Wafer structure and method for improving electrostatic adsorption capacity of high-resistance wafer

Through the bonding connection between high-resistance wafer and low-resistance wafer, hydrophilic bonding is used to improve the electrostatic adsorption capacity of high-resistance wafers at room temperature, solving the problem of insufficient adsorption capacity of high-resistance wafers and reducing production cycle and cost, and avoid the defects of high temperature processes.

CN118943146APending Publication Date: 2024-11-12JC INNOVATIVE SEMICON SUBSTRATE TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411019163.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The adsorption force of high-resistance wafers in the electrostatic suction cup is insufficient, resulting in the risk of chip drop. The existing methods require changing the wafer structure or conducting high-temperature processes, resulting in waste of costs and resources.

Method used

By bonding high resistance wafers to low resistance wafers, temporary bonding of heterogeneous materials is achieved at room temperature using hydrophilic bonding, reducing production cycles, and debonding and reusing low resistance wafers.

Benefits of technology

It improves the electrostatic adsorption capacity of high-resistance wafers, reduces production cycle and cost, avoids the defects of elemental contamination and high-temperature processes, and is suitable for large-scale production and small-scale experimental research and development.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943146A_ABST
    Figure CN118943146A_ABST
Patent Text Reader

Abstract

The invention provides a wafer structure and method for improving the electrostatic adsorption capacity of a high-resistance wafer, and the wafer structure comprises the high-resistance wafer and a low-resistance wafer disposed at one side of the high-resistance wafer, and the high-resistance wafer is in bonding connection with the low-resistance wafer. And the resistance value of the low-resistance wafer is less than 3000 ohm. Cm. According to the wafer structure and the method, annealing is not needed to increase the bonding force, the requirement of electrostatic chuck equipment in the next procedure can be directly met, temporary bonding of heterogeneous materials can be achieved at the room temperature, and the production period is greatly shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the field of semiconductor manufacturing and relates to a wafer structure and method for improving the electrostatic adsorption capability of a high-resistance wafer. Background Art

[0002] With the rapid development of the semiconductor industry, the most commonly used single-crystal silicon material can no longer meet market demand. For example, in the SOI field, very high-resistance materials are required, such as high-resistance silicon (>3000 ohm.cm). In the POI composite substrate field, lithium niobate and lithium tantalate wafers are used. In the SiC composite substrate field, semi-insulating SiC and common quartz wafers are used. These materials cannot be held by electrostatic chucks. High-resistance wafers pose a significant challenge to the electrostatic chuck used in tool processing. Excessive resistance can lead to insufficient holding force of the electrostatic chuck, resulting in a high risk of wafer drop and fragmentation during the process, significantly impacting the stable operation of the tool. For example, in the ion implantation process, an automated robot transfers the wafer to the electrostatic chuck in the vacuum chamber. The electrostatic chuck holds the wafer for the ion implantation process. However, the weak holding force of the electrostatic chuck on high-resistance wafers can cause tool alarms or wafer drop, making processing impossible.

[0003] Among the existing methods, the first method is to deposit doped polysilicon to form a low-resistance buffer layer, and then remove the buffer layer on the front side to reduce the resistivity of the contact surface and increase the adsorption force of the electrostatic chuck; the second method is to deliberately reduce the contact surface resistance by injecting doping elements and then annealing and diffusing to increase the adsorption force of the electrostatic chuck. Both methods change the original structure of the wafer and introduce unnecessary film thickness structure and elements. High-resistance wafers are extremely sensitive to doping elements. Under the high-temperature process of deposition or diffusion, the doping elements will diffuse and migrate, which can easily cause element contamination and lead to material failure. At the same time, the processing of the two methods is relatively complicated. The first method requires multiple depositions and removal of the film layer on the front side. The second method requires a high-energy injection machine. The high-temperature annealing and diffusion increase production capacity, cost, and processing cycle, resulting in waste of resources. Summary of the Invention

[0004] In order to solve the technical problems existing in the prior art, the present invention provides a wafer structure and method for improving the electrostatic adsorption ability of high-resistance wafers. The wafer structure and method do not require annealing to increase the bonding force, and can directly meet the needs of electrostatic chuck equipment in the subsequent process. Temporary bonding of heterogeneous materials can be achieved at room temperature, greatly reducing the production cycle.

[0005] In order to achieve the above technical effects, the present invention adopts the following technical solutions:

[0006] One of the purposes of the present invention is to provide a wafer structure for improving the electrostatic adsorption capability of a high-resistance wafer, the wafer structure comprising a high-resistance wafer and a low-resistance wafer disposed on one side of the high-resistance wafer, the high-resistance wafer and the low-resistance wafer being bonded to each other;

[0007] The resistance of low-resistance wafers is less than 3000 ohm.cm.

[0008] Among them, the resistance value of the low-resistance wafer can be 2800ohm.cm, 2500ohm.cm, 2000ohm.cm, 1500ohm.cm, 1000ohm.cm or 500ohm.cm, etc., but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0009] As a preferred technical solution of the present invention, the resistance of the high-resistance wafer is greater than 3000ohm.cm, such as 3200ohm.cm, 3500ohm.cm, 4000ohm.cm, 4500ohm.cm or 5000ohm.cm, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0010] Preferably, the material of the high-resistance wafer includes any one of high-resistance silicon, silicon oxide, semi-insulating silicon carbide, quartz, lithium tantalate, lithium niobate, sapphire or ceramic.

[0011] Preferably, the material of the low-resistance wafer includes low-resistance silicon or conductive silicon carbide.

[0012] As a preferred technical solution of the present invention, the bonding strength of the bonding connection is 0.3 to 0.5 J / m 2 , such as 0.3J / m 2 , 0.32J / m 2 , 0.35J / m 2 , 0.38J / m 2 , 0.4J / m 2 , 0.42J / m 2 , 0.45J / m 2 , 0.48J / m 2 or 0.5 J / m 2 etc., but are not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0013] As a preferred technical solution of the present invention, the bonding connection is a hydrophilic connection.

[0014] A second object of the present invention is to provide a method for improving the electrostatic adsorption capability of a high-resistance wafer, the method comprising:

[0015] The bonding surface of the high-resistance wafer and the bonding surface of the low-resistance wafer are sequentially cleaned and activated;

[0016] The bonding surface of the high-resistance wafer and the bonding surface of the low-resistance wafer are pressed relative to each other.

[0017] As a preferred technical solution of the present invention, the cleaning method includes RCA cleaning.

[0018] As a preferred technical solution of the present invention, after cleaning, the bonding surfaces of the high-resistance wafer and the low-resistance wafer have an independent roughness of less than 0.3 nm, and the number of particles larger than 0.3 μm is ≤20.

[0019] Among them, the roughness can be 0.28nm, 0.25nm, 0.22nm, 0.2nm, 0.18nm, 0.15nm, 0.12nm or 0.1nm, etc., and the number of particles larger than 0.3μm can be 20, 18, 15, 12, 10, 8 or 5, etc., but is not limited to the listed values. Other values ​​not listed within the above numerical ranges are also applicable.

[0020] As a preferred technical solution of the present invention, the activation treatment method includes using ionized gas to perform plasma bombardment on the bonding surface of the high-resistance wafer or the bonding surface of the low-resistance wafer after cleaning.

[0021] As a preferred technical solution of the present invention, the ionized gas includes any one of ionized argon, nitrogen or oxygen, or a combination of at least two of them. Typical but non-limiting examples of the combination include a combination of argon and nitrogen, a combination of nitrogen and oxygen, a combination of oxygen and argon, or a combination of argon, nitrogen and oxygen, etc.

[0022] Preferably, the power of the activation treatment is 10 to 200 W, such as 10 W, 20 W, 50 W, 80 W, 100 W, 120 W, 150 W, 180 W or 200 W, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0023] Preferably, the activation treatment time is 30 to 300 s, such as 30 s, 60 s, 90 s, 120 s, 150 s, 180 s, 210 s, 240 s, 270 s or 300 s, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0024] Preferably, the flow rate of the ionized gas is 5 to 200 sccm, such as 5 sccm, 10 sccm, 20 sccm, 50 sccm, 80 sccm, 100 sccm, 120 sccm, 150 sccm, 180 sccm or 200 sccm, but is not limited to the listed values. Other values ​​not listed within the numerical range are also applicable.

[0025] As a preferred technical solution of the present invention, the method of debonding the high-resistance wafer and the low-resistance wafer includes independently applying a pulling force to the high-resistance wafer and the low-resistance wafer respectively.

[0026] Compared with the prior art, the present invention has at least the following beneficial effects:

[0027] (1) The present invention provides a wafer structure and method for improving the electrostatic adsorption capability of high-resistance wafers. The wafer structure and method do not require annealing after bonding to increase the bonding force, directly meeting the processing requirements of the subsequent process, and can achieve temporary bonding of heterogeneous materials at room temperature, greatly reducing the production cycle;

[0028] (2) The present invention provides a wafer structure and method for improving the electrostatic adsorption capability of high-resistance wafers. The wafer structure and method can reuse low-resistance wafers multiple times, significantly reducing production costs.

[0029] (3) The present invention provides a wafer structure and method for improving the electrostatic adsorption capability of high-resistance wafers. The wafer structure and method can be used to prepare semi-insulating silicon carbide composite substrates and high-resistance lithium niobate / lithium tantalate thin film POI composite substrates, etc.

[0030] (4) The present invention provides a wafer structure and method for improving the electrostatic adsorption ability of high-resistance wafers. The wafer structure and method are suitable for large-scale production and small-scale experimental research and development, and the method is simple. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] Figure 1 Schematic flow chart of the method for improving the electrostatic adsorption capability of a high-resistance wafer provided in Examples 1-6 of the present invention;

[0032] In the figure: 10 - high-resistance wafer; 11 - low-resistance wafer; 100 - cleaning the bonding surface of the high-resistance wafer; 110 - cleaning the bonding surface of the low-resistance wafer; 210 - hydrophilic bonding of the high-resistance wafer and the low-resistance wafer; 220 - ion implantation process of the bonded body into the high-resistance wafer; 230 - mechanical separation of the bonded body.

[0033] The present invention is further described in detail below. However, the following examples are merely simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims. DETAILED DESCRIPTION

[0034] The technical solution of this application is further described below through specific implementation methods.

[0035] A specific embodiment of the present invention provides a wafer structure for improving the electrostatic adsorption capability of a high-resistance wafer, the wafer structure comprising a high-resistance wafer and a low-resistance wafer disposed on one side of the high-resistance wafer, wherein the high-resistance wafer and the low-resistance wafer are bonded to each other;

[0036] The resistance of low-resistance wafers is less than 3000 ohm.cm.

[0037] In the present invention, the wafer structure does not require annealing to improve the bonding strength, which facilitates debonding after processing. There is no high-temperature process and no element contamination problem. At the same time, the film thickness structure of the high-resistance wafer will not be changed and element doping will not be performed. There is no intermediate layer at the bonding interface, and the material itself and its own properties will not be affected after debonding.

[0038] In a specific embodiment of the present invention, the wafer structure is not only applicable to ion implantation processes, but also applicable to other processes using electrostatic chuck equipment.

[0039] In a specific embodiment of the present invention, the resistance value of the low-resistance wafer is smaller than the resistance value of the high-resistance wafer.

[0040] In a specific embodiment of the present invention, after hydrophilic bonding, the bonding surfaces of the high-resistance wafer and the low-resistance wafer are connected by van der Waals forces and hydrogen bonds.

[0041] In one embodiment of the present invention, the strength of the hydrophilic bond is 0.3 to 0.5 J / m 2 The strength is sufficient to support the adsorption of the electrostatic chuck, and the low-resistance silicon wafer can be debonded after processing is completed; the strength is easy to debond, and debonding can be completed by simply applying mechanical tension.

[0042] A specific embodiment of the present invention provides a method for improving the electrostatic adsorption capability of a high-resistance wafer, the method comprising:

[0043] The bonding surface of the high-resistance wafer and the bonding surface of the low-resistance wafer are sequentially cleaned and activated;

[0044] The bonding surface of the high-resistance wafer and the bonding surface of the low-resistance wafer are pressed relative to each other.

[0045] In a specific embodiment of the present invention, after the activation treatment, the bonding surface of the high-resistance wafer and the bonding surface of the low-resistance wafer are cleaned with pure water and then dried.

[0046] In a specific embodiment of the present invention, the drying rate is 1000-3000 rpm, and the drying time is 30-90 s.

[0047] In a specific embodiment of the present invention, the pressure and time for pressing the bonding surfaces of the high-resistance wafer and the low-resistance wafer relative to each other can be specifically adjusted according to the material and processing requirements of the high-resistance wafer and the low-resistance wafer to achieve the required bonding strength, which is not further limited here.

[0048] In this invention, the hydrophilic bonding principle involves plasma bombarding the clean, polished wafer surface, creating a hydrophilic surface with a high density of hydroxyl groups (-OH). Water molecules in the atmospheric environment readily adsorb to this hydrophilic surface. Subsequently, at room temperature, the two wafers with hydrophilic surfaces are bonded together. During a high-temperature annealing process, the weak intermolecular forces (van der Waals forces and hydrogen bonds) at the interface are converted into stronger covalent bonds, resulting in a secure bonded interface. This invention utilizes the pre-annealing intermolecular forces (van der Waals forces and hydrogen bonds) to temporarily bond the high-resistance wafer to the low-resistance wafer.

[0049] In a specific embodiment of the present invention, the high-resistance wafer and the low-resistance wafer after bonding can be used in an ion implantation process.

[0050] In one embodiment of the present invention, the ion implantation process may have an implantation energy of 10 to 300 KEV and an implantation dose of 2E15 to 5E17 atoms / cm 2 .

[0051] In a specific embodiment of the present invention, after the ion implantation process is completed, the high-resistance wafer and / or the low-resistance wafer may be mechanically and independently subjected to pulling force to complete debonding.

[0052] To better illustrate the present invention and facilitate understanding of the technical solutions of the present invention, typical but non-limiting embodiments of the present invention are as follows:

[0053] Example 1

[0054] This embodiment provides a method for improving the electrostatic adsorption capability of high-resistance wafers, and the process is as follows: Figure 1 As shown, the method includes:

[0055] (1) Clean the high-resistance wafer 10 (quartz wafer) and the low-resistance wafer 11 (low-resistance silicon wafer) according to the RCA standard until the number of particles larger than 0.3 μm on the bonding surface 100 of the high-resistance wafer and the bonding surface 110 of the low-resistance wafer is ≤20 and the roughness Ra is <0.25 nm;

[0056] (2) Bonding the high-resistance wafer 10 and the low-resistance wafer 11 by hydrophilic bonding: wherein, ionized N2 generates plasma to bombard the high-resistance wafer bonding surface 100 and the low-resistance wafer bonding surface 110; activation power 200W, activation time 30s, gas flow rate 20sccm;

[0057] The high-resistance wafer bonding surface 100 and the low-resistance wafer bonding surface 110 are cleaned with pure water and dried at a drying speed of 2000 rpm for 60 seconds.

[0058] The vacuum degree of the chamber is reduced to 0.1 Pa. After the vacuum degree reaches the standard, the high-resistance wafer bonding surface 100 and the low-resistance wafer bonding surface 110 are bonded together. At the same time, the upper tray is pressed down to apply pressure. The upper and lower trays continuously press the bonded body for 120 seconds. After the pressing is completed, the bonded body is taken out. The bonding strength is 0.49 J / m 2 ;

[0059] (3) Perform ion implantation on the bonded body with an implantation energy of 100keV and an implantation dose of 5E16atom / cm 2 At this time, due to the bonding with the low-resistance wafer 11, a larger adsorption force can be obtained when the electrostatic chuck is adsorbed. The bonding strength of the bonded body is sufficient to meet the implantation process, and the wafer drop problem will not occur. After the implantation is completed, it is transferred out of the machine;

[0060] (4) After the injection is completed, the bonded body is debonded, and the high-resistance wafer 10 and the low-resistance wafer 11 can be completely debonded along the bonding surface by using mechanical pulling force.

[0061] (5) The high-resistance wafer 10 continues to undergo subsequent processing, and the low-resistance wafer 11 can be reused.

[0062] Example 2

[0063] This embodiment provides a method for improving the electrostatic adsorption capability of high-resistance wafers, and the process is as follows: Figure 1 As shown, the method includes:

[0064] (1) Clean the high-resistance wafer 10 (quartz wafer) and the low-resistance wafer 11 (low-resistance silicon wafer) according to the RCA standard until the number of particles larger than 0.3 μm on the bonding surface 100 of the high-resistance wafer and the bonding surface 110 of the low-resistance wafer is ≤20 and the roughness Ra is <0.25 nm;

[0065] (2) Bonding the high-resistance wafer 10 and the low-resistance wafer 11 by hydrophilic bonding: ionizing Ar to generate plasma, bombarding the high-resistance wafer bonding surface 100 and the low-resistance wafer bonding surface 110; activation power 10W, activation time 300s, gas flow rate 200sccm;

[0066] The high-resistance wafer bonding surface 100 and the low-resistance wafer bonding surface 110 are cleaned with pure water and then dried at a drying speed of 1000 rpm for 90 seconds.

[0067] The vacuum degree of the chamber is reduced to 0.1 Pa. After the vacuum degree reaches the standard, the high-resistance wafer bonding surface 100 and the low-resistance wafer bonding surface 110 are bonded together. At the same time, the upper tray is pressed down to apply pressure. The upper and lower trays continuously pressurize the bonded body for 60 seconds. After the pressing is completed, the bonded body is taken out. The bonding strength is 0.48 J / m 2 ;

[0068] (3) Perform ion implantation on the bonded body with an implantation energy of 10keV and an implantation dose of 2E16 atoms / cm 2 At this time, due to the bonding with the low-resistance wafer 11, a larger adsorption force can be obtained when the electrostatic chuck is adsorbed. The bonding strength of the bonded body is sufficient to meet the implantation process, and the wafer drop problem will not occur. After the implantation is completed, it is transferred out of the machine;

[0069] (4) After the injection is completed, the bonded body is debonded, and the high-resistance wafer 10 and the low-resistance wafer 11 can be completely debonded along the bonding surface by using mechanical pulling force.

[0070] (5) The high-resistance wafer 10 continues to undergo subsequent processing, and the low-resistance wafer 11 can be reused.

[0071] Example 3

[0072] This embodiment provides a method for improving the electrostatic adsorption capability of high-resistance wafers, and the process is as follows: Figure 1 As shown, the method includes:

[0073] (1) Clean the high-resistance wafer 10 (quartz wafer) and the low-resistance wafer 11 (low-resistance silicon wafer) according to the RCA standard until the number of particles larger than 0.3 μm on the bonding surface 100 of the high-resistance wafer and the bonding surface 110 of the low-resistance wafer is ≤20 and the roughness Ra is <0.25 nm;

[0074] (2) Bonding the high-resistance wafer 10 and the low-resistance wafer 11 by hydrophilic bonding: ionizing O2 to generate plasma, bombarding the high-resistance wafer bonding surface 100 and the low-resistance wafer bonding surface 110; activation power 100W, activation time 120s, gas flow rate 200sccm;

[0075] The high-resistance wafer bonding surface 100 and the low-resistance wafer bonding surface 110 are cleaned with pure water and dried at a drying speed of 3000 rpm for 30 seconds.

[0076] The vacuum degree of the chamber is reduced to 0.1 Pa. After the vacuum degree reaches the standard, the high-resistance wafer bonding surface 100 and the low-resistance wafer bonding surface 110 are bonded together. At the same time, the upper tray is pressed down to apply pressure. The upper and lower trays continuously pressurize the bonded body for 90 seconds. After the pressing is completed, the bonded body is taken out. The bonding strength is 0.47 J / m 2 ;

[0077] (3) Perform ion implantation on the bonded body with an implantation energy of 300keV and an implantation dose of 5E17atom / cm 2 At this time, due to the bonding with the low-resistance wafer 11, a larger adsorption force can be obtained when the electrostatic chuck is adsorbed. The bonding strength of the bonded body is sufficient to meet the implantation process, and the wafer drop problem will not occur. After the implantation is completed, it is transferred out of the machine;

[0078] (4) After the injection is completed, the bonded body is debonded, and the high-resistance wafer 10 and the low-resistance wafer 11 can be completely debonded along the bonding surface by using mechanical pulling force.

[0079] (5) The high-resistance wafer 10 continues to undergo subsequent processing, and the low-resistance wafer 11 can be reused.

[0080] Example 4

[0081] In this embodiment, except that the material of the high-resistance wafer 10 is replaced with a high-resistance silicon carbide wafer, the other conditions are the same as those in Example 1. The bonding strength between the high-resistance wafer 10 and the low-resistance wafer 11 is 0.47 J / m 2 .

[0082] Example 5

[0083] In this embodiment, except that the material of the high-resistance wafer 10 is replaced with lithium niobate, the other conditions are the same as those in Example 1. The bonding strength between the high-resistance wafer 10 and the low-resistance wafer 11 is 0.48 J / m 2 .

[0084] Example 6

[0085] In this embodiment, except that the material of the low-resistance wafer 11 is replaced with a conductive silicon carbide wafer, the other conditions are the same as those in Example 1. The bonding strength between the high-resistance wafer 10 and the low-resistance wafer 11 is 0.46 J / m 2 .

[0086] Comparative Example 1

[0087] In this comparative example, except that the low-resistance wafer 11 is not bonded and the high-resistance wafer 10 is directly subjected to the ion implantation process after RCA cleaning, other conditions are the same as those of Example 1.

[0088] When the high-resistance wafer 10 is transferred to the implantation chamber, an alarm is triggered and the electrostatic chuck cannot absorb the quartz wafer, resulting in implantation failure.

[0089] Comparative Example 2

[0090] In this comparative example, the conditions are the same as those in Example 4, except that the low-resistance wafer 11 is not bonded and the high-resistance wafer 10 is directly subjected to the ion implantation process after RCA cleaning.

[0091] When the high-resistance wafer 10 is transferred to the implantation chamber, the high-resistance wafer may fall off and become fragmented during implantation, resulting in implantation failure.

[0092] Comparative Example 3

[0093] In this comparative example, except that the low-resistance wafer 11 is not bonded and the high-resistance wafer 10 is directly subjected to the ion implantation process after RCA cleaning, the other conditions are the same as those of Example 5.

[0094] After the high-resistance wafer 10 is transferred to the implantation chamber, the electrostatic chuck can normally adsorb the lithium niobate wafer with a small adsorption force. The initial implantation energy is 100keV and the implantation dose is 5E16 atoms / cm 2 , after injection is completed 1E16 atom / cm 2 Later, the chip fell off and the lithium niobate shattered in the chamber, resulting in injection failure.

[0095] The resistance of the quartz wafer used in Examples 1-5 of the present invention is approximately 5E14 ohm.cm, the resistance of the high-resistance silicon carbide wafer is approximately 1E10 ohm.cm, the resistance of the lithium niobate wafer is approximately 6E13 ohm.cm, the resistance of the low-resistance silicon wafer is approximately 10 ohm.cm, and the resistance of the conductive silicon carbide wafer is approximately 500 ohm.cm.

[0096] The test method for bond strength is the cleavage method, which is the crack propagation diffusion method.

[0097] The applicant declares that the present invention is not limited to the above-described detailed structural features through the above-described embodiments, and does not necessarily rely on the above-described detailed structural features for implementation. Those skilled in the art should understand that any improvements to the present invention, equivalent replacements for selected components, additions of auxiliary components, and selection of specific embodiments, etc., fall within the scope of protection and disclosure of the present invention.

[0098] The preferred embodiments of the present invention are described in detail above. However, the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, various simple modifications can be made to the technical solution of the present invention, and these simple modifications all fall within the scope of protection of the present invention.

[0099] It should also be noted that the various specific technical features described in the above specific embodiments can be combined in any appropriate manner without contradiction. In order to avoid unnecessary repetition, the present invention will not further describe various possible combinations.

[0100] In addition, the various embodiments of the present invention may be arbitrarily combined, and as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A wafer structure for improving the electrostatic adsorption capability of a high-resistance wafer, characterized in that: The wafer structure includes a high-resistance wafer and a low-resistance wafer arranged on one side of the high-resistance wafer, and the high-resistance wafer is bonded to the low-resistance wafer; The resistance of the low-resistance wafer is less than 3000 ohm.cm.

2. The wafer structure according to claim 1, characterized in that: The resistance of the high-resistance wafer is greater than 3000 ohm.cm; The material of the high-resistance wafer includes any one of high-resistance silicon, silicon oxide, semi-insulating silicon carbide, quartz, lithium tantalate, lithium niobate, sapphire or ceramic; The material of the low-resistance wafer includes low-resistance silicon or conductive silicon carbide.

3. The wafer structure according to claim 1, characterized in that: The bonding strength of the bonding connection is 0.3 to 0.5 J / m 2 .

4. The wafer structure according to claim 1, characterized in that: The bonding connection is a hydrophilic connection.

5. A method for improving the electrostatic adsorption capability of a high-resistance wafer, characterized in that: The method comprises: Sequentially performing cleaning treatment and activation treatment on the bonding surface of the high-resistance wafer and the bonding surface of the low-resistance wafer; The bonding surface of the high-resistance wafer and the bonding surface of the low-resistance wafer are pressed relative to each other.

6. The method according to claim 5, characterized in that The cleaning method includes RCA cleaning.

7. The method according to claim 5, characterized in that After the cleaning process, the bonding surface of the high-resistance wafer and the bonding surface of the low-resistance wafer have a roughness independently less than 0.3 nm, and the number of particles with a size of 0.3 μm or more is ≤20.

8. The method according to claim 5, characterized in that The activation treatment method includes using ionized gas to perform plasma bombardment on the bonding surface of the high-resistance wafer or the bonding surface of the low-resistance wafer after the cleaning treatment.

9. The method according to claim 8, characterized in that The ionized gas includes any one of ionized argon, nitrogen or oxygen or a combination of at least two thereof; The power of the activation treatment is 10 to 200 W; The activation treatment time is 30 to 300 seconds; The flow rate of the ionized gas is 5-200 sccm.

10. The method according to claim 5, characterized in that The method of debonding the high-resistance wafer and the low-resistance wafer includes independently applying a pulling force to the high-resistance wafer and the low-resistance wafer respectively.