Slurry, pole piece with three-dimensional long-range conductive network structure and preparation process and application of pole piece
By optimizing the slurry mixing and dispersion process and adding nonionic surfactant to form a three-dimensional long-range conductive network structure, the problem of poor dispersion stability and uniformity of nanocobalt oxide in the slurry suspension is solved, and lithium is significantly improved The electrical and pulse power performance of ion capacitors.
Patent Information
- Application Number
- CN202411234930.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-09-04
AI Technical Summary
In the electrode preparation process of lithium ion capacitors, the dispersion stability and uniformity of nanocobalt oxide in the slurry suspension are poor, which affects the physical and chemical properties and electrical properties of the electrode sheet, especially under high-rate charging and discharging conditions. Great impact.
By optimizing the slurry mixing and dispersion process, using the dry mixing and kneading stirring strategy, non-ionic surfactants such as OP-10, AES and PAS are added, and the stirring parameters are adjusted, and the stability and dispersion uniformity of the slurry are improved to form a three-dimensional long-range conductive network The structure of the extreme piece.
The preparation of high uniformity and high stability slurry is achieved. The electrode sheet shows strong peel strength, low resistivity and excellent three-dimensional conductive network structure, which improves the electrical performance and pulse power performance of lithium-ion capacitors.
Smart Images

Figure CN118942926A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of electrochemical energy storage, and in particular relates to a slurry, a pole piece with a three-dimensional long-range conductive network structure, and a preparation process and application thereof. Background Art
[0002] Lithium-ion capacitors are a new type of electrochemical energy storage device with relatively higher specific power compared to lithium-ion batteries and relatively higher specific energy compared to supercapacitors. Therefore, lithium-ion capacitors that have the advantages of both lithium-ion batteries and supercapacitors have received widespread attention.
[0003] Since lithium-ion capacitors must have both high specific energy and high specific power, lithium-ion capacitors have high requirements for electrode preparation technology: (1) There should not be too many closed pores and complex pore structures in the electrode coating; (2) The dispersion uniformity of the slurry should be relatively stable, otherwise it will affect the consistency of the electrode, the stability of continuous coating (resistivity, porosity, coating load) and the power characteristics of the capacitor. Therefore, in order for lithium-ion capacitors to quickly enter the market and be widely used in the market, it is necessary to conduct in-depth research on the electrode preparation process of lithium-ion capacitors to solve the above problems. Among them, the mixing and dispersion process of lithium-ion capacitor slurry determines the physical and chemical properties of the electrode, so it puts forward high requirements for the pulping process. Among them, the pulping process will affect the distribution state of active substances and inactive substances in the electrode coating, pore distribution, pore structure, conductive network structure, coating stability, etc., thereby having a greater impact on the diffusion rate of lithium ions in the positive electrode, especially under high-rate charge and discharge conditions. It is more obvious, and its impact on electrical performance exceeds 30%. However, the nano-lithium cobalt oxide (LCO) currently used in lithium-ion capacitors has poor dispersion stability and uniformity in the slurry suspension, which is a common problem in the industry and there is currently no better process strategy. Summary of the invention
[0004] Based on the problems existing in the prior art, the present invention optimizes the slurry mixing and dispersion process, obtains a high-uniformity and high-stability slurry dispersion process suitable for industrial production, prepares a pole piece with a three-dimensional long-range conductive network structure, and establishes the relationship between the stirring strategy, slurry dispersion stability, electrode sheet conductive network structure and the electrical properties of lithium-ion capacitors. Compared with the traditional slurry preparation process, the prepared pole piece exhibits strong peel strength, low resistivity and excellent three-dimensional conductive network structure.
[0005] In the first aspect, a slurry preparation process in this scheme includes the following preparation steps:
[0006] S1. Prepare the raw materials for the slurry: including nano lithium cobalt oxide, activated carbon, conductive agent, polyvinylidene fluoride and N-methyl-2-pyrrolidone solvent, and divide the N-methyl-2-pyrrolidone solvent into two parts for standby use;
[0007] S2, mixing: using a dry mixing method to uniformly mix the nano lithium cobalt oxide, activated carbon, conductive agent and polyvinylidene fluoride to obtain a primary mixture;
[0008] S3, kneading: adding a portion of the N-methyl-2-pyrrolidone solvent to the primary mixture obtained in S2 and mixing again to obtain a mixture;
[0009] S4, dispersion: add another portion of the N-methyl-2-pyrrolidone solvent to the mixture obtained in S3, mix well, then add appropriate amounts of dodecylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether sodium sulfate and monolauryl phthalate, and mix well again to obtain the slurry.
[0010] Furthermore, the mass ratio of the nano lithium cobalt oxide, activated carbon, conductive agent and polyvinylidene fluoride is 85:9:3:3.
[0011] Furthermore, the conductive agent includes a mixture of an SP conductive agent and a CNT conductive agent in a mass ratio of 2:1.
[0012] Furthermore, in S2, the nano lithium cobaltate, activated carbon, conductive agent and polyvinylidene fluoride are mixed twice, the time interval between the two feedings is 30 to 60 minutes, and the stirring rates during the feedings are 30 to 50 rpm and 500 to 800 rpm respectively. After all the powders are added to the agitator, dry mixing is performed at a rate of 30 to 50 rpm and 4000 to 6000 rpm for 60 to 80 minutes.
[0013] Further, in S3, an appropriate amount of N-methyl-2-pyrrolidone solvent is added to the initial mixture of S2, and the solid content is 70% to 75% at this time, and the mixture is first stirred at 30 to 50 rpm and 500 to 700 rpm for 10 to 30 minutes, and then stirred at 70 to 90 rpm and 3000 to 4000 rpm for 4 to 7 hours. The solid content refers to the weight proportion of all powders in the mixture system of this step.
[0014] Further, in S4, the remaining N-methyl-2-pyrrolidone solvent is added to the mixture obtained in S3 twice, at which time the final solid content is 50% to 55%, the interval between the two additions is 30 to 60 minutes, and the stirring rate during the addition is 70 to 90 rpm and 2000 to 3000 rpm.
[0015] Furthermore, after all the N-methyl-2-pyrrolidone solvent is added to S4, dodecylphenol polyoxyethylene ether, sodium fatty alcohol polyoxyethylene ether sulfate and monolauryl phthalate are added, and the mixture is dispersed at a high speed at a stirring rate of 50-70 rpm and 4000-5000 rpm for 3-5 hours.
[0016] Furthermore, the dodecylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether sodium sulfate and monolauryl phthalate account for 0.4% of the solid content. In a second aspect, the present invention also provides a pole piece with a three-dimensional long-range conductive network structure, wherein the pole piece is obtained by uniformly coating the slurry prepared by the process described in the first aspect on an aluminum foil, drying it, pressing it into a sheet and cutting it.
[0017] In a third aspect, a pole piece having a three-dimensional long-range conductive network structure prepared by the present invention is used for preparing a lithium ion capacitor.
[0018] For lithium ion capacitors, the introduction of activated carbon in the positive electrode formula can bring out the performance of double-layer capacitors, thereby improving the specific power of hybrid capacitors. However, compared with positive electrode active materials such as lithium cobalt oxide, activated carbon (AC) and conductive agents (SP, CNT) have larger specific surface area, lower density, larger particle diameter, and complex pore structure, which will greatly affect the preparation process and stability of electrode slurry. The present invention is mainly aimed at the technical defects of poor dispersion stability and uniformity of nano lithium cobalt oxide (LCO) in slurry suspension in the prior art, and solves the problem of poor slurry stability and dispersion uniformity by optimizing the slurry preparation process, adding the selected non-ionic surfactant, and determining the addition ratio. Therefore, on the basis of the battery type slurry preparation process, the present invention further studies the influence of the stirring process parameters of the composite slurry on its uniformity and stability, constructs the influence law of the slurry stirring process parameters on the slurry stability and consistency, and provides guidance for the preparation of nano lithium cobalt oxide slurry.
[0019] The present invention aims at the deficiencies of the prior art, optimizes the slurry mixing and dispersing process, and obtains a high-uniformity and high-stability positive electrode material dispersion process suitable for industrial production. By adding OP-10 (dodecylphenol polyoxyethylene ether), AES (fatty alcohol polyoxyethylene ether sodium sulfate) and PAS (monolauryl phthalate) non-charged nonionic surfactants at the end of the dispersion step, it has good wettability and mild surface activity, can significantly reduce the interaction between the van der Waals force and hydrogen bonds between particles in the suspension, so that the stability and dispersion uniformity of the suspension are significantly improved, and finally achieve the purpose of constructing a pole piece with a three-dimensional long-range conductive network structure.
[0020] The slurry prepared by the present invention is used to prepare pole pieces, and the conductive agent forms a sponge-like three-dimensional conductive network structure on the pole piece surface and between particle gaps, indicating that the slurry coating prepared under the process conditions does not undergo obvious migration and agglomeration of the conductive agent and the binder during the coating and drying process.
[0021] The impedance spectrum of the electrode prepared by the obtained slurry has a higher slope in the low-frequency region, showing relatively good capacitance performance, indicating that the electrode ion diffusion resistance prepared by this process is relatively small. Combining the above advantages, the electrode presents relatively optimal pulse power performance and peeling strength, and the overall performance of the electrode is improved.
[0022] The method of the present invention establishes the relationship between dry mixing and kneading stirring strategy, slurry dispersion stability, electrode sheet conductive network structure and lithium ion capacitor electrical performance. Compared with the traditional slurry preparation process, the electrode sheet prepared by the slurry obtained by the present invention exhibits strong peel strength, low resistivity and excellent three-dimensional conductive network structure. The electrode sheet with the three-dimensional long-range conductive network structure has excellent ionic and electronic conductivity and exhibits a good ion migration rate. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 From left to right are the contact angle test results of the slurries obtained by the three processes of Comparative Example 1, Example 1 and Comparative Example 2;
[0024] Figure 2 From left to right are SEM images of pole pieces prepared by the slurries obtained by the three processes of Comparative Example 1, Comparative Example 2 and Example 1;
[0025] Figure 3 The impedance test spectrum of the electrode sheets prepared by the slurries obtained by the three processes of Example 1, Comparative Example 1 and Comparative Example 2, in which strategy A corresponds to Example 1, strategy B corresponds to Comparative Example 1, and strategy C corresponds to Comparative Example 2;
[0026] Figure 4 The pulse power test of the electrode sheets prepared by the slurries obtained by the three processes of Example 1, Comparative Example 1 and Comparative Example 2; in the figure, strategy A corresponds to Example 1, strategy B corresponds to Comparative Example 1, and strategy C corresponds to Comparative Example 2;
[0027] Figure 5 The peeling force test curves of the electrodes prepared by the slurries obtained by the three processes of Example 1, Comparative Example 1 and Comparative Example 2 are shown. In the figure, strategy A corresponds to Example 1, strategy B corresponds to Comparative Example 1, and strategy C corresponds to Comparative Example 2. DETAILED DESCRIPTION
[0028] The following is further described in detail through specific implementation methods:
[0029] In the following processes, all stirring steps are carried out using a planetary stirrer.
[0030] Embodiment 1: A process for preparing a slurry, comprising the following steps:
[0031] S1. Prepare raw materials for slurry: the raw materials include nano lithium cobalt oxide (LCO), activated carbon (AC), conductive agent (including a mixture of SP conductive agent and CNT conductive agent in a mass ratio of 2:1), polyvinylidene fluoride (PVDF) and N-methyl-2-pyrrolidone (NMP) solvent. All materials are divided into two parts for standby use, among which the mass ratio of LCO, AC, conductive agent and polyvinylidene fluoride is 85:9:3:3.
[0032] S2. Dry mixing: LCO, activated carbon (AC), conductive agent and PVDF were added into the mixer twice for dry mixing. The time interval between the two additions was 30 min. The stirring rates during the additions were 30 rpm and 500 rpm respectively. After all the powders were added into the mixer, dry mixing was performed at 30 rpm and 4000 rpm for 60 min.
[0033] S3, kneading: Add NMP to the mixed powder, at which time the solid content of the mixed components is 70%, first stir at 30 rpm and 500 rpm for 10 min, and then stir at 70 rpm and 3000 rpm for 4 h.
[0034] S4, dispersion: the remaining NMP solvent is added twice, the interval between the two times is 30min, and the stirring speed during the addition is 70rpm and 3000rpm. After the NMP solvent is fully added, the final solid content is 50%, and then an appropriate amount of non-ionic surfactant is added to the dispersion, the non-ionic surfactant is a mixed component of OP-10 (dodecylphenol polyoxyethylene ether), AES (fatty alcohol polyoxyethylene ether sodium sulfate) and PAS (monolauryl phthalate), and the non-ionic surfactant accounts for 0.4% of the solid content, and the high-speed dispersion is carried out at a stirring speed of 70rpm and 4000rpm for 3h.
[0035] Comparative Example 1: Process flow of wet mixing and stirring strategy for making glue:
[0036] (1) Preparation of gel: Dissolve all PVDF in NMP. Stir at 30 rpm and 500 rpm for 15 min, then stir at 45 rpm and 2000 rpm for 4 h.
[0037] (2) Mixing: Add LCO, CNTs and SP into the glue solution at once. Stir at 30 rpm and 500 rpm for 10 min, then knead at 70 rpm and 3000 rpm for 4 h.
[0038] (3) Dispersion: Add NMP (final solid content is 50%) to the above slurry and disperse at high speeds of 60 rpm and 3000 rpm for 3 h.
[0039] Comparative Example 2: Process flow of wet mixing and stirring strategy for making glue:
[0040] (1) Preparation of gel: Dissolve all PVDF in NMP. Stir at 40 rpm and 700 rpm for 25 min, then stir at 50 rpm and 3000 rpm for 5 h.
[0041] (2) Mixing: Add LCO, CNTs and SP into the glue solution at once. Stir at 40 rpm and 600 rpm for 20 min, then knead at 60 rpm and 2500 rpm for 5 h.
[0042] (3) Dispersion: Add NMP (final solid content 53%) to the above slurry and disperse at high speeds of 70 rpm and 4000 rpm for 3 h.
[0043] Figure 1 From left to right are the contact angle test results of the slurries obtained by the three processes of Comparative Example 1, Example 1 and Comparative Example 2. Figure 1 It can be seen that the slurry suspension prepared in Example 1 has the smallest contact angle on the aluminum foil surface, which is 63.5°, showing the best wettability. The better the wettability, the stronger the bonding force between the slurry and the current collector, and the lower the influence of surface tension on the slurry coating during the drying process, that is, the binder migration and thick edge problems of the coating during the baking process will be significantly improved. Therefore, the suspension prepared in Example 1 is more conducive to the coating stability during the preparation of the pole piece.
[0044] Comparative Example 3: The slurry preparation process is different from that of Comparative Example 1 in that, after NMP is added and mixed in the dispersion step, the same nonionic surfactant as in Example 1 is added.
[0045] Example 2: Preparation of pole pieces. The slurries obtained in Example, Comparative Example 1, Comparative Example 2, and Comparative Example 3 are used to prepare pole pieces in the same manner. The specific preparation method is as follows:
[0046] The prepared slurry was evenly coated on a 12 μm aluminum foil, and then dried in a vacuum drying oven at 140° C. for 72 h, and then pressed into sheets using a tablet press, and finally the electrode sheet was cut into electrode sheets.
[0047] Figure 2 From left to right in the figure are SEM images of the pole pieces prepared by the slurries obtained by the three processes of Comparative Example 1, Comparative Example 2 and Example 1. Figure 2It can be seen that there are many large pores between the active material particles on the surface of the pole pieces prepared by the slurries of Comparative Examples 1 and 2, and no long-range conductive network structure coated with a conductive agent is formed between the particles. The pore structure on the surface of the pole piece is not conducive to the rapid transmission of electrons and cannot meet the performance requirements of large current pulse discharge. For the pole piece prepared by the slurry of Example 1, the conductive agent forms a sponge-like three-dimensional conductive network structure on the surface of the pole piece and between the particle gaps, that is, the slurry coating prepared under this process condition does not undergo obvious migration and agglomeration of the conductive agent and the binder during the coating and drying process.
[0048] from Figure 3 It can be seen that the electrode impedance spectrum prepared by the slurry of Example 1 has a higher slope in the low-frequency region, showing relatively good capacitance performance, indicating that the electrode ion diffusion resistance prepared by this process is relatively small.
[0049] from Figure 4 It can be seen that the electrode prepared by the slurry of Example 1 exhibits the highest pulse power (4312.5W), while the electrode prepared by Comparative Example 1 and Comparative Example 2 have relatively poor pulse power performance. Instantaneous high-power pulse discharge is mainly determined by the porosity of the electrode, the resistivity of the electrode and other indicators. The electrode prepared by the slurry of Example 1 exhibits the best pulse power performance.
[0050] The present invention conducted resistivity test, limit pulse power test and peel strength test on the pole pieces prepared by the slurries of Example 1, Comparative Example 3 and Comparative Example 4, and the test results are shown in Tables 1, 2 and 3. It can be seen from the test results that the pole piece prepared by the slurry of Example 1 shows relatively excellent comprehensive performance compared with the pole piece prepared by the slurry of Comparative Example 3.
[0051] Table 1 Electrode resistivity test
[0052] Group Internal resistance(mΩ) Comparative Example 3 1.21 Example 1 1.03
[0053] Table 2 Pole piece limit pulse power test
[0054] Group Power (W, 2000A) Comparative Example 3 3910.4 Example 1 4312.5
[0055] Table 3 Pole peel strength test
[0056] Group N Comparative Example 3 0.78 Example 1 1.92
[0057] The present invention tests and analyzes the bonding strength between the electrode coating and the current collector. The peeling effect is as follows Figure 5As shown in the figure below, the peeling force data results show that the electrode prepared by the slurry of Example 1 shows a relatively maximum peeling force of 1.92N, while the electrode prepared by the slurry of Comparative Example 3 has a peeling force less than that of the electrode prepared by the slurry of Example 1.
[0058] Example 3: Preparation of soft-pack lithium ion capacitors:
[0059] The assembly of the soft-pack laminated lithium-ion capacitor is carried out in a drying room. First, 20 lithium cobalt oxide / activated carbon pole pieces (pole pieces prepared from the slurry obtained in Example 1) and 21 hard carbon pole pieces (N:P=1.3, hard carbon mass fraction of 94%) are taken as positive and negative electrodes respectively. The diaphragm adopts a polypropylene diaphragm, and the electrolyte is an organic electrolyte (1 mol / L LiPF6, EC:PC:DMC volume ratio is 1:1:1). Then, the soft-pack lithium-ion capacitor is laminated, and the shape is designed to be rectangular.
Claims
1. A process for preparing a slurry, characterized in that The preparation steps involved are as follows: S1. Prepare the raw materials for the slurry: including nano lithium cobalt oxide, activated carbon, conductive agent, polyvinylidene fluoride and N-methyl-2-pyrrolidone solvent, and divide the N-methyl-2-pyrrolidone solvent into two parts for standby use; S2, mixing: using a dry mixing method to uniformly mix the nano lithium cobalt oxide, activated carbon, conductive agent and polyvinylidene fluoride to obtain a primary mixture; S3, kneading: adding a portion of the N-methyl-2-pyrrolidone solvent to the primary mixture obtained in S2 and mixing again to obtain a mixture; S4, dispersion: add another portion of the N-methyl-2-pyrrolidone solvent to the mixture obtained in S3, mix well, then add appropriate amounts of dodecylphenol polyoxyethylene ether, fatty alcohol polyoxyethylene ether sodium sulfate and monolauryl phthalate, and mix well again to obtain the slurry.
2. A process for preparing a slurry according to claim 1, characterized in that: The mass ratio of the nano lithium cobalt oxide, activated carbon, conductive agent and polyvinylidene fluoride is 85:9:3:
3.
3. The process for preparing a slurry according to claim 2, characterized in that: The conductive agent includes a mixture of an SP conductive agent and a CNT conductive agent in a mass ratio of 2:
1.
4. The process for preparing a slurry according to claim 1, characterized in that: In S2, the nano lithium cobaltate, activated carbon, conductive agent and polyvinylidene fluoride are mixed twice, the time interval between the two feedings is 30 to 60 minutes, and the stirring rates during the feedings are 30 to 50 rpm and 500 to 800 rpm respectively. After all the powders are added to the agitator, dry mixing is performed at a rate of 30 to 50 rpm and 4000 to 6000 rpm for 60 to 80 minutes.
5. The process for preparing a slurry according to claim 4, characterized in that: The S3, add an appropriate amount of N-methyl-2-pyrrolidone solvent to the initial mixture of S2, at which time the solid content is 70% to 75%, first stir at 30 to 50 rpm, 500 to 700 rpm for 10 to 30 minutes, and then stir at 70 to 90 rpm, 3000 to 4000 rpm for 4 to 7 hours.
6. The process for preparing a slurry according to claim 5, characterized in that: In the step S4, the remaining N-methyl-2-pyrrolidone solvent is added to the mixture obtained in step S3 twice, and the final solid content is 50% to 55%. The interval between the two additions is 30 to 60 minutes, and the stirring speed during the addition is 70 to 90 rpm and 2000 to 3000 rpm.
7. The process for preparing a slurry according to claim 6, characterized in that: After all the N-methyl-2-pyrrolidone solvent is added to S4, dodecylphenol polyoxyethylene ether, sodium fatty alcohol polyoxyethylene ether sulfate and monolauryl phthalate are added, and high-speed dispersion is carried out for 3 to 5 hours at a stirring rate of 50 to 70 rpm and 4000 to 5000 rpm; the dodecylphenol polyoxyethylene ether, sodium fatty alcohol polyoxyethylene ether sulfate and monolauryl phthalate account for 0.4% of the solid content.
8. A slurry, characterized in that: The invention is prepared by the preparation process described in any one of claims 1 to 7.
9. A pole piece having a three-dimensional long-range conductive network structure, characterized in that: The pole piece is obtained by uniformly coating the slurry described in claim 8 on aluminum foil, and then pressing and cutting the resulting foil after drying.
10. The electrode having a three-dimensional long-range conductive network structure according to claim 9 is used for preparing a lithium ion capacitor.
Citation Information
Patent Citations
Three-dimensional nano composite electrode material for electrochemical energy storage and preparation method thereof
CN110415994A
Method of preparing supercapacitor slurry and supercapacitor prepared using same
CN110459410A
Nonaqueous electric double layer capacitor and method of producing cell using the same
JP1999329904A