Positive pole piece with high overdischarge stability
By adding LixMoS2 to the positive electrode material layer of the lithium-ion battery, lowering the zero-voltage electrode potential, the problem of rapid increase in the negative electrode potential and decomposition of the SEI film during the overdischarge process of lithium-ion battery is solved, and the overdischarge stability of the battery is improved. Cycling performance ensures battery safety and capacity maintenance.
Patent Information
- Application Number
- CN202310516512.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-09
- Publication Date
- 2024-11-12
AI Technical Summary
During the overdischarge process of lithium-ion batteries, the rapid rise in the negative electrode potential leads to the dissolution of SEI film and foil, resulting in battery capacity loss and safety problems. The existing technology mainly focuses on improving the stability of the negative electrode current collector, but it has not effectively solved the negative electrode. The problem of decomposition of SEI films under long-term high potential.
By adding LixMoS2 to the positive electrode material layer, the zero-voltage electrode potential of the electrochemical device is lowered, the negative electrode potential rises too quickly and the dissolution of the SEI film is suppressed, and the layered structure of LixMoS2 is used to provide lithium embedded sites to avoid excessive downregulation of the positive electrode potential. Damage to material stability.
It effectively improves the overdischarge stability and cycling performance of lithium-ion batteries, maintains the stability of the positive electrode, extends the zero-volt storage performance of the battery, and significantly improves the battery's circulation capacity retention rate and safety.
Smart Images

Figure BDA0004219365890000201
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of battery materials and relates to a positive electrode sheet with high over-discharge stability. Background Art
[0002] Lithium-ion batteries are the most widely used automotive power batteries. In national standards, various group standards, and industry standards, battery overdischarge is one of the important mandatory inspection indicators.
[0003] The power system of electric vehicles needs to use high-capacity lithium-ion battery packs to provide power. The performance of each single cell in the battery pack cannot be completely consistent. Among them, the single cell with low capacity will be forced to over-discharge to below the rated cut-off voltage. Generally, a battery management system is used to monitor each battery in the battery pack, which increases the cost, volume and weight of the battery pack. When the battery is over-discharged to a specific voltage, the protection circuit will disconnect the battery from the load to prevent the battery voltage from further decreasing. However, as time goes on, the battery will still gradually self-discharge to a low voltage. In addition, a failure in the battery management system will also cause the battery to over-discharge. Therefore, the lithium-ion battery itself needs to have a good ability to tolerate low voltage or even zero volts for a long time. That is, when the battery is used in groups and packages, due to the inevitable lack of consistency, some cells will inevitably be over-discharged and in a low-voltage state during long-term work.
[0004] Since the voltage source of the chemical power source is the potential difference between the positive and negative electrodes of the battery, the low voltage state means that the positive electrode potential of the battery decreases and the negative electrode potential increases. When the negative electrode is at a higher potential, the SEI film and foil of the negative electrode will inevitably lose electrons due to the electric field catalysis and produce a reaction.
[0005] During overdischarge, when the negative electrode potential rises rapidly to 3.5V vs. Li / Li + When the current collector copper foil is oxidized, a potential platform will appear. Jin Kawakita et al. found that the copper foil was severely pitted after oxidation, indicating that copper ions were dissolved into the electrolyte. After the negative electrode current collector copper foil is dissolved, the electrical contact between the active material and the copper foil will deteriorate and the adhesion of the active material on the copper foil will decrease, resulting in the shedding of the active material, the reduction of the amount of electricity collected by the current collector, and the loss of battery capacity. Severe copper dissolution at the connection between the copper current collector and the nickel tab in commercial lithium-ion batteries can also cause the battery to short circuit.
[0006] After the copper current collector dissolves, when the battery is charged again, the negative electrode potential decreases, causing the copper ions in the electrolyte to undergo a reduction reaction on the negative electrode surface and deposit on the negative electrode surface in the form of metallic copper, blocking the Li + Transport channel, hindering Li +The copper deposited on the negative electrode surface may also grow in the form of dendrites, piercing the diaphragm and causing a short circuit between the positive and negative electrodes. In addition, when a low-capacity single cell in a battery pack is forced to over-discharge to a negative voltage, the copper ions dissolved from the negative electrode will be reduced to metallic copper on the surface of the low-potential positive electrode. The copper dendrites growing on the positive electrode surface will also pierce the diaphragm, causing a short circuit between the positive and negative electrodes.
[0007] During over-discharge, as the negative electrode potential rises rapidly, the negative electrode SEI film will undergo oxidative decomposition. Hisashi Tsukamoto et al. used titanium foil that is stable at high potential instead of copper foil as the negative electrode current collector to avoid the dissolution of copper foil during over-discharge. The results showed that the capacity loss of LiCoO2 / graphite battery could not be completely avoided. After the battery was stored at zero volt for one week at 37°C, the capacity retention rate was only 73.5%. They believe that the SEI film at the negative electrode at a high potential during zero-volt storage decomposes, and the negative electrode active material is damaged. Fan Maosong et al. proposed that the negative electrode SEI film will partially decompose during over-discharge, and the repair of the SEI film during subsequent charging will consume the active Li + , causing the battery capacity to decay. Yu Zhongbao et al. found that after the LiCoO2 / mesophase carbon microsphere battery was over-discharged to 0V, the polarization of the charge and discharge curve increased and the discharge capacity decreased. They believe that the deposition of the copper current collector on the electrode surface after dissolution; and the poor quality of the regenerated SEI film when charging again after the decomposition of the negative electrode SEI film during over-discharge, are the reasons for the increase in battery impedance. Yadong Liu et al. pointed out that the regeneration of the SEI film will consume the solvent and lithium salt in the electrolyte, so repeated over-discharge will cause the electrolyte to dry up, thereby increasing the internal resistance of the battery. Yong Zheng et al. found that after the LiFePO4 / graphite battery was repeatedly over-discharged to 0V, the SEI film impedance increased; and then during normal cycle charge and discharge, the SEI film impedance increased further. They believe that the SEI film decomposed at the negative electrode during over-discharge, and the impedance of the regenerated SEI film increased during re-charging; the SEI film will continue to thicken in subsequent cycles, continuously consuming active Li + , resulting in degradation of battery cycle performance. After Hui-Fang Li et al. over-discharged the LiCoO2 / graphite soft-pack battery to 0V, they found that the battery had obvious bloating. They believed that the main gas components such as CO2 and CO that caused the battery bloating came from the decomposition of the negative electrode SEI film. When Yong Zheng et al. repeatedly over-discharged the LiFePO4 / graphite soft-pack battery to 0.5V and 0V, the battery also had obvious bloating. They believed that the gas components such as H2 that caused the battery bloating were generated by the decomposition of the negative electrode SEI film.
[0008] In summary, the damage of battery over-discharge comes from the fact that the negative electrode active Li +After all the electrons are removed, the vacancies of the positive electrode active material are not filled, the potential remains high, and the negative electrode potential rises too fast. The negative electrode continues to lose electrons at high potential, and the compounds in the SEI film are destroyed and the single substance Cu is oxidized to Cu 2+ When the negative electrode enters the electrolyte, the negative electrode structure is destroyed, resulting in a decrease in battery capacity and safety issues. Therefore, the key to improving the safety performance of battery over-discharge is that the positive electrode potential drops earlier than the negative electrode potential rises to the potential where the SEI film and foil are destroyed during over-discharge.
[0009] The main method to improve the over-discharge performance of batteries is to improve the stability of the negative electrode current collector at high potential. The stability range of titanium in alkyl carbonate solution is 0V-5V vs.Li / Li + , with a wide electrochemical stability window, Hisashi Tsukamoto et al. used titanium foil to replace copper foil as the negative electrode current collector, improving the capacity retention rate of LiCoO2 / graphite batteries stored at zero volts for one week. Zhang Songtong et al. used magnetron sputtering to deposit a protective titanium film on the surface of the copper current collector, improving the corrosion resistance of the negative electrode current collector. However, the refining and processing costs of titanium current collectors are high, and the conductivity is not as good as that of copper current collectors. Sohrab Hossain et al. used carbon fiber negative electrodes without metal current collectors to assemble batteries, so that the performance of LiCoO2 batteries did not deteriorate significantly after repeated overdischarge to -3V. KRCrompton et al. proposed using carbon nanotube sheets to replace copper foil as the negative electrode current collector, which has the advantage of improving the battery's overdischarge resistance. Young-Soo Kim et al. added succinonitrile (SN) to the electrolyte, and used the coordination reaction of the nitrile group of SN with positive Cu to make the surface of the copper current collector rise to 2.9Vvs.Li / Li + When the Cu(SN)2PF6 passivation film is formed, the dissolution of copper is prevented, thereby improving the capacity recovery rate of the LiCoO2 / graphite battery after repeated overdischarge to 0V. It is worth noting that in the above reports, after the battery is overdischarged to a low voltage, there is no storage time or the storage time is short. As the low-voltage storage time increases, the adverse effects of the decomposition of the negative electrode SEI film on the battery will be reflected. At present, there have been many reports on the research on improving the corrosion resistance of the negative electrode current collector, but the research on improving the stability of the negative electrode SEI film at high potential for a long time has been widely ignored.
[0010] Lowering the zero voltage electrode potential of lithium-ion batteries to 3.5 V vs. Li / Li + The following can also solve the problem of dissolution of the negative electrode copper collector; further lowering the zero voltage electrode potential can also alleviate the decomposition of the negative electrode SEI film and improve the zero volt storage performance of the battery. The reduction of the zero voltage electrode potential can be achieved by lowering the positive electrode discharge platform, lowering the positive electrode first coulomb efficiency and increasing the negative electrode first coulomb efficiency.
[0011] By adding an additive to the positive electrode with a discharge platform lower than that of the active material, the discharge platform of the doped positive electrode can be lowered, thereby reducing the zero voltage electrode potential. Hui-Fang Li et al. added Li(Ni) to the LiCoO2 positive electrode, which accounts for 20 wt% of the active material. 1 / 3 Co 1 / 3 Mn 1 / 3 )O2, the discharge platform of the positive electrode is reduced, and the zero voltage electrode potential is reduced to 3V vs.Li / Li + , the platform for the dissolution of the copper current collector disappears. In addition, the reduction in the zero voltage electrode potential also alleviates the decomposition of the SEI film of the graphite negative electrode, reducing the battery's over-discharge rate to 0V from 27.1% to 9.6%. Kyu-Sung Park et al. added 10wt% Li2MoO3 to the active material of the LiCoO2 positive electrode, causing the discharge platform of the doped positive electrode to tilt downward at the end of the discharge, and finally intersecting with the discharge curve of the graphite negative electrode at 2.2V vs. Li / Li + It is worth noting that in the above reports, the discharge platform of the doped positive electrode is reduced by adding additives with a discharge platform lower than that of the active material to the positive electrode, which will reduce the discharge voltage of the battery and thus reduce the specific energy of the battery.
[0012] When a conventional lithium-ion battery is charged for the first time, the interface side reaction between the negative electrode and the electrolyte is more significant than the interface side reaction between the positive electrode and the electrolyte, so the first coulomb efficiency of the negative electrode is usually lower than the first coulomb efficiency of the positive electrode. + When all are detached, the positive electrode is still in an unembedded state; at this time, the negative electrode potential rises rapidly, while the positive electrode potential drops slowly, and finally the two intersect at an excessively high zero voltage electrode potential, causing the negative electrode copper collector to dissolve and the negative electrode SEI film to decompose. It can be seen that by lowering the first coulombic efficiency of the positive electrode or increasing the first coulombic efficiency of the negative electrode, the zero voltage electrode potential of the battery can be lowered and the zero volt storage performance of the battery can be improved. Reducing the first coulombic efficiency of the positive electrode to a level close to the first coulombic efficiency of the negative electrode can make the Li in the negative electrode in the over-discharge stage + When all are removed, the positive electrode is filled with Li + Therefore, when the negative electrode potential rises rapidly, the positive electrode potential can also drop rapidly, so that the two intersect at a lower zero voltage electrode potential. Alternatively, the first coulomb efficiency of the positive electrode is adjusted to a level lower than the first coulomb efficiency of the negative electrode, so that the positive electrode is first filled with Li during the over-discharge stage. + , its potential drops rapidly; while Li +The potential rises slowly, and the discharge curves of the two finally intersect at a lower zero voltage electrode potential, which inhibits the dissolution of the negative electrode copper collector and the decomposition of the negative electrode SEI film. In order to lower the first coulomb efficiency of the positive electrode, a positive electrode material with a lower first coulomb efficiency can be added to the positive electrode. The Li2NiO2 synthesized by Hochun Lee et al. was first charged to 4.3Vvs.Li / Li + The capacity is as high as 370mAh / g, and the first coulombic efficiency is as low as 32%. They added Li2NiO2, which accounts for 5wt% of the active material, to the positive electrode of the LiCoO2 / graphite battery, which reduced the first coulombic efficiency of the positive electrode from 96.8% to 89.8%, slightly lower than the first coulombic efficiency of the negative electrode of 92%, thereby reducing the zero voltage electrode potential to 3.5Vvs.Li / Li + The dissolution of the negative electrode copper current collector is avoided. After the battery is repeatedly over-discharged to 0V for 3 times, the capacity recovery rate increases from 50% to nearly 100%.
[0013] Eun-Young Goh et al. also used Li2NiO2 as a positive electrode additive for LiCoO2 / graphite batteries, which increased the capacity recovery rate of the battery after a single over-discharge to 0V from 67.4% to nearly 100%. At the same time, they also pointed out that the addition of Li2NiO2 would reduce the cycle performance of LiCoO2 / graphite batteries. As the proportion of Li2NiO2 in the mixed powder of LiCoO2 and Li2NiO2 increases, the cycle stability of the battery gradually deteriorates. KRCrompton et al. used HE5050 (0.49Li2MnO3·0.51LiNi 0.37 Co 0.24 Mn 0.39 O2) replaces LiCoO2 as the positive electrode active material, and its first coulomb efficiency is 83%, which is significantly lower than the first coulomb efficiency of MCMB negative electrode of more than 90%; and the discharge platform of HE5050 positive electrode is tilted compared with LiCoO2 positive electrode, and the discharge curve is at 3V vs.Li / Li + Therefore, the zero voltage electrode potential of HE5050 / MCMB battery is as low as 1.5V vs.Li / Li + Among them, 1.5V vs.Li / Li +The positive electrode platform at is a low potential characteristic platform of layered lithium-rich materials. The lower zero voltage electrode potential makes the capacity recovery rate of HE5050 / MCMB battery close to 100% after 5 weeks of zero volt storage. In addition, the first discharge capacity of HE5050 is 254mAh / g, which is significantly higher than the first discharge capacity of LiCoO2 of 150mAh / g, thus making up for the specific energy lost by the tilt of the HE5050 discharge platform. It is worth noting that KRCrompton et al. also pointed out that the cycle stability of HE5050 is poor, which will accelerate the degradation of capacity during the full battery cycle.
[0014] Similar to lowering the first coulombic efficiency of the positive electrode, raising the first coulombic efficiency of the negative electrode to a level close to the first coulombic efficiency of the positive electrode can make the Li in the negative electrode in the over-discharge stage + When all are removed, the positive electrode is filled with Li + ; Therefore, when the negative electrode potential rises rapidly, the positive electrode potential can also drop rapidly, and finally the two intersect at a lower zero voltage electrode potential, thereby inhibiting the dissolution of the negative electrode copper collector and the decomposition of the negative electrode SEI film, and improving the zero-volt storage performance of the battery. Given that the negative electrode materials of lithium-ion batteries generally have the characteristic of low first coulombic efficiency, it is difficult to find a negative electrode additive that can increase the first coulombic efficiency of the negative electrode to the level of the first coulombic efficiency of the positive electrode. The methods reported in the literature to improve the first coulombic efficiency of the negative electrode include surface modification of the negative electrode, use of new negative electrode binders, and pre-lithiation of the negative electrode. The active sites and defects on the surface can be reduced by slightly oxidizing the graphite surface, and coating with metal oxides or polymers can also cover the active sites on the graphite surface, thereby reducing the reduction and decomposition of the electrolyte on the graphite surface, reducing the irreversible capacity of the negative electrode, that is, improving the first coulombic efficiency of the negative electrode. Pallavi Verma et al. used n-butyl lithium solution to pre-reduce the surface of graphite powder, which reduced the irreversible capacity loss rate of the graphite negative electrode in the first cycle from 22% to 17%. Lili Chai et al. used chitosan to replace polyvinylidene fluoride (PVDF) as a binder for graphite negative electrodes and found that the first coulombic efficiency of graphite negative electrodes increased from 89.3% to 95.4%. They believed that chitosan would promote the formation of a thinner SEI film on the surface of the graphite negative electrode. It is worth noting that even if the negative electrode is surface modified or a new binder is used, some negative electrode SEI films are still generated during the charging process of the battery, so these two methods have limited effect on improving the first coulombic efficiency of the negative electrode.
[0015] Negative electrode pre-lithiation can also improve the first coulombic efficiency of the negative electrode. Negative electrode pre-lithiation refers to the formation of SEI film in the negative electrode before the first charge of the full battery, or even the embedding of some Li +This improves the coulombic efficiency of the negative electrode when the full battery is charged for the first time. In addition, pre-lithiation of the negative electrode can also improve the reversible capacity and cycle performance of the battery. There are two common methods for pre-lithiation of the negative electrode: one is to short-circuit the negative electrode with metallic lithium; the other is to pre-lithiate the negative electrode with a lithium-ion battery. + The counter electrodes are assembled into a battery and discharged.
[0016] It should be pointed out that there is a lower limit to the reduction of the zero voltage electrode potential. This is because excessive reduction of the zero voltage electrode potential will damage the stability of the positive electrode material. Jie Shu et al. found that LiCoO2 at 1.25V vs. Li / Li + The following potentials will be converted into Co and Li2O, resulting in a significant decrease in the reversible capacity in the normal potential range. KRCrompton et al. found that repeated over-embedding of 5% Li+ in LiCoO2 will cause cation mixing, resulting in increased polarization of the discharge curve. Johanna Nelson Weker et al. found that LiCoO2 particles will undergo significant cracking and pulverization during a single discharge to 0.8V vs. Li / Li+.
[0017] In summary, the existing over-discharge stability technologies include preventing the current collector from dissolving and reducing the zero voltage electrode potential of lithium-ion batteries to 3.5V vs. Li / Li + The following. Although the replacement of the current collector, coating, and addition of passivating agents can prevent the destruction and dissolution of the current collector and ensure the overall integrity of the negative electrode, they cannot prevent the reaction of the active material at high potential. As the low-voltage storage time increases, the adverse effects of the decomposition of the negative electrode SEI film on the battery will be reflected. The existing method of improving the over-discharge resistance of lithium-ion batteries by lowering the zero-voltage electrode potential may have an adverse effect on the cycle performance of the positive electrode. Summary of the invention
[0018] In view of the problems existing in the prior art, the present invention provides a positive electrode sheet with high over-discharge stability, an electrochemical device containing the positive electrode sheet, and a method for improving the over-discharge stability of the electrochemical device using the positive electrode sheet. x MoS2 (0<x≤0.8) moderately lowers the zero voltage electrode potential of electrochemical devices, such as lithium-ion batteries, inhibits the rapid increase of the negative electrode potential during over-discharge, inhibits the dissolution of the SEI film and the dissolution of the foil, and Li x MoS2 can maintain the cycle performance of the positive electrode.
[0019] Specifically, one aspect of the present invention provides a positive electrode sheet, the positive electrode sheet comprising a positive electrode current collector and a positive electrode material layer located on the surface of the positive electrode current collector, the positive electrode material layer comprising a positive electrode active material and Li xMoS2, where 0<x≤0.8.
[0020] In one or more embodiments, the Li x MoS2 can intercalate lithium ions during overdischarge.
[0021] In one or more embodiments, the positive electrode material layer has Li x The mass fraction of MoS2 is 1%-3%.
[0022] In one or more embodiments, the positive electrode active material is lithium nickel cobalt manganese oxide.
[0023] In one or more embodiments, the Li x In MoS2, 0.3≤x≤0.7.
[0024] In one or more embodiments, the mass fraction of the positive electrode active material in the positive electrode material layer is 85%-97%.
[0025] In one or more embodiments, the positive electrode material layer further includes a conductive agent and a binder; preferably, the mass fraction of the conductive agent in the positive electrode material layer is 0.5%-1.5%; preferably, the mass fraction of the binder in the positive electrode material layer is 1%-5%.
[0026] Another aspect of the present invention provides an electrochemical device, wherein the electrochemical device comprises the positive electrode sheet described in any embodiment of the present invention.
[0027] In one or more embodiments, the electrochemical device is a lithium ion battery.
[0028] In one or more embodiments, the Li in the positive electrode sheet x MoS2 did not undergo lithium desorption during the first charging process.
[0029] In one or more embodiments, the electrochemical device further comprises a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, and the negative electrode active material is graphite.
[0030] Another aspect of the present invention provides a method for improving overdischarge stability of an electrochemical device, the method comprising using the positive electrode sheet described in any embodiment of the present invention in the electrochemical device.
[0031] In one or more embodiments, the electrochemical device is a lithium ion battery.
[0032] In one or more embodiments, the method includes making the Li x MoS2 does not undergo delithiation during the first charge process of the electrochemical device.
[0033] In one or more embodiments, the electrochemical device further comprises a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, and the negative electrode active material is graphite. DETAILED DESCRIPTION
[0034] In order to enable those skilled in the art to understand the characteristics and effects of the present invention, the following is a general description and definition of the terms and expressions mentioned in the specification and claims. Unless otherwise specified, all technical and scientific terms used in the text are the common meanings understood by those skilled in the art for the present invention. In the event of a conflict, the definition in this specification shall prevail.
[0035] The theories or mechanisms described and disclosed herein, whether correct or incorrect, should not limit the scope of the present invention in any way, that is, the present invention can be implemented without being limited by any specific theory or mechanism.
[0036] Herein, “comprising”, “including”, “containing” and similar terms encompass the meanings of “consisting essentially of” and “consisting of”. For example, when “A comprises B and C” is disclosed herein, “A consists essentially of B and C” and “A consists of B and C” should be deemed to be disclosed herein.
[0037] In this article, all features such as values, quantities, contents and concentrations defined in the form of numerical ranges or percentage ranges are only for brevity and convenience. Accordingly, the description of numerical ranges or percentage ranges should be considered to have included and specifically disclosed all possible secondary ranges and individual values within the range (including integers and fractions).
[0038] Herein, the sum of the percentage content or mass fraction of each component of the composition is 100%.
[0039] In this document, unless otherwise specified, percentage refers to mass percentage and ratio refers to mass ratio.
[0040] Herein, when describing embodiments or examples, it should be understood that they are not used to limit the present invention to these embodiments or examples. On the contrary, all substitutes, improvements and equivalents of the methods and materials described in the present invention can be included in the scope limited by the claims.
[0041] In this document, in order to make the description concise, not all possible combinations of various technical features in various embodiments or examples are described. Therefore, as long as there is no contradiction in the combination of these technical features, the various technical features in various embodiments or examples can be combined arbitrarily, and all possible combinations should be considered to be within the scope of this specification.
[0042] The over-discharge and under-voltage state of lithium-ion power batteries during over-discharge inspection and use will inevitably cause damage to the negative electrode of the battery at high potential. The main means of improving the over-discharge performance of the battery is to improve the stability of the negative electrode current collector at high potential. However, if only the current collector is replaced, the adverse effect of the decomposition of the negative electrode SEI film on the battery will be reflected as the low-voltage storage time increases. Another solution to improve the over-discharge performance of the battery is to lower the zero-voltage electrode potential, which can not only avoid the oxidation and dissolution of the negative electrode foil, but also alleviate the decomposition of the negative electrode SEI film and improve the zero-volt storage performance of the battery. However, there is a lower limit to the reduction of the zero-voltage electrode potential, because excessively lowering the zero-voltage electrode potential will damage the stability of the positive electrode material.
[0043] The inventors of the present invention found that Li x MoS2 material has a low potential and a special layered structure, which can provide multiple vacancies of different energy levels as lithium insertion sites, and is an excellent lithium insertion potential regulating buffer. x The lithium intercalation potential of MoS2 material (about 1.13V) is lower than the working voltage of NMC positive electrode material (3.0-4.4V). x MoS2 material intercalation does not undergo lithium insertion reaction. During overdischarge, the working voltage of the positive electrode material drops to Li x The intercalation voltage of MoS2 material is 1.13V, which intersects with the rapid rising curve of the negative electrode potential of 0.1-2.0V, preventing the negative electrode potential from further rising to the copper dissolution potential of 3.5V. It can provide bridge vacancies for lithium ion embedding before and only before the positive electrode vacancies are filled, thereby lowering the positive electrode potential and allowing the negative electrode potential to reach the termination potential in advance. It can both lower the electrode potential when discharging to a value close to zero voltage and avoid excessively lowering the zero voltage electrode potential which will damage the stability of the positive electrode material.
[0044] In the present invention, Li x MoS2 is present in the positive electrode material layer as an additive, rather than as a part of the positive electrode active material (such as a coating on the surface of the positive electrode active material). In other words, Li x MoS2 and the positive electrode active material exist relatively independently in the positive electrode material layer.
[0045] The present invention uses positive electrode additive Li x MoS2 moderately lowers the zero voltage electrode potential of lithium-ion batteries during over-discharge, especially nickel cobalt manganese oxide (NCM) positive electrode / graphite negative electrode batteries, inhibits the rapid increase of negative electrode potential during over-discharge, and inhibits the dissolution of SEI film and foil. x MoS2 has no adverse effect on the cycle stability of lithium-ion battery positive electrodes, such as NCM positive electrodes. xMoS2 can maintain the cycle performance of lithium-ion battery positive electrodes, such as NCM positive electrodes.
[0046] In the mixing process of making the positive electrode of the battery, a certain amount of Li x MoS2 material, and then enter the subsequent process. During the over-discharge process, lithium ions are embedded in Li x The layered structure of MoS2 has bridge vacancies, and the positive electrode potential drops to Li x The lithium intercalation potential of MoS2 material is about 1.13V. x The intercalation potential of MoS2 intersects with the rapid rise curve of the potential of the negative electrode (such as a graphite negative electrode), so that when the battery reaches 0V, the negative electrode still maintains a lower potential to avoid damage. The electrochemical device using the positive electrode of the battery of the present invention, such as a lithium ion battery, has good over-discharge stability while maintaining good positive electrode cycle performance.
[0047] The positive electrode sheet of the present invention includes a positive electrode current collector and a positive electrode material layer disposed on at least one surface of the positive electrode current collector. The positive electrode current collector can be aluminum foil, copper foil, titanium foil, nickel foil, iron foil, zinc foil, etc. In some embodiments, the positive electrode current collector is aluminum foil.
[0048] The positive electrode material layer of the positive electrode sheet includes a positive electrode active material. The positive electrode active material may include a compound capable of reversibly inserting and extracting lithium ions. The positive electrode active material may include a composite oxide containing lithium and at least one selected from cobalt, manganese, nickel, aluminum and iron. In a preferred embodiment, the positive electrode active material is lithium nickel cobalt manganese oxide. In some embodiments, the positive electrode active material is LiNi a Co b Mn c O2, wherein a+b+c=1, 0<a<1, 0<b<1, 0<c<1, preferably 0.6≤a<1, more preferably 0.8≤a<1. For example, the preferred positive electrode active material includes LiNi 0.8 Co 0.1 Mn 0.1 O2. The present invention discovered that Li x MoS2 is particularly suitable for nickel cobalt manganese oxide lithium positive electrode. When nickel cobalt manganese oxide is used as the positive electrode active material, Li x MoS2 will not be deintercalated during the first charge process, and can smoothly intercalate lithium during the over-discharge process. In the positive electrode material layer, the mass fraction of the positive electrode active material can be 85%-97%, such as 86%, 87%, 88%, 89%, 90%, 91%, 92%, 93%, 94%, 95%, 96%.
[0049] The positive electrode material layer of the positive electrode plate of the present invention includes Li x MoS2. Li used in the present invention xIn MoS2, 0<x≤0.8, for example, x can be 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7. In some preferred embodiments, Li x In MoS2, 0.3≤x≤0.7, for example, x can be 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65. More preferably, Li x In MoS2, 0.3≤x≤0.5. x MoS2 has a layered structure with bridge vacancies, which can be used for lithium ion embedding during overdischarge. At zero voltage, the positive electrode potential is constrained to its lithium embedding potential (1.13V). x The mass fraction of MoS2 is preferably 1%-3%, such as 1.5%, 2%, 2.5%. x Controlling the mass fraction of MoS2 within the range of 1%-3% can moderately lower the zero voltage electrode potential of the electrochemical device, which is beneficial to obtain significantly improved over-discharge stability and maintain good stability of the positive electrode active material, which is beneficial to obtain a high battery cycle capacity retention rate.
[0050] The positive electrode material layer of the positive electrode sheet may also include one or two selected from a conductive agent and a binder. The conductive agent is used to improve the conductivity. Examples of the conductive agent in the positive electrode material layer include one or more of carbon nanotubes, graphene, vapor-deposited carbon fibers, conductive graphite, conductive carbon black, polyacetylene, polythiophene, polypyrrole, polyaniline, polyphenylene, polyphenylene ethylene, polydiyne, etc. The binder in the positive electrode material layer is used to improve the bonding properties between the positive electrode active material particles and between the positive electrode active material particles and the current collector. Examples of the binder in the positive electrode material layer include one or more of polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC-Na), lithium carboxymethyl cellulose, cyclodextrin, gelatin, polyvinyl alcohol, polyacrylate, acrylonitrile multipolymer, etc. In some embodiments, the conductive agent in the positive electrode material layer is conductive carbon black, and the binder is PVDF. In the positive electrode material layer, the mass fraction of the conductive agent can be 0.5%-5%, such as 1%, 2%, 3%, 4%, and the mass fraction of the binder can be 1%-10%, such as 2%, 5%, 7%, 9%.
[0051] The components of the positive electrode material layer can be uniformly dispersed in a solvent to obtain a positive electrode material slurry, which is then coated on a current collector, dried, and pressed to obtain the positive electrode sheet of the present invention. The solvent of the positive electrode material slurry can be N-methylpyrrolidone.
[0052] The present invention includes an electrochemical device, such as a lithium-ion battery, containing the positive electrode sheet of the present invention. The electrochemical device includes a positive electrode sheet, a negative electrode sheet, a separator and an electrolyte. The separator can be arranged between the positive and negative electrode sheets.
[0053] The negative electrode sheet includes a negative electrode current collector and a negative electrode material layer disposed on the negative electrode current collector. The negative electrode current collector may be a copper foil or the like. The negative electrode material layer includes a negative electrode active material. The negative electrode active material may include a material capable of reversibly embedding / de-embedding lithium ions, lithium metal, lithium metal alloy, a material capable of doping / de-doping lithium, or a transition metal oxide. Examples of negative electrode active materials include carbon materials (graphite, soft carbon, hard carbon, etc.), silicon, silicon compounds, lithium titanate, tin, tin compounds, etc. Preferably, the working potential of the negative electrode active material used in the present invention is between 0-0.1V, and the negative electrode active material that meets this condition includes graphite.
[0054] The negative electrode material layer may also include one or two selected from a conductive agent and a binder. The conductive agent is used to improve the conductivity of the electrode. Examples of the conductive agent in the negative electrode material layer include carbon nanotubes, graphene, vapor-deposited carbon fibers, conductive graphite, conductive carbon black, polyacetylene, polythiophene, polypyrrole, polyaniline, polyphenylene, polyphenylene ethylene, polydiyne, etc. The binder in the negative electrode material layer is used to improve the bonding properties between the negative electrode active material particles and between the negative electrode active material particles and the current collector. Examples of the binder in the negative electrode material layer include polyvinylidene fluoride (PVDF), styrene-butadiene rubber (SBR), sodium carboxymethyl cellulose (CMC-Na), lithium carboxymethyl cellulose, cyclodextrin, gelatin, polyvinyl alcohol, polyacrylate, acrylonitrile multipolymer, etc. In some embodiments, the conductive agent in the negative electrode material layer is conductive carbon black, and the binder is SBR and CMC-Na. The mass ratio of each component in the negative electrode material layer can be conventional.
[0055] The negative electrode material layer is obtained by coating the negative electrode material slurry containing the components of the negative electrode material layer and a solvent onto the negative electrode current collector, followed by drying and pressing. The solvent of the negative electrode material slurry can be water.
[0056] The separator can be a polymer porous separator, an inorganic porous separator or a polymer-inorganic composite porous separator. The polymer porous separator includes a single-layer polymer porous separator and a multi-layer polymer porous separator.
[0057] The electrolyte solution includes an organic solvent and an electrolyte salt.
[0058] Organic solvents suitable for electrolytes may include carbonate solvents, carboxylate solvents, ether solvents or other aprotic solvents. In some embodiments, the electrolyte includes carbonate solvents. In the electrolyte of the present invention, the mass of carbonate solvents may be 80%-100% of the total mass of the organic solvent, such as 85%, 90%, 95%. Examples of carbonate solvents include ethylene carbonate (EC), propylene carbonate (PC), dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate, butyl propionate, etc. In some embodiments, the organic solvent is selected from at least two of ethylene carbonate, propylene carbonate, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, γ-butyrolactone, methyl acetate, ethyl acetate, propyl acetate, butyl acetate, ethyl propionate, propyl propionate and butyl propionate. In some embodiments, the organic solvent comprises at least one cyclic carbonate and at least one linear carbonate. Examples of cyclic carbonates include ethylene carbonate, propylene carbonate, butylene carbonate, gamma-butyrolactone, etc. Examples of linear carbonates include dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, etc.
[0059] The electrolyte salt suitable for the electrolyte may include or be selected from a lithium salt. The lithium salt may be selected from one or more of an organic lithium salt and an inorganic lithium salt. In some embodiments, the electrolyte salt is selected from at least one of LiPF6, LiBF4, LiFSI, LiTFSI, LiBOB, LiODFB and LiPO2F2. In some embodiments, the concentration of the electrolyte salt in the electrolyte is 0.5 to 2 mol / L, for example, 1 mol / L, 1.5 mol / L.
[0060] The electrolyte may optionally contain various additives that can be used in the electrolyte, such as desolvating agents, cosolvents, film-forming additives, etc. The mass fraction of each type of additive in the electrolyte may be 0.1% to 10%, such as 1%, 2%, 3%, 4%, 5%.
[0061] The positive electrode sheet, the negative electrode sheet and the separator are stacked and / or wound, encapsulated in a shell, and dried, injected (electrolyte is injected), sealed, left to stand, formed, and divided to obtain a lithium-ion battery. The form of the lithium-ion battery of the present invention is not particularly limited, and can be a cylindrical lithium-ion battery, a soft-pack lithium-ion battery or an aluminum-shell lithium-ion battery.
[0062] The present invention also includes an electronic device containing the electrochemical device of the present invention. The electrochemical device of the present invention is applicable to electronic devices in various fields. The use of the electrochemical device of the present invention is not particularly limited, and it can be used for any use known in the prior art. In some embodiments, the electrochemical device of the present invention can be used for but not limited to the following electronic devices: laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD TVs, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries, drones, and lithium-ion capacitors, etc.
[0063] The present invention has the following beneficial effects:
[0064] (1) The present invention adds Li to the positive electrode x The new method of MoS2 lowers the zero voltage electrode potential of the battery and can use traditional production processes, which has good practicality.
[0065] (2) Li added to the positive electrode of the present invention x MoS2 can maintain the cycle stability of the battery, and its discharge platform has a new use in suppressing excessive reduction of the zero-voltage electrode potential, which can avoid the adverse effects of too low potential on the stability of the positive electrode material.
[0066] (3) In the existing method of lowering the zero-point voltage electrode potential to improve over-discharge stability, as the battery cycle increases, the side reaction to Li + The consumption of the positive electrode continues to accumulate, resulting in the complete lithium insertion of the positive electrode lagging behind the complete lithium removal of the negative electrode, so that the rapid rise of the negative electrode potential occurs earlier during overdischarge, thereby offsetting the partial effect of lowering the zero voltage electrode potential, triggering the decomposition of the negative electrode SEI film again, and even causing the dissolution of the negative electrode copper current collector, which does not solve the problem of the degradation of the zero volt storage performance of the battery after multiple cycles. The Li x Due to its special layered structure, MoS2 can provide multiple vacancies at different energy levels as lithium insertion sites, and is an excellent potential buffer. It further improves the stability of the negative electrode SEI film and the negative electrode copper current collector at high potentials, which is conducive to achieving the reliability and safety of zero-volt storage throughout the battery life cycle.
[0067] (4) CN106129380A discloses a positive electrode plate and an amorphous carbon lithium battery containing the positive electrode plate. The document adds a transition metal lithium sulfide (such as LiMoS2) to the positive electrode material layer of the positive electrode plate of the amorphous carbon lithium battery. During charging, the lithium released from the transition metal lithium sulfide is used to form the SEI film on the surface of the negative electrode active material. During discharge, the lithium ions will not return to the released transition metal lithium sulfide, thereby avoiding the irreversible consumption of lithium in the positive electrode active material and improving the battery's initial charge and discharge efficiency and battery capacity. In the document, the transition metal lithium sulfide is used as a positive electrode lithium supplement, which releases lithium ions into the negative electrode before the positive electrode active material to participate in the film formation reaction. In the subsequent charge and discharge, the lithium ions can no longer be embedded in the transition metal sulfide formed by the de-embedding of the transition metal lithium sulfide. It can be seen that in this document, transition metal lithium sulfide is used as a one-time lithium replenisher in the first charging process. The mechanism of action is to deintercalate the contained lithium ions into the negative electrode at one time under the action of an external electric field during the first charge. For example, the upper limit potential of LiMoS2 material is 3V lower than that of NCA material. It can complete deintercalation first in the first charge and no longer intercalate lithium, so it can be used as a one-time lithium replenisher.
[0068] The present invention is based on Li x MoS2 (0<x≤0.8) has the advantages of providing bridge vacancies for lithium ion embedding at low voltage or at reduced positive electrode potential, i.e., Li x MoS2 can embed lithium ions during overdischarge. During overdischarge, the positive electrode lithium embedding potential decreases, and the negative electrode de-embedding potential increases. When the negative electrode potential rises above 3V, negative electrode damage is likely to occur. x MoS2 material has a lithium intercalation potential of about 1.13V, which is just between the high potential slope area of the lithium intercalation potential of the negative electrode active material (for example, 0.1-2V for graphite). It can intercalate lithium during over-discharge, so it can suppress the rapid rise of the negative electrode potential before the negative electrode potential reaches 2V. x The role of MoS2 is to embed lithium ions into Li x The layered structure of MoS2 has bridge vacancies, and the positive electrode potential drops to Li x The lithium intercalation potential of MoS2 material is about 1.13V. x The intercalation potential of MoS2 intersects with the rapid rise curve of the negative electrode potential, so that when the battery reaches 0V, the negative electrode still maintains a low potential to avoid damage. x MoS2 is not used as a lithium supplement. It does not take precedence over the positive electrode active material in delithiation during the first charge and does not participate in SEI film formation.
[0069] (5) The present invention controls Li xThe mass content of MoS2 additive in the positive electrode material layer of the positive electrode sheet is 1%-3%. Within this range, the battery has a high cycle retention rate after over-discharge. After a 4.2V-0V over-discharge, a conventional cycle test of 4.2V-2.8V is performed, and the 300-week capacity retention rate can be above 79%. The control group without the additive of the present invention has a capacity retention rate that drops to 79% after 100 cycles. The ternary-graphite system battery cell composed of the positive electrode sheet using the additive of the present invention has a significantly improved over-discharge cycle retention rate compared to the positive electrode sheet without the additive.
[0070] The present invention will be described below in the form of specific examples. It should be understood that these examples are merely illustrative and are not intended to limit the scope of the present invention. The methods, reagents and materials used in the examples are, unless otherwise stated, conventional methods, reagents and materials in the art. The raw material compounds in the examples can all be purchased through commercial routes.
[0071] Example 1
[0072] Step 1: Use 12μm thick aluminum foil as the positive electrode current collector;
[0073] Step 2: NCM ternary material (LiNi 0.8 Co 0.1 Mn 0.1 O2), conductive carbon black, Li 0.5 MoS2 and polyvinylidene fluoride (PVDF) were mixed in a weight ratio of 90:3:2:5 and uniformly dispersed in N-methylpyrrolidone to prepare NCM ternary-Li x MoS2 slurry;
[0074] Step 3: Use extrusion coating equipment to coat NCM ternary-Li x The MoS2 slurry is evenly coated on the upper and lower surfaces of the aluminum foil, so that the coating amount on one side is 26 mg / cm 2 After drying, the upper and lower surfaces have NCM ternary-Li x MoS2 coated aluminum foil;
[0075] Step 4: The NCM ternary-Li x The MoS2-coated aluminum foil is rolled, sheared, and dried to obtain a doped positive electrode sheet.
[0076] Example 2
[0077] Step 1: Use 12μm thick aluminum foil as the positive electrode current collector;
[0078] Step 2: NCM ternary material (LiNi 0.8 Co 0.1 Mn0.1 O2), conductive carbon black, Li 0.5 MoS2 and polyvinylidene fluoride (PVDF) were mixed in a weight ratio of 91:3:1:5 and uniformly dispersed in N-methylpyrrolidone to prepare NCM ternary-Li x MoS2 slurry;
[0079] Step 3: Use extrusion coating equipment to coat NCM ternary-Li x The MoS2 slurry is evenly coated on the upper and lower surfaces of the aluminum foil, so that the coating amount on one side is 26 mg / cm 2 After drying, the upper and lower surfaces have NCM ternary-Li x MoS2 coated aluminum foil;
[0080] Step 4: The NCM ternary-Li x The MoS2-coated aluminum foil is rolled, sheared, and dried to obtain a doped positive electrode sheet.
[0081] Example 3
[0082] Step 1: Use 12μm thick aluminum foil as the positive electrode current collector;
[0083] Step 2: NCM ternary material (LiNi 0.8 Co 0.1 Mn 0.1 O2), conductive carbon black, Li 0.5 MoS2 and polyvinylidene fluoride (PVDF) were mixed in a weight ratio of 89:3:3:5 and uniformly dispersed in N-methylpyrrolidone to prepare NCM ternary-Li x MoS2 slurry;
[0084] Step 3: Use extrusion coating equipment to coat NCM ternary-Li x The MoS2 slurry is evenly coated on the upper and lower surfaces of the aluminum foil, so that the coating amount on one side is 26 mg / cm 2 After drying, the upper and lower surfaces have NCM ternary-Li x MoS2 coated aluminum foil;
[0085] Step 4: The NCM ternary-Li x The MoS2-coated aluminum foil is rolled, sheared, and dried to obtain a doped positive electrode sheet.
[0086] Example 4
[0087] Step 1: Use 12μm thick aluminum foil as the positive electrode current collector;
[0088] Step 2: NCM ternary material (LiNi 0.8Co 0.1 Mn 0.1 O2), conductive carbon black, Li 0.3 MoS2 and polyvinylidene fluoride (PVDF) were mixed in a weight ratio of 90:3:2:5 and uniformly dispersed in N-methylpyrrolidone to prepare NCM ternary-Li x MoS2 slurry;
[0089] Step 3: Use extrusion coating equipment to coat NCM ternary-Li x The MoS2 slurry is evenly coated on the upper and lower surfaces of the aluminum foil, so that the coating amount on one side is 26 mg / cm 2 After drying, the upper and lower surfaces have NCM ternary-Li x MoS2 coated aluminum foil;
[0090] Step 4: The NCM ternary-Li x The MoS2-coated aluminum foil is rolled, sheared, and dried to obtain a doped positive electrode sheet.
[0091] Example 5
[0092] Step 1: Use 12μm thick aluminum foil as the positive electrode current collector;
[0093] Step 2: NCM ternary material (LiNi 0.8 Co 0.1 Mn 0.1 O2), conductive carbon black, Li 0.7 MoS2 and polyvinylidene fluoride (PVDF) were mixed in a weight ratio of 90:3:2:5 and uniformly dispersed in N-methylpyrrolidone to prepare NCM ternary-Li x MoS2 slurry;
[0094] Step 3: Use extrusion coating equipment to coat NCM ternary-Li x The MoS2 slurry is evenly coated on the upper and lower surfaces of the aluminum foil, so that the coating amount on one side is 26 mg / cm 2 After drying, the upper and lower surfaces have NCM ternary-Li x MoS2 coated aluminum foil;
[0095] Step 4: The NCM ternary-Li x The MoS2-coated aluminum foil is rolled, sheared, and dried to obtain a doped positive electrode sheet.
[0096] Comparative Example 1
[0097] The existing ternary positive electrode sheet is prepared by ordinary method:
[0098] Step 1: Use 12μm thick aluminum foil as the positive electrode current collector;
[0099] Step 2: NCM ternary material (LiNi 0.8 Co 0.1 Mn 0.1 O2), conductive carbon black and PVDF are mixed in a weight ratio of 92:3:5 and uniformly dispersed in N-methylpyrrolidone to prepare NCM ternary slurry;
[0100] Step 3: Use extrusion coating equipment to evenly coat the NCM ternary slurry on the upper and lower surfaces of the aluminum foil. The coating amount on one side is 26 mg / cm 2 After drying, an aluminum foil with NCM ternary coating on both sides is obtained;
[0101] Step 4: Roll, shear and dry the aluminum foil with NCM ternary coating obtained in the third step to obtain the existing NCM ternary positive electrode sheet.
[0102] Comparative Example 2
[0103] Step 1: Use 12μm thick aluminum foil as the positive electrode current collector;
[0104] Step 2: NCM ternary material (LiNi 0.8 Co 0.1 Mn 0.1 O2), conductive carbon black, Li 0.5 MoS2 and polyvinylidene fluoride (PVDF) were mixed in a weight ratio of 87:3:5:5 and uniformly dispersed in N-methylpyrrolidone to prepare NCM ternary-Li x MoS2 slurry;
[0105] Step 3: Use extrusion coating equipment to coat NCM ternary-Li x The MoS2 slurry is evenly coated on the upper and lower surfaces of the aluminum foil, so that the coating amount on one side is 26 mg / cm 2 After drying, the upper and lower surfaces have NCM ternary-Li x MoS2 coated aluminum foil;
[0106] Step 4: The NCM ternary-Li x The MoS2-coated aluminum foil is rolled, sheared, and dried to obtain a doped positive electrode sheet.
[0107] Comparative Example 3
[0108] Step 1: Use 12μm thick aluminum foil as the positive electrode current collector;
[0109] Step 2: NCM ternary material (LiNi 0.8 Co0.1 Mn 0.1 O2), conductive carbon black, Li 0.5 MoS2 and polyvinylidene fluoride (PVDF) were mixed in a weight ratio of 91.5:3:0.5:5 and uniformly dispersed in N-methylpyrrolidone to prepare NCM ternary-Li x MoS2 slurry;
[0110] Step 3: Use extrusion coating equipment to coat NCM ternary-Li x The MoS2 slurry is evenly coated on the upper and lower surfaces of the aluminum foil, so that the coating amount on one side is 26 mg / cm 2 After drying, the upper and lower surfaces have NCM ternary-Li x MoS2 coated aluminum foil;
[0111] Step 4: The NCM ternary-Li x The MoS2-coated aluminum foil is rolled, sheared, and dried to obtain a doped positive electrode sheet.
[0112] Comparative Example 4
[0113] Step 1: Use 12μm thick aluminum foil as the positive electrode current collector;
[0114] Step 2: NCM ternary material (LiNi 0.8 Co 0.1 Mn 0.1 O2), conductive carbon black, LiMoS2 and polyvinylidene fluoride PVDF were mixed in a weight ratio of 90:3:2:5 and uniformly dispersed in N-methylpyrrolidone to prepare NCM ternary-Li x MoS2 slurry;
[0115] Step 3: Use extrusion coating equipment to coat NCM ternary-Li x The MoS2 slurry is evenly coated on the upper and lower surfaces of the aluminum foil, so that the coating amount on one side is 26 mg / cm 2 After drying, the upper and lower surfaces have NCM ternary-Li x MoS2 coated aluminum foil;
[0116] Step 4: The NCM ternary-Li x The MoS2-coated aluminum foil is rolled, sheared, and dried to obtain a doped positive electrode sheet.
[0117] Comparative Example 5
[0118] Step 1: Use 12μm thick aluminum foil as the positive electrode current collector;
[0119] Step 2: NCA ternary material (LiNi0.8 Co 0.15 Al 0.05 O2), conductive carbon black, Li 0.5 MoS2 and polyvinylidene fluoride PVDF were mixed in a weight ratio of 90:3:2:5 and uniformly dispersed in N-methylpyrrolidone to prepare NCA ternary-Li x MoS2 slurry;
[0120] Step 3: Use extrusion coating equipment to coat NCA ternary-Li x The MoS2 slurry is evenly coated on the upper and lower surfaces of the aluminum foil, so that the coating amount on one side is 26 mg / cm 2 After drying, the upper and lower surfaces have NCA ternary-Li x MoS2 coated aluminum foil;
[0121] Step 4: The NCA ternary-Li x The MoS2-coated aluminum foil is rolled, sheared, and dried to obtain a doped positive electrode sheet.
[0122] Test Case
[0123] The positive electrode sheets prepared in each embodiment and comparative example were cut into pieces with a length of 105 mm and a width of 86 mm. At the same time, a graphite negative electrode (the current collector was an 8 μm thick copper foil, and the negative electrode material layer contained graphite, conductive carbon black and sodium carboxymethyl cellulose in a mass ratio of 97:1.5:1.5, and the surface density was 14 mg / cm 2 ), 12+2+2 ceramic diaphragm as diaphragm, aluminum-plastic film as shell, make laminated soft-pack battery cell, and then inject electrolyte (the solvent is DMC, the lithium salt is LiPF6, and the concentration of lithium salt in the electrolyte is 0.5mol / L), after sealing, standing, formation, and capacity separation, a soft-pack battery is obtained.
[0124] Li x The potential range of MoS2 lithium insertion (about 1.13V) is lower than the lower limit of the working potential range of NMC materials (about 3V). In the formation process, NMC preferentially removes lithium and forms a voltage difference of more than 2.8V with the negative electrode, which exceeds Li x The deintercalation voltage of MoS2 is high, so in the NMC formation stage, Li x MoS2 does not participate in the reaction.
[0125] Each soft pack battery was subjected to a 4.2V-0V over-discharge test, left to stand for 1 day, and then charged to 4.2V with a 1C constant current and constant voltage test, followed by a 4.2V-2.8V 1C cycle test, and the discharge capacity of the battery was recorded. Under the same assembly process, the cycle discharge capacity results of the battery assembled with the doped positive electrode sheet prepared in the embodiment of the present invention and the positive electrode sheet prepared in the comparative example are shown in Table 1 below, and " / " means not tested.
[0126] Table 1: Battery cycle capacity retention rate
[0127]
[0128] It can be seen from the test results that when the doped positive electrode sheets prepared in Examples 1-5 are used in soft-pack laminated batteries, the over-discharge performance is significantly improved, and the capacity after cycling is further utilized.
[0129] The ternary positive electrode sheet prepared in Comparative Example 1 (without Li x MoS2) batteries have very few cycle cycles, with less than 80% of their capacity remaining after 100 cycles.
[0130] In Comparative Examples 2 and 3, Li x The addition amount of MoS2 is higher or lower, and the over-discharge stability performance is improved compared with that of comparative example 1, but the improvement effect is not as good as that of examples 1-5.
[0131] Comparative Example 4 uses LiMoS2 as a positive electrode material layer additive, and the over-discharge stability performance is not improved compared with Comparative Example 1, indicating that LiMoS2 cannot embed lithium ions during over-discharge and cannot suppress the increase in negative electrode potential.
[0132] Comparative Example 5: Li 0.5 When MoS2 is applied to NCA materials, the over-discharge stability of the battery cannot be improved. This is because the positive electrode potential of the battery made of NCA material is higher than that of Li 0.5 The voltage limit of MoS2 is such that lithium ions will not be embedded back into Li 0.5 MoS2 is a good lithium supplement, but during over-discharge, the positive electrode potential drops below 3V and enters Li 0.5 The working potential of MoS2 is such that some lithium ions will be embedded back into the structure, which will destroy the lithium replenishment effect and the capacity of the NCA material under the initial design. This will cause the NCA material to be in a state of power loss during the charge and discharge process, destroying the cycle performance of NCA and making Li 0.5 MoS2 material cannot improve the over-discharge stability of the NCA system.
[0133] The above comparative tests show that the doped positive electrode plate provided by the present invention effectively alleviates the failure problem of the existing ternary positive electrode plate caused by over-discharge, and has high industrial and commercial value.
[0134] It can be seen that compared with the prior art, the doped positive electrode provided by the present invention has a Li x The presence of MoS2 reduces the positive electrode potential during the over-discharge process, which is beneficial to reducing the intersection point of the positive and negative electrode over-discharge potentials, thereby improving the over-discharge stability.
[0135] It can be seen that the doped positive electrode plate provided by the present invention is conducive to improving the over-discharge stability of the battery. Compared with the prior art, the doped positive electrode plate provided by the present invention can effectively solve the problem of over-discharge stability of ternary batteries, greatly improve the overall performance of ternary batteries, and is conducive to improving the market application prospects of battery manufacturers' products, and has great production practical significance.
Claims
1. A positive electrode sheet, It is characterized in that The positive electrode sheet includes a positive electrode current collector and a positive electrode material layer located on the surface of the positive electrode current collector, wherein the positive electrode material layer includes a positive electrode active material and Li x MoS 2 , wherein 0<x≤0.8, Li in the positive electrode material layer x MoS 2 The mass fraction of Li is 1%-3%. x MoS 2 Lithium ions can be inserted into the positive electrode during over-discharge, and the positive electrode active material is lithium nickel cobalt manganese oxide.
2. The positive electrode sheet according to claim 1, It is characterized in that The Li x MoS 2 Where 0.3≤x≤0.
7.
3. The positive electrode sheet according to claim 1, It is characterized in that The mass fraction of the positive electrode active material in the positive electrode material layer is 85%-97%.
4. The positive electrode sheet according to claim 1, It is characterized in that The positive electrode material layer further includes a conductive agent and a binder; preferably, the mass fraction of the conductive agent in the positive electrode material layer is 0.5%-1.5%; preferably, the mass fraction of the binder in the positive electrode material layer is 1%-5%.
5. An electrochemical device, It is characterized in that The electrochemical device comprises the positive electrode sheet according to any one of claims 1 to 4; preferably, the electrochemical device is a lithium-ion battery.
6. The electrochemical device according to claim 5, It is characterized in that The Li in the positive electrode sheet x MoS 2 No delithiation occurred during the first charge.
7. The electrochemical device according to claim 5, It is characterized in that The electrochemical device further comprises a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, and the negative electrode active material is graphite.
8. A method for improving the overdischarge stability of an electrochemical device, It is characterized in that The method comprises using the positive electrode sheet according to any one of claims 1 to 4 in the electrochemical device; preferably, the electrochemical device is a lithium-ion battery.
9. The method according to claim 8, It is characterized in that The method includes making the Li in the positive electrode sheet x MoS 2 No delithiation occurs during the first charge of the electrochemical device.
10. The method according to claim 8, It is characterized in that The electrochemical device further comprises a negative electrode sheet, wherein the negative electrode sheet comprises a negative electrode active material, and the negative electrode active material is graphite.
Citation Information
Patent Citations
Positive pole piece and amorphous carbon lithium battery comprising same
CN106129380A