The unexposed non-polymer optical waveguide lower core layer structure is removed, and then placed in an isopropanol solution to wash away the EpoCore and developer remaining on the surface of the silicon substrate, and then repeatedly rinsed with deionized water (rinsing should be done along the waveguide direction to prevent the waveguide from being damaged), the isopropanol is removed, and then dried with nitrogen; finally, the film is post-baked, that is, heated at 120° C. for 60 minutes, and then cooled at room temperature for 1 hour after heating, so that a strip-shaped polymer optical waveguide lower core layer 33 is prepared on the polymer optical waveguide lower cladding layer;
[0050] D: Preparation of polymer optical waveguide intermediate cladding 34
[0051] The polymer optical waveguide intermediate cladding material EpoClad is spin-coated on the strip polymer optical waveguide lower core layer 33 by a spin coating process, the spin coating speed is 3000 rpm, and then heated at 120° C. for 5 minutes, and the entire layer is exposed to ultraviolet light with a wavelength of 365 nm for 12 seconds, and then heated at 120° C. for 60 minutes. The thickness of the prepared polymer optical waveguide intermediate cladding 34 is 1 μm (the distance from the upper surface of the polymer optical waveguide intermediate cladding to the upper surface of the strip polymer optical waveguide lower core layer);
[0052] E: Preparation of the core layer 35 on the strip polymer optical waveguide
[0053] The polymer optical waveguide upper core layer material EpoCore is spin-coated on the polymer optical waveguide intermediate cladding 34 by a spin coating process to form a thin film, the rotation speed is 3100 rpm, and the thickness of the EpoCore film 35' is 4 μm; then the spin-coated EpoCore film 35' is pre-baked, that is, it is heated at 50° C. for 2 minutes by a step-by-step heating method, and then heated at 90° C. for 20 minutes; the EpoCore film 35' is photolithographically processed, that is, it is photolithographically processed under ultraviolet light with a wavelength of 365 nm, and the waveguide mask is complementary to the polymer optical waveguide upper core layer structure to be prepared (such as Figure 2 As shown), the exposure time is 5.8 seconds, so that the EpoCore of the upper output straight waveguide 5 area of the device to be prepared is exposed to ultraviolet light; after the photolithography is completed, it is taken out from the photolithography machine for intermediate baking, that is, heating at 50°C for 2 minutes, then heating at 85°C for 20 minutes, and cooling at room temperature for 1 hour after heating; after cooling, it is developed, first wet etching in the developer corresponding to EpoCore for 15 seconds, the unexposed non-polymer optical waveguide upper core layer structure is removed, and then it is placed in an isopropanol solution to wash away the EpoCore and developer remaining on the surface of the silicon substrate, and then repeatedly rinsed with deionized water (rinsing should be rinsed along the waveguide direction to prevent the waveguide from being damaged), remove the isopropanol, and then blown dry with nitrogen; finally, the film is post-baked, heated at 120°C for 60 minutes, and cooled at room temperature for 1 hour after heating, so that a strip polymer optical waveguide upper core layer 35 is prepared on the polymer optical waveguide intermediate cladding;
[0054] F: Preparation of the upper cladding layer 36 of the polymer optical waveguide
[0055] The polymer optical waveguide upper cladding material EpoClad is spin-coated on the strip polymer optical waveguide upper core layer 35 by a spin coating process at a spin coating speed of 2000 rpm, and then heated at 120°C for 5 minutes, and the entire layer is exposed to ultraviolet light with a wavelength of 365nm for 12 seconds, and then heated at 120°C for 60 minutes. The thickness of the obtained polymer optical waveguide upper cladding 36 is 5μm (the distance from the upper surface of the polymer optical waveguide upper cladding to the upper surface of the strip polymer optical waveguide upper core layer); thereby, the ultra-wideband interlayer waveguide optical beam splitter described in the present invention is obtained.
[0056] It should be noted that the specific implementations mentioned in this patent are only representative examples of the present invention. Obviously, the present invention is not limited to the details of the above exemplary embodiments, and there may be more forms. Moreover, the materials of the design are not limited to this, and waveguide materials such as lithium niobate, silicon, silicon nitride, and silicon dioxide may also be used. Any reference numerals in the claims should not be regarded as limiting the claims involved. Those skilled in the art who have clearly disclosed the present invention or have obtained it without objection based on the written description of the document are all within the scope of protection of this patent.
Claims
1. An ultra-wideband interlayer waveguide optical beam splitter, Features: The optical waveguide structure is composed of, from bottom to top, a silicon substrate (31), a polymer optical waveguide lower cladding (32) prepared on the silicon substrate (31), a strip-shaped polymer optical waveguide lower core layer (33) prepared on the polymer optical waveguide lower cladding (32), a polymer optical waveguide intermediate cladding (34) prepared on the polymer optical waveguide lower cladding (32) and the strip-shaped polymer optical waveguide lower core layer (33), a strip-shaped polymer optical waveguide upper core layer (35) prepared on the polymer optical waveguide intermediate cladding (34), and a polymer optical waveguide upper cladding (36) prepared on the polymer optical waveguide intermediate cladding (34) and the strip-shaped polymer optical waveguide upper core layer (35). The strip-shaped polymer optical waveguide lower core layer (33) is coated in the polymer optical waveguide intermediate cladding (34). The strip-shaped polymer optical waveguide upper core layer (35) is coated in the strip-shaped polymer optical waveguide 5) is coated in the upper cladding layer (36) of the polymer optical waveguide; the lower core layer (33) of the strip-shaped polymer optical waveguide is composed of a discrete lower output waveguide (1), a lower left straight waveguide (2), a lower input straight waveguide (3) and a lower right straight waveguide (4); the upper core layer (35) of the strip-shaped polymer optical waveguide is composed of an upper output straight waveguide (5); the lower left straight waveguide (2) and the lower right straight waveguide (4) are symmetrically arranged with respect to the lower input straight waveguide (3); the upper output straight waveguide (5) is arranged in parallel with the lower input straight waveguide (3); the projection length of the lower output waveguide (1), the lower left straight waveguide (2) and the lower right straight waveguide (4) along the direction of the lower input straight waveguide (3) is equal to the length of the lower input straight waveguide (3) and the upper output straight waveguide (5), which is L 1 , the width is equal to W 1 At the input end, the gap between the lower left straight waveguide (2) and the lower input straight waveguide (3), and the gap between the lower right straight waveguide (4) and the lower input straight waveguide (3) are equal to G 1 At the output end, the gap between the lower left straight waveguide (2) and the lower input straight waveguide (3), and the gap between the lower right straight waveguide (4) and the lower input straight waveguide (3) are equal to G 2 , and G 1 >G 2 ; At the input end, the upper output straight waveguide (5) is located directly above the lower right straight waveguide (4), with a gap of G 3 ; The position of the lower output waveguide (1) makes the "coupling coefficient between the lower output waveguide (1) and the lower left straight waveguide (2)" and the "coupling coefficient between the lower right straight waveguide (4) and the upper output straight waveguide (5)" the same; the refractive index of the material of the strip polymer optical waveguide lower core layer (33) and the strip polymer optical waveguide upper core layer (35) is higher than the refractive index of the material of the polymer optical waveguide lower cladding layer (32), the polymer optical waveguide middle cladding layer (34) and the polymer optical waveguide upper cladding layer (36).
2. An ultra-wideband interlayer waveguide optical beam splitter as claimed in claim 1, Features: The thickness of the silicon substrate (31) is 0.5 to 2 mm, the thickness of the polymer optical waveguide lower cladding (32) is 3 to 20 μm, the thickness of the strip-shaped polymer optical waveguide lower core layer (33) is 3 to 10 μm, the thickness of the polymer optical waveguide intermediate cladding (34) on the strip-shaped polymer optical waveguide lower core layer (33) is 0.5 to 12 μm, the thickness of the strip-shaped polymer optical waveguide upper core layer (35) is 3 to 10 μm, and the thickness of the polymer optical waveguide upper cladding (36) on the strip-shaped polymer optical waveguide upper core layer (35) is 3 to 20 μm; L 1 =100~10000μm,W 1 =1~20μm, G 1 =2~30μm, G 2 =0.5~12μm, and G 1 >G 2 ; G 3 =0.5~12μm.
3. An ultra-wideband interlayer waveguide optical beam splitter as claimed in claim 1, Features: The materials of the polymer optical waveguide lower cladding (32), the polymer optical waveguide middle cladding (34) and the polymer optical waveguide upper cladding (36) are polymethyl methacrylate, polycarbonate, polyimide, polyethylene, polyester, polystyrene or EpoClad; the materials of the strip-shaped polymer optical waveguide lower core layer (33) and the strip-shaped polymer optical waveguide upper core layer (35) are EpoCore, SU-8 2002 or SU-8 2005.
4. An ultra-wideband interlayer waveguide optical beam splitter as claimed in claim 1, Features: The polymer optical waveguide lower cladding (32), the polymer optical waveguide middle cladding (34) and the polymer optical waveguide upper cladding (36) are made of the same material, and the strip-shaped polymer optical waveguide lower core layer (33) and the strip-shaped polymer optical waveguide upper core layer (35) are made of the same material.
5. A method for preparing an ultra-wideband interlayer waveguide optical beam splitter according to any one of claims 1 to 4, wherein the steps are as follows: A: Cleaning of silicon substrate (31) The silicon substrate (31) was wiped with cotton balls soaked in acetone and ethanol respectively, then rinsed with deionized water, and then dried with nitrogen gas; B: Preparation of polymer optical waveguide lower cladding (32) The polymer optical waveguide lower cladding material is spin-coated on a cleaned silicon substrate (31) by a spin coating process, the spin coating speed is 1000-5000 rpm, and then heated at 110-150° C. for 2-20 minutes, the whole is exposed to ultraviolet light with a wavelength of 350-400 nm for 2-20 seconds, and then heated at 110-150° C. for 20-70 minutes to obtain a polymer optical waveguide lower cladding (32); C: Preparation of the lower core layer (33) of the strip polymer optical waveguide The polymer optical waveguide lower core layer material is spin-coated on the polymer optical waveguide lower cladding layer (32) by a spin coating process to form a polymer optical waveguide lower core layer film (33'), with a rotation speed of 600 to 5000 revolutions per minute; the spin-coated polymer optical waveguide lower core layer film (33') is then pre-baked, that is, heated at 40 to 80° C. for 2 to 20 minutes by a step-by-step heating method, and then heated at 70 to 120° C. for 2 to 40 minutes; the polymer optical waveguide lower core layer film (33') is photolithographically processed, that is, plate-aligned photolithography is performed under ultraviolet light with a wavelength of 350 to 400 nm, the waveguide mask is complementary to the polymer optical waveguide lower core layer structure to be prepared, and the exposure time is 3 to 20 seconds, so that the polymer optical waveguide in the lower output waveguide (1), the lower left straight waveguide (2), the lower input straight waveguide (3) and the lower right straight waveguide (4) regions of the device to be prepared are formed. The polymer optical waveguide lower core layer material is exposed to ultraviolet light; after the photolithography is completed, it is taken out from the photolithography machine for intermediate baking, that is, heating at 40-80°C for 2-20 minutes, and then heating at 80-120°C for 2-40 minutes, and cooling at room temperature for 1-2 hours after the heating is completed; after the cooling is completed, it is developed, firstly wet-etching in a developer corresponding to the polymer optical waveguide lower core layer material for 5-80 seconds to remove the unexposed non-polymer optical waveguide lower core layer structure, and then it is placed in an isopropanol solution to wash away the polymer optical waveguide lower core layer material and the developer remaining on the surface of the silicon substrate, and then repeatedly rinsed with deionized water to remove the isopropanol, and then blown dry with nitrogen; finally, post-baking is performed to harden the film, that is, heating at 110-150°C for 20-70 minutes, and cooling at room temperature for 1-2 hours after the heating is completed, so that a strip-shaped polymer optical waveguide lower core layer (33) is obtained on the polymer optical waveguide lower cladding; D: Preparation of polymer optical waveguide intermediate cladding (34) The polymer optical waveguide intermediate cladding material is spin-coated on the polymer optical waveguide lower cladding (32) and the polymer optical waveguide lower core (33) by a spin coating process, the spin coating speed is 1500-6000 rpm, and then heated at 110-150° C. for 2-20 minutes, and the whole is exposed to ultraviolet light with a wavelength of 350-400 nm for 2-20 seconds, and then heated at 110-150° C. for 20-70 minutes to obtain a polymer optical waveguide intermediate cladding (34); E: Preparation of the core layer (35) of the strip polymer optical waveguide The polymer optical waveguide upper core layer material is spin-coated on the polymer optical waveguide intermediate cladding (34) by a spin coating process, and the rotation speed is 600 to 5000 revolutions per minute; then the spin-coated polymer optical waveguide upper core layer film (35') is pre-baked, that is, the step-by-step heating method is used to heat it at 40 to 80° C. for 2 to 20 minutes, and then the temperature is 70 to 120° C. for 2 to 40 minutes; the polymer optical waveguide upper core layer film (35') is photolithographically processed, that is, the plate is photolithographically processed under ultraviolet light with a wavelength of 350 to 400 nm, the waveguide mask is complementary to the polymer optical waveguide upper core layer structure to be prepared, and the exposure time is 3 to 20 seconds, so that the polymer optical waveguide upper core layer material in the upper output straight waveguide (5) area of the device to be prepared is exposed to ultraviolet light; after the photolithography is completed, Remove from the photolithography machine and perform intermediate baking, heat at 40-80°C for 2-20 minutes, then heat at 80-120°C for 2-40 minutes, and cool at room temperature for 1-2 hours after heating; perform development after cooling, first wet-etch in a developer corresponding to the polymer optical waveguide upper core layer material for 5-80 seconds to remove the unexposed non-polymer optical waveguide upper core layer structure, then place in an isopropanol solution to wash away the polymer optical waveguide upper core layer material and developer remaining on the surface of the silicon substrate, then repeatedly rinse with deionized water to remove the isopropanol, and then blow dry with nitrogen; finally perform post-baking to harden the film, i.e., heat at 110-150°C for 20-70 minutes, and cool at room temperature for 1-2 hours after heating, so that a strip-shaped polymer optical waveguide upper core layer (35) is obtained on the polymer optical waveguide intermediate cladding (34); F: Preparation of the upper cladding layer (36) of the polymer optical waveguide The polymer optical waveguide upper cladding material is spin-coated on the polymer optical waveguide intermediate cladding (34) and the strip polymer optical waveguide upper core layer (35) by a spin coating process, the spin coating speed is 1000-5000 rpm, and then heated at 110-150° C. for 2-20 minutes, and the whole is exposed to ultraviolet light with a wavelength of 350-400 nm for 2-20 seconds, and then heated at 110-150° C. for 20-70 minutes to obtain the polymer optical waveguide upper cladding (36), thereby obtaining the ultra-wideband interlayer waveguide optical beam splitter.
Citation Information
Patent Citations
Methods for fabrication of large core hollow waveguides
CN102089688A
Polarization rotation beam splitter based on strip-shaped geometric waveguide and preparation method thereof
CN111474629A
High-speed electro-optical modulator based on silicon nitride / organic polymer hybrid waveguide structure