Barium titanate-based ceramic dielectric material, capacitor dielectric ceramic and preparation method thereof

By doping modification and optimizing the sintering process, barium titanate-based ceramic dielectric materials with high dielectric constant, low dielectric loss and low capacitance temperature change rate were prepared, solving the technical problems of miniaturization and temperature stability of barium titanate-based multilayer ceramic capacitors, and realizing high-performance capacitor dielectric ceramics.

CN118942901APending Publication Date: 2024-11-12SHENZHEN INST OF ADVANCED ELECTRONICS MATERIALS
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202310515289.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-09
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing barium titanate-based multilayer ceramic capacitors have reliability issues in terms of miniaturization and large capacitance, and their dielectric properties are unstable with temperature changes, making it difficult to simultaneously meet the requirements of high dielectric constant, low dielectric loss, and high dielectric temperature stability.

Method used

Using BaTiO3 as the main material, doped with Dy2O3, MgO, MnO2, CaO, and SiO2, it is synthesized by hydrothermal method and then subjected to wet ball milling and drying. After adding a binder, it is molded and sintered to form a high-density capacitor dielectric ceramic. The grain structure is adjusted to improve the dielectric properties.

Benefits of technology

A barium titanate-based ceramic dielectric material with high dielectric constant, low dielectric loss and low capacitance temperature change rate was prepared. It meets the X7S standard and is suitable for capacitor dielectric ceramics in mobile electronic devices. It has good temperature stability and reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118942901A_ABST
    Figure CN118942901A_ABST
Patent Text Reader

Abstract

The invention discloses a barium titanate-based ceramic dielectric material with high temperature stability and high dielectric constant, capacitor dielectric ceramic and a preparation method thereof, and belongs to the technical field of ceramic dielectric. The dielectric ceramic material of the barium titanate-based ceramic takes 100 mol% of BaTiO3 as a main body material, 6.10-9.00 mol% of Dy2O3, MgO, MnO2, CaO and SiO2 are added as doping materials, the dielectric constant of the dielectric ceramic material is between 1980 and 2579, the room temperature dielectric loss can reach 1.00-2.10%, and the temperature characteristic meets the X7S requirement of EIA. The barium titanate-based ceramic material prepared by the invention is simple in preparation process, excellent in performance, economical and environment-friendly, and has a huge industrial application value.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of ceramic dielectrics, and in particular relates to a barium titanate-based ceramic dielectric material, a capacitor dielectric ceramic and a preparation method thereof. Background Art

[0002] Multilayer ceramic capacitors (MLCC) are widely used in communication infrastructure circuits in the fields of communication equipment, automotive electronics, industrial machinery, medical equipment, etc. In recent years, the miniaturization of mobile electronic devices has gradually led to the development of MLCC in the direction of miniaturization and large capacity. Barium titanate (BaTiO3) is the base material of Class II capacitors in MLCC. It has a high dielectric constant, but in order to obtain a large-capacity barium titanate-based MLCC, the number of stacking layers needs to be increased, resulting in a significant decrease in the reliability of MLCC. BaTiO3-based ceramics also have high dielectric constants, good ferroelectric, electrical and piezoelectric properties, and have broad application prospects in multilayer ceramic capacitors, piezoelectric converters, varistors and other devices. However, barium titanate materials are not suitable for the performance required by the current use environment. Therefore, in order to improve the relaxation behavior and dielectric properties of barium titanate ceramics, domestic and foreign researchers have made unremitting efforts. It was found that doping modification can improve the dielectric properties of BT to a certain extent, such as increasing the relative dielectric constant and reducing dielectric loss. Therefore, it is also particularly important to seek a sintering process suitable for the current dopant on this basis.

[0003] The capacitor specification of the Electronic Industries Alliance (EIA) of the United States states that the capacitance change rate of X7S must be within ±22% when the temperature is between -55℃ and 125℃. The stability of barium titanate when the temperature changes will affect its dielectric properties. Usually, its dielectric properties will suddenly change near the Curie temperature. In order to overcome the above problems, the performance of barium titanate powder needs to be optimized to meet the performance standards for capacitor use.

[0004] Therefore, there is an urgent need for a barium titanate-based ceramic material that not only has a high dielectric constant and low dielectric loss but also has high dielectric temperature stability. Summary of the invention

[0005] In order to solve the above technical problems, the present invention provides a barium titanate-based ceramic dielectric material with a high dielectric constant and a dielectric constant temperature change rate that meets the X7S standard, a capacitor dielectric ceramic and a preparation method thereof.

[0006] To achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0007] The first aspect of the present invention provides a barium titanate-based ceramic dielectric material, wherein the barium titanate-based ceramic dielectric material uses BaTiO3 as a main material and uses Dy2O3, MgO, MnO2, CaO, and SiO2 as modified doping materials; wherein the addition amount of the main material is 100 mol%, and the total addition amount of the modified doping materials is 6.10 mol% to 9.00 mol%.

[0008] Furthermore, in the barium titanate-based ceramic dielectric material, the added amount of Dy2O3 is 0.5mol% to 0.8mol%, the added amount of MgO is 3.0mol% to 4.6mol%, the added amount of MnO2 is 0.9mol% to 1.1mol%, the added amount of CaO is 0.5mol% to 0.7mol%, and the added amount of SiO2 is 1.2mol% to 1.8mol%.

[0009] Furthermore, the particle size of the BaTiO3 is 150nm to 280nm, and the particle sizes of the Dy2O3, MgO, MnO2, CaO, and SiO2 are nano-scale particle reagents.

[0010] The second aspect of the present invention provides a method for preparing the above-mentioned barium titanate-based ceramic dielectric material, which comprises: synthesizing the main material by a hydrothermal method, mixing the main material and a modified doping material, and then sequentially performing wet ball milling treatment and drying treatment to obtain the barium titanate-based ceramic dielectric material.

[0011] Furthermore, the wet ball milling treatment specifically includes: using 3 mm zirconium beads as grinding media, wet milling with anhydrous ethanol, the ball milling speed is 200 r / min to 280 r / min, and the ball milling time is 12 h to 48 h.

[0012] Furthermore, the drying process specifically includes: drying in an oven at 100° C. until completely dried.

[0013] The third aspect of the present invention provides a method for preparing a capacitor dielectric ceramic, which comprises: adding a binder to the barium titanate-based ceramic dielectric material as described above, grinding it and then performing a compression molding process to obtain a round blank, and sintering the round blank to obtain the capacitor dielectric ceramic.

[0014] Furthermore, the binder is 8wt% PVA, which is dripped into the barium titanate-based ceramic dielectric material at 12wt% to 18wt% for grinding and dispersion; the parameters of the compression molding process are 340Mpa to 380Mpa, the holding time is 20s to 30s, and it is pressed into a φ8mm×1.8mm round billet.

[0015] Furthermore, the sintering treatment specifically includes: in a sintering atmosphere, in a tubular furnace, heating to a temperature in the range of 1190°C to 1280°C at a rate of 1°C / min to 2°C / min and keeping warm for 1h to 2h, sintering into porcelain, and then cooling to room temperature at a rate of 4°C / min to 8°C / min; wherein during the heating process, keeping warm at 300°C and 600°C for 25min to 35min respectively for sufficient debinding; the sintering atmosphere is air or a reducing atmosphere; wherein the reducing atmosphere includes 1% H2 and 99% N2 by volume fraction.

[0016] A fourth aspect of the present invention provides a capacitor dielectric ceramic obtained by the above-mentioned method for preparing the capacitor dielectric ceramic.

[0017] Compared with the prior art, the technical solution provided by the present invention has at least the following advantages:

[0018] 1. The present invention uses BaTiO3 as the main material, and optimizes the performance of BaTiO3 material by modification and doping to prepare barium titanate-based ceramic dielectric materials with high dielectric constant, low dielectric loss and low capacitance-temperature change rate. Among them, SiO2 is often used as a sintering aid to reduce the sintering temperature and expand the sintering temperature range, inhibit or promote the growth of ceramic grains, and react with BT to form a low eutectic phase. When this temperature is exceeded, the liquid phase flows and wets the grains, promoting densification sintering. The addition of CaO can form a SiO2-CaO-BT ternary system. In the grain dissolution-precipitation mechanism with the participation of the liquid phase in sintering, the growth of BT grains can be prevented to form particles with small particle size and high density; MnO2 is added as an anti-reducing agent to inhibit Ti 4+ Sintering in a reducing atmosphere to form Ti 3+ Oxygen vacancies and other defects are generated, which deteriorate the dielectric properties of the ceramic and increase its residual polarization strength. MgO exists as a grain inhibitor, regulating the element distribution of grain boundaries and inhibiting grain growth. MgO and the rare earth element Dy2O3 have a synergistic effect, regulating the "core-shell" structure of ceramic grains, thereby stabilizing the effect of temperature on capacitance.

[0019] 2. Under the synergistic effect of BaTiO3 grains and MgO-Dy2O3, the "core-shell" structure of the ceramic grains and the induction of the dispersed phase change significantly improve the capacitance coefficient of the ceramic material, which meets the X7S standard. The barium titanate-based ceramic dielectric material and capacitor provided by the present invention have a simple preparation process, do not contain toxic substances, have a good match with nickel and other base metal internal electrodes, have high density, small grains, few defects, and have broad application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] One or more embodiments are exemplarily described by pictures in the corresponding drawings, and these exemplifications do not constitute limitations on the embodiments. Unless otherwise stated, the pictures in the drawings do not constitute proportional limitations.

[0021] Figure 1 is a schematic diagram of the dielectric constant, dielectric loss and temperature of the capacitor dielectric ceramic in Example 1 of the present invention;

[0022] Figure 2 is a schematic diagram of the capacitance change rate and temperature of the capacitor dielectric ceramic in Example 1 of the present invention;

[0023] Figure 3 is a schematic diagram of the dielectric constant, dielectric loss and temperature of the capacitor dielectric ceramic in Example 2 of the present invention;

[0024] Figure 4 is a schematic diagram of the capacitance change rate and temperature of the capacitor dielectric ceramic in Example 2 of the present invention;

[0025] Figure 5 is a schematic diagram of the dielectric constant, dielectric loss and temperature of the capacitor dielectric ceramic in Example 3 of the present invention;

[0026] Figure 6 Schematic diagram of the capacitance change rate and temperature of the capacitor dielectric ceramic in Example 3 of the present invention. DETAILED DESCRIPTION

[0027] The first aspect of the present invention provides a barium titanate-based ceramic dielectric material, wherein the barium titanate-based ceramic dielectric material uses BaTiO3 as a main material and uses Dy2O3, MgO, MnO2, CaO, and SiO2 as modified doping materials; wherein the addition amount of the main material is 100 mol%, and the total addition amount of the modified doping materials is 6.10 mol% to 9.00 mol%.

[0028] The second aspect of the present invention provides a method for preparing the above-mentioned barium titanate-based ceramic dielectric material, which comprises: synthesizing the main material by a hydrothermal method, mixing the main material and a modified doping material, and then sequentially performing wet ball milling treatment and drying treatment to obtain the barium titanate-based ceramic dielectric material.

[0029] The third aspect of the present invention provides a method for preparing a capacitor dielectric ceramic, which comprises: adding a binder to the barium titanate-based ceramic dielectric material as described above, grinding it and then performing a compression molding process to obtain a round blank, and sintering the round blank to obtain the capacitor dielectric ceramic.

[0030] A fourth aspect of the present invention provides a capacitor dielectric ceramic obtained by the above-mentioned method for preparing the capacitor dielectric ceramic.

[0031] The following embodiments are only some embodiments of the present invention, rather than all embodiments. Therefore, the detailed description in the embodiments of the present invention provided below is not intended to limit the scope of the present invention claimed for protection, but merely represents selected embodiments of the present invention. Based on the embodiments of the present invention, all other embodiments obtained by those skilled in the art without making creative work belong to the protection scope of the present invention.

[0032] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0033] Example 1

[0034] In this embodiment, the main material is selected as BaTiO3 powder with a particle size of 200nm, the sintering temperature in air atmosphere is 1220℃, the holding time is 1h, and the other process steps involved remain unchanged. The details are as follows:

[0035] This embodiment provides a method for preparing a capacitor dielectric ceramic, the method comprising:

[0036] Step (1) synthesizes the main material BaTiO3 by a hydrothermal method, mixes the main material BaTiO3 and modified doping materials (including Dy2O3, MgO, MnO2, CaO, SiO2) according to the formula, and then performs wet ball milling and drying in sequence to obtain the barium titanate-based ceramic dielectric material.

[0037] The barium titanate-based ceramic dielectric material of this embodiment includes the following components by mole percentage:

[0038]

[0039] Step (2) adding a binder to the barium titanate-based ceramic dielectric material as described above, grinding and then subjecting the material to compression molding to obtain a round blank, and sintering the round blank to obtain the capacitor dielectric ceramic.

[0040] Wherein, in step (1), the BaTiO3 powder is a 150-280nm nanoparticle synthesized by a hydrothermal method, and Dy2O3, MgO, MnO2, CaO, and SiO2 are nano-particle reagents of high-grade pure GR.

[0041] Among them, in step (1), the wet ball milling is to mix porcelain material: 3mm zirconium beads: anhydrous ethanol in a mass ratio of 1:1:1.5 and put it into a grinding tank, adjust the parameter process to 480r / min, and continue for 24 hours to evenly stir and mix.

[0042] Wherein, in step (1), the drying is carried out in an oven at 100° C. until the drying is complete.

[0043] Wherein, in step (2), the binder is 8wt% PVA, which is dripped into the barium titanate-based ceramic material at 15wt% and ground and dispersed.

[0044] Among them, in step (2), the compression molding process is 340-380Mpa, the holding time is 20-30s, and the round billet of φ8mm×1.8mm is pressed.

[0045] Among them, in step (2), the sintering process is: heating to 350°C at 1°C / min, keeping warm for 30 minutes to debind, then heating to 600°C at 1°C / min, keeping warm for 30 minutes to debind again, then heating to sintering temperature at 1°C / min, keeping warm for a certain time, and finally cooling to room temperature at 5°C / min.

[0046] Wherein, in step (2), the sintering is carried out in an air atmosphere, or in a reducing atmosphere (1% H2+99% N2) at 1190-1280°C.

[0047] Table 1 Formula table of Example 1

[0048]

[0049] Table 2 Performance test results of Example 1

[0050]

[0051] The prepared sample has a smooth surface, a dense and shrunk structure, a clear grain outline, an obvious granular feel, and a high uniformity of grain size distribution. The prepared capacitor dielectric porcelain material is tested for performance. It can be seen that the room temperature dielectric constant of the capacitor dielectric porcelain material prepared in this embodiment is 1910, the room temperature dielectric loss is 2.1%, and the temperature change rate is within the range of ±22% in the range of -55 to +125°C, which meets the X7S capacitor standard. Figure 1 and Figure 2 shown.

[0052] Example 2

[0053] In this embodiment, the particle size of the main material BaTiO3 powder is 250nm, the sintering temperature in the air atmosphere is 1250°C, the time is 1h, and the furnace is cooled to room temperature. The other process steps involved remain unchanged.

[0054] Table 3 Formula table of Example 2

[0055]

[0056] Table 4 Performance test results of Example 2

[0057]

[0058] The ceramic structure is dense and shrunk, the grain outline is relatively clear, and the grain size distribution is highly uniform. The performance test of the prepared capacitor dielectric ceramic material shows that the room temperature dielectric constant of the capacitor dielectric ceramic material prepared in this embodiment is 2190, the room temperature dielectric loss is 1.31%, and the temperature change rate is within the range of ±22% in the range of -55 to +125°C, which meets the X7S capacitor standard. Figure 3 and Figure 4 shown.

[0059] Example 3

[0060] In this embodiment, the particle size of the main material BaTiO3 powder is 200nm, the sintering temperature in the air atmosphere is 1250°C, the sintering time is 1h, and the other process steps involved remain unchanged.

[0061] Table 5: Formula of Example 3

[0062]

[0063] Table 6 Performance test results of Example 3

[0064]

[0065] The performance test of the prepared capacitor dielectric porcelain shows that the room temperature dielectric constant of the capacitor dielectric porcelain prepared in this embodiment is 2110, the room temperature dielectric loss is 1.10%, the temperature change rate in the range of -55 to +125°C is within the range of ±22%, the temperature stability of the dielectric temperature spectrum at the high temperature end is relatively good, and meets the X7S capacitor standard, such as Figure 5 and Figure 6 shown.

[0066] Those skilled in the art can understand that the above-mentioned embodiments are specific examples for implementing the present application, and in practical applications, various changes can be made to them in form and detail without departing from the spirit and scope of the present application. Any person skilled in the art can make their own changes and modifications without departing from the spirit and scope of the present application, so the scope of protection of the present application shall be based on the scope defined in the claims.

Claims

1. Barium titanate-based ceramic dielectric material, characterized in that: The barium titanate-based ceramic dielectric material uses BaTiO3 as the main material and Dy2O3, MgO, MnO2, CaO and SiO2 as modified doping materials; wherein the addition amount of the main material is 100 mol%, and the total addition amount of the modified doping materials is 6.10 mol% to 9.00 mol%.

2. The barium titanate-based ceramic dielectric material according to claim 1, characterized in that: In the barium titanate-based ceramic dielectric material, the addition amount of Dy2O3 is 0.5mol% to 0.8mol%, the addition amount of MgO is 3.0mol% to 4.6mol%, the addition amount of MnO2 is 0.9mol% to 1.1mol%, the addition amount of CaO is 0.5mol% to 0.7mol%, and the addition amount of SiO2 is 1.2mol% to 1.8mol%.

3. The barium titanate-based ceramic dielectric material according to claim 1, characterized in that: The particle size of the BaTiO3 is 150nm-280nm, and the particle sizes of the Dy2O3, MgO, MnO2, CaO and SiO2 are nano-scale particle reagents.

4. The method for preparing the barium titanate-based ceramic dielectric material according to any one of claims 1 to 3, characterized in that: The method comprises: synthesizing the main material by a hydrothermal method, mixing the main material and a modified doping material, and then sequentially performing wet ball milling treatment and drying treatment to obtain the barium titanate-based ceramic dielectric material.

5. The method for preparing the barium titanate-based ceramic dielectric material according to claim 4, characterized in that: The wet ball milling treatment specifically includes: using 3mm zirconium beads as grinding media, wet milling with anhydrous ethanol, the ball milling speed is 200r / min to 280r / min, and the ball milling time is 12h to 48h.

6. The method for preparing the barium titanate-based ceramic dielectric material according to claim 4, characterized in that: The drying process specifically includes: drying in an oven at 100° C. until the drying is complete.

7. A method for preparing a capacitor dielectric ceramic, characterized in that: The method comprises: adding a binder to the barium titanate-based ceramic dielectric material as claimed in any one of claims 1 to 3, grinding and then performing compression molding to obtain a round blank, and sintering the round blank to obtain the capacitor dielectric ceramic.

8. The method for preparing capacitor dielectric ceramic according to claim 7, characterized in that: The binder is 8wt% PVA, which is dripped into the barium titanate-based ceramic dielectric material at 12wt% to 18wt% for grinding and dispersion; the parameters of the compression molding process are 340Mpa to 380Mpa, the holding time is 20s to 30s, and the round billet of φ8mm×1.8mm is pressed.

9. The method for preparing capacitor dielectric ceramic according to claim 8, characterized in that: The sintering treatment specifically includes: in a sintering atmosphere, in a tubular furnace, heating to a range of 1190°C to 1280°C at 1°C / min to 2°C / min and keeping warm for 1h to 2h, sintering into porcelain, and then cooling to room temperature at 4°C / min to 8°C / min; wherein during the heating process, keeping warm at 300°C and 600°C for 25min to 35min respectively for sufficient debinding; the sintering atmosphere is air or a reducing atmosphere; wherein the reducing atmosphere includes 1% H2 and 99% N2 by volume fraction. 10 . The capacitor dielectric ceramic obtained by the method for preparing the capacitor dielectric ceramic according to claim 7 .

Citation Information

Cited By

  • High-temperature-stability high-dielectric-constant ceramic composition and preparation method thereof

    CN121850646A