Method for forming cobalt-titanium silicide layer and preparation method of semiconductor structure

By sputtering cobalt-titanium alloy on the silicon layer and performing rapid heat treatment, the cobalt-titanium silicide layer is formed, which solves the problems of excessive silicon growth and high defect rate caused by cobalt oxidation, simplifies the process flow and reduces the contact resistance.

CN118943010APending Publication Date: 2024-11-12CHENGDU HIGH-TECH JIN SCI&TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410541844.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-04-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

In the prior art, cobalt oxidation leads to problems such as excessive silicon growth and high defect rate of silicide layer and increased process complexity.

Method used

Using cobalt titanium alloy as the target material, the cobalt titanium layer is sputtered on the silicon layer, and the cobalt titanium silicide layer is formed through rapid heat treatment, simplifying the process flow, avoiding sputtering of multi-layer metal or metal nitride layers, and improving phase stability .

Benefits of technology

The defect rate and contact resistance of the silicide layer are reduced, the heat treatment process is simplified, the phase stability of the cobalt titanium silicide layer is improved, and the defects caused by phase instability are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943010A_ABST
    Figure CN118943010A_ABST
Patent Text Reader

Abstract

The invention relates to a method for forming a cobalt-titanium silicide layer and a preparation method of a semiconductor structure. The invention relates to a method for forming a cobalt-titanium silicide layer, which comprises the following steps of: sputtering a cobalt-titanium layer on a silicon layer by taking a cobalt-titanium alloy as a target material; and heating the cobalt-titanium layer by using a rapid heat treatment method to convert the cobalt-titanium layer into the cobalt-titanium silicide layer. According to the invention, the problem of silicon overgrowth caused by cobalt oxidation is solved, and the defect rate of the silicide layer is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of semiconductor manufacturing technology, and in particular to a method for forming a cobalt-titanium silicide layer and a method for preparing a semiconductor structure. Background Art

[0002] Among the factors that determine device performance, contact resistance is one of the issues that must be addressed. Currently, in order to reduce contact resistance, a subsequent heat treatment is performed after depositing a metal layer in the contact area to form a silicide, which is an alloy form of metal and silicon. Metal silicide can significantly reduce defects at the metal-silicon interface, reduce the Schottky barrier, and drive doped atoms (dopants) to the interface. The more common metal silicides include cobalt silicide, titanium silicide, and the like. In the prior art, the following method is usually used to form cobalt / titanium silicide: first, a Si / Co / TiN stacked structure (such as a cobalt film 2 and a titanium nitride 3 (TiN) film) is formed on a silicon layer 1. Figure 1 ); then two rapid heat treatments are performed to form cobalt / titanium silicide and remove the remaining metal layer that has not formed silicide. In this method, although the addition of the titanium nitride film prevents the disordered flow of cobalt during heat treatment, the following problems still exist: on the one hand, the easily oxidized cobalt will cause excessive growth of silicon in the subsequent high-temperature process, thereby causing defects; on the other hand, the deposited film layers are more, which increases the complexity of the process.

[0003] To this end, the present invention is proposed. Summary of the invention

[0004] The main purpose of the present invention is to provide a method for forming a cobalt-titanium silicide layer and a method for preparing a semiconductor structure, which solves the problem of excessive silicon growth caused by cobalt oxidation and reduces the defect rate of the silicide layer.

[0005] In order to achieve the above objectives, the present invention provides the following technical solutions.

[0006] A first aspect of the present invention provides a method for forming a cobalt-titanium silicide layer, comprising the following steps:

[0007] Using cobalt-titanium alloy as a target, a cobalt-titanium layer is sputtered on the silicon layer;

[0008] The cobalt-titanium layer is heated by a rapid thermal process to transform it into a cobalt-titanium silicide layer.

[0009] Therefore, the present invention obtains the alloy layer by sputtering the alloy target material once, thus avoiding sputtering of multiple metal or metal nitride layers and simplifying the process.

[0010] On the other hand, because cobalt and titanium synergistically form polymetallic silicide, its phase stability is significantly improved compared to cobalt silicide. Even in narrow linewidth devices, the formation of silicide will not show abnormal overgrowth, thereby reducing the defect rate caused by phase instability.

[0011] On the other hand, the method of the present invention does not require the addition of an additional protective film, thereby simplifying the heat treatment process.

[0012] On this basis, the following improvements can be made.

[0013] Further, after the conversion into the cobalt titanium silicide layer, the method further comprises:

[0014] The unreacted cobalt and titanium are removed by wet etching.

[0015] Furthermore, the sputtering is performed under vacuum conditions.

[0016] Furthermore, the sputtering adopts an alternating current power supply.

[0017] Furthermore, the temperature of heating the cobalt-titanium layer by rapid thermal processing is 500-800°C.

[0018] A second aspect of the present invention provides a method for preparing a semiconductor structure, comprising:

[0019] Forming a source electrode, a drain electrode and a gate electrode on a substrate, wherein the surface layers of the source electrode, the drain electrode and the gate electrode are silicon;

[0020] Using cobalt-titanium alloy as a target material, sputtering cobalt-titanium layers on the surfaces of the source electrode, the drain electrode and the gate electrode respectively;

[0021] The cobalt-titanium layer is heated by a rapid thermal process to transform it into a cobalt-titanium silicide layer.

[0022] Therefore, the present invention forms a cobalt-titanium silicide layer in the conductive contact area of ​​each electrode using the above method, which can significantly reduce the contact resistance of each electrode.

[0023] Furthermore, the cobalt-titanium layers on the surfaces of the source, drain and gate are formed by synchronous sputtering.

[0024] Furthermore, the sputtering is performed under vacuum conditions.

[0025] Furthermore, the sputtering adopts an alternating current power supply.

[0026] Furthermore, the semiconductor device includes at least one of a transistor, a memory, a display screen, and a detector.

[0027] In summary, compared with the prior art, the present invention achieves the following technical effects: it simplifies the process of forming a cobalt-titanium silicide layer, improves the phase stability of the silicide layer, thereby reducing the defect rate and reducing the contact resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Various other advantages and benefits will become apparent to those of ordinary skill in the art by reading the following detailed description of the preferred embodiment.The drawings are only for the purpose of illustrating the preferred embodiments and are not to be construed as limiting the invention.

[0029] Figure 1 A schematic diagram of a stacked structure formed when preparing a silicide layer in the prior art;

[0030] Figure 2 A flow chart of a method for forming a cobalt-titanium silicide layer provided by the present invention;

[0031] Figures 3 to 5 The present invention provides a schematic structural diagram of each step in a method for forming a cobalt-titanium silicide layer on a semiconductor structure.

[0032] Reference numerals:

[0033] Silicon layer-1, cobalt film-2, titanium nitride-3;

[0034] Source-21, drain-22, gate-23;

[0035] Cobalt titanium layer-211, cobalt titanium layer-221, cobalt titanium layer-231;

[0036] Cobalt titanium silicide layer-212, cobalt titanium silicide layer-222, cobalt titanium silicide layer-232. DETAILED DESCRIPTION

[0037] Hereinafter, embodiments of the present disclosure will be described with reference to the accompanying drawings. However, it should be understood that these descriptions are exemplary only and are not intended to limit the scope of the present disclosure. In addition, in the following description, descriptions of well-known structures and technologies are omitted to avoid unnecessary confusion of the concepts of the present disclosure.

[0038] Various structural schematic diagrams according to embodiments of the present disclosure are shown in the accompanying drawings. These figures are not drawn to scale, and some details are magnified and some details may be omitted for the purpose of clear expression. The shapes of various regions and layers shown in the figures and the relative sizes and positional relationships therebetween are only exemplary, and may deviate in practice due to manufacturing tolerances or technical limitations, and those skilled in the art may further design regions / layers with different shapes, sizes, and relative positions according to actual needs.

[0039] In the context of the present disclosure, when a layer / element is referred to as being "on" another layer / element, the layer / element may be directly on the other layer / element or an intervening layer / element may exist therebetween. In addition, if a layer / element is "on" another layer / element in one orientation, the layer / element may be "below" the other layer / element when the orientation is reversed.

[0040] In the manufacturing process of transistors, memory, display screens, and detectors, when contacting and wiring each electrode, in order to reduce the contact resistance, silicide treatment is usually performed in the contact area, that is, a metal silicide layer is formed. The more common treatment method is to form a stack of multiple different metals to maximize their strengths and minimize their weaknesses. Taking cobalt titanium as an example, the above method does not fundamentally solve the problem of poor phase stability of cobalt silicide, and the multi-layer deposition increases the process complexity, affecting production efficiency.

[0041] To this end, the present invention provides a method for forming a cobalt-titanium silicide layer, such as Figure 2 As shown, it includes the following steps:

[0042] Step S1, using cobalt-titanium alloy as a target, sputtering a cobalt-titanium layer on the silicon layer.

[0043] Step S2, heating the cobalt-titanium layer by rapid thermal processing to transform it into a cobalt-titanium silicide layer.

[0044] The above method has the following characteristics.

[0045] On the one hand, the alloy target is used to obtain the alloy layer by sputtering it once, thus avoiding the sputtering of multiple metal or metal nitride layers and simplifying the process.

[0046] On the other hand, because cobalt and titanium synergistically form polymetallic silicide, its phase stability is significantly improved compared to cobalt silicide. Even in narrow linewidth devices, the formation of silicide will not show abnormal overgrowth, thereby reducing the defect rate caused by phase instability.

[0047] On the other hand, the method of the present invention does not require the addition of an additional protective film, thereby simplifying the heat treatment process.

[0048] In order to further reduce the contact resistance, it is also necessary to remove the metal that undergoes the silicidation reaction. Therefore, in some embodiments, Figure 2 As shown, after step S2, it also includes:

[0049] Step S3, removing unreacted cobalt and titanium by wet etching.

[0050] The sputtering in step S1 can be performed under vacuum conditions, and the sputtering can use an AC power supply.

[0051] The silicon layer in step S1 can be single crystal silicon or polycrystalline silicon, and is usually a film layer in a semiconductor device that needs to lead out wires to connect to a power source, including but not limited to a source, a drain, a gate, a cathode, an anode, and the like.

[0052] The temperature of heating the cobalt-titanium layer by the rapid thermal treatment method in step S2 can be 500-800° C. The thermal treatment in this step can include one or more thermal treatments, and the temperatures of the multiple thermal treatments can be the same or different. The purpose of the multiple thermal treatments is to transform the cobalt-titanium silicide into a phase with lower resistance.

[0053] The present invention also provides a method for silicidation in a semiconductor structure containing a transistor, specifically, comprising the following steps:

[0054] The first step, such as Figure 3 As shown, a source electrode 21, a drain electrode 22 and a gate electrode 23 are formed on a substrate. Usually, the surface layers of the source electrode 21, the drain electrode 22 and the gate electrode 23 are silicon. Figure 1 Taking a traditional planar transistor as an example, the present invention is not limited thereto, and may also be a fin field effect transistor FinFET or a gate-all-around transistor GAAFET, etc. The surface layers of the source, drain, and gate include silicon, which means that these structures may be a single-layer structure containing only silicon, or a stacked structure of silicon and metal or other semiconductors stacked together.

[0055] In the second step, a cobalt-titanium alloy is used as a target material to sputter a cobalt-titanium layer on the surface of the source electrode 21, the drain electrode 22 and the gate electrode 23, respectively. Figure 4 As shown, they are cobalt-titanium layer 211 , cobalt-titanium layer 221 , and cobalt-titanium layer 231 , respectively.

[0056] In this step, the cobalt-titanium layer on the surface of the source, drain and gate is formed by synchronous sputtering, that is, it can be realized by using the self-aligned silicide method (SALICIDE). The sputtering in this step can be carried out under vacuum conditions and can use an AC power supply.

[0057] In the third step, the cobalt-titanium layer is heated by a rapid thermal process to transform it into a cobalt-titanium silicide layer, such as Figure 5 As shown, they are respectively cobalt titanium silicide layer 212, cobalt titanium silicide layer 222, and cobalt titanium silicide layer 232. Similarly, this step can also be completed simultaneously.

[0058] Therefore, the above embodiment forms a cobalt-titanium silicide layer in the conductive contact region of each electrode, which can significantly reduce the contact resistance of each electrode.

[0059] The embodiments of the present disclosure are described above. However, these embodiments are for illustrative purposes only and are not intended to limit the scope of the present disclosure. The scope of the present disclosure is defined by the appended claims and their equivalents. Without departing from the scope of the present disclosure, a person skilled in the art may make a variety of substitutions and modifications, which should all fall within the scope of the present disclosure.

Claims

1. A method for forming a cobalt-titanium silicide layer, characterized in that: The following steps are involved: Using cobalt-titanium alloy as a target, a cobalt-titanium layer is sputtered on the silicon layer; The cobalt-titanium layer is heated by a rapid thermal process to transform it into a cobalt-titanium silicide layer.

2. The method according to claim 1, characterized in that After the transformation into the cobalt titanium silicide layer, it also includes: The unreacted cobalt and titanium are removed by wet etching.

3. The method according to claim 1, characterized in that The sputtering is performed under vacuum conditions.

4. The method according to claim 1 or 3, characterized in that: The sputtering adopts an alternating current power supply.

5. The method according to claim 1, characterized in that The temperature of heating the cobalt-titanium layer by rapid thermal processing is 500-800°C.

6. A method for preparing a semiconductor structure, characterized in that: include: Forming a source electrode, a drain electrode and a gate electrode on a substrate, wherein the surface layers of the source electrode, the drain electrode and the gate electrode are silicon; Using cobalt-titanium alloy as a target material, sputtering cobalt-titanium layers on the surfaces of the source electrode, the drain electrode and the gate electrode respectively; The cobalt-titanium layer is heated by a rapid thermal process to transform it into a cobalt-titanium silicide layer.

7. The method according to claim 6, characterized in that The cobalt-titanium layers on the surfaces of the source electrode, the drain electrode and the gate electrode are formed by synchronous sputtering.

8. The method according to claim 6, characterized in that The sputtering is performed under vacuum conditions.

9. The method according to claim 6, characterized in that The sputtering adopts an alternating current power supply.

10. The method according to claim 6, characterized in that The semiconductor device includes at least one of a transistor, a memory, a display screen, and a detector.