Electrochemical device and electronic apparatus

By adding titanium, lanthanum and silicon elements to the positive and negative electrode sheets of lithium-ion batteries, the mass content and particle size distribution are optimized, and the conductive network is constructed, and the poor structural stability of lithium-ion batteries is solved in the cyclic attenuation and high-temperature environment of lithium-ion batteries are solved. The problem of high energy density and dynamic performance has been improved.

CN118943290AActive Publication Date: 2024-11-12NINGDE AMPEREX TECHNOLOGY LTD

Patent Information

Application Number
CN202410992748.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

When existing lithium-ion batteries improve weight energy density and kinetic performance, they have fast cycle attenuation and poor structural stability in high-temperature environments, making it difficult to meet the demand for large-scale charging and discharging.

Method used

Add the second particles containing titanium elements to the positive electrode sheet, and add lanthanum and silicon elements to the negative electrode sheet to control their mass content to build a conductive network, optimize the film formation quality and stability of the solid electrolyte film, and at the same time regulate the The proportion and particle size distribution of each element are used to improve the kinetics, thermal stability and high temperature performance of the electrochemical device.

Benefits of technology

It significantly improves the circulation performance, rate performance, expansion suppression performance and high-temperature storage performance of lithium-ion batteries, improves the weight energy density and thermal stability of electrochemical devices, and is suitable for large-scale charging and discharging equipment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004959367100000041
    Figure BDA0004959367100000041
  • Figure BDA0004959367100000121
    Figure BDA0004959367100000121
  • Figure BDA0004959367100000171
    Figure BDA0004959367100000171
Patent Text Reader

Abstract

The invention relates to an electrochemical device and electronic equipment, and belongs to the technical field of energy storage. Wherein the electrochemical device comprises a positive pole piece and a negative pole piece, the positive pole piece comprises a positive pole mixture layer, the negative pole piece comprises a negative pole mixture layer, the mass content of titanium in the positive pole mixture layer is N2%, and 0.08 < = N2 < = 0.2; in the negative electrode mixture layer, the mass content of lanthanum is 3%, 0.1 < = N3 < = 0.5, the mass content of silicon is 4%, and 36 < = N4 < = 40. According to the present invention, the positive electrode mixture layer comprises the titanium element, and the negative electrode mixture layer comprises the lanthanum element, such that the ionic conductivity and the structural stability of the positive electrode mixture layer and the negative electrode mixture layer can be optimized, and the rate performance, the cycle performance, the high temperature performance and the expansion inhibition performance of the secondary battery can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application belongs to the field of energy storage technology, and specifically relates to an electrochemical device and an electronic device. Background Art

[0002] Secondary batteries, as a type of battery that can be repeatedly charged and discharged, play a vital role in the field of modern energy storage. They can not only effectively store electrical energy, but also be used again after charging, greatly improving energy efficiency and environmental protection. Especially in the fields of electric vehicles and mobile devices, the application of secondary batteries is becoming more and more extensive. Among the performance indicators of secondary batteries, kinetic performance is particularly critical. Batteries with excellent kinetic performance mean faster charging and discharging speeds and higher energy conversion efficiency.

[0003] In order to improve the kinetic performance of secondary batteries, the prior art proposes measures such as optimizing the electrolyte formula and improving the battery structure. For example, additives with high ionic conductivity are added to the electrolyte or a porous electrode structure is used to increase the contact area between the electrode and the electrolyte. Although these methods are beneficial to the kinetic performance of secondary batteries, it is necessary to balance the ionic conductivity and chemical stability of the entire electrolyte formula when improving the electrolyte. In addition, improving the battery structure also needs to consider issues such as the feasibility and cost of the production process, and the above measures may also worsen the safety of the battery. Summary of the invention

[0004] In view of this, the present application provides an electrochemical device and an electronic device, in which different solid electrolytes are added to the positive and negative electrode plates respectively. The obtained electrochemical device has the characteristics of high energy density and high rate and long cycle, and has good application prospects.

[0005] In the first aspect, the present application provides an electrochemical device, including a positive electrode plate and a negative electrode plate, the positive electrode plate including a positive electrode mixture layer, the negative electrode plate including a negative electrode mixture layer, wherein the positive electrode mixture layer includes a first particle and a second particle, the first particle contains nickel, cobalt and manganese elements, and the second particle contains titanium; based on the mass of the positive electrode mixture layer, the mass content of the titanium element is N2%, 0.08≤N2≤0.2; the negative electrode mixture layer includes a third particle, the third particle contains silicon and lanthanum; based on the mass of the negative electrode mixture layer, the mass content of the lanthanum element is N3%, 0.1≤N3≤0.5, and the mass content of the silicon element is N4%, 36≤N4≤40.

[0006] The inventors found that when adding a second particle containing titanium to the positive electrode in an electrochemical device of a ternary material-silicon system and controlling the mass content of titanium in the positive electrode mixture layer N2% to satisfy 0.08≤N2≤0.2, a conductive network can be constructed at the positive electrode, while reducing the impedance of the solid electrolyte membrane (CEI membrane) on the surface of the positive electrode material, improving the kinetics of the positive electrode and the cathode potential of the battery cell when fully discharged. However, the increase in cathode potential will lead to a synchronous increase in anode potential, and negative electrode materials, especially silicon materials, are prone to side reactions with electrolytes at high potentials, which can easily damage the solid electrolyte membrane (SEI membrane) on the surface of the negative electrode material, affecting the cycle life and performance of the electrochemical device. On this basis, the inventors added a third particle containing lanthanum to the negative electrode, and controlled the mass content of lanthanum in the negative electrode mixture layer to meet 0.1≤N3≤0.5. After formation, it can partially replace the inorganic components of the SEI film, improve the structural stability of the SEI film and the negative electrode active material, and can also significantly improve the ionic conductivity of the surface of the negative electrode material and the pole piece, and reduce the chemical reaction impedance when lithium ions pass through the SEI film, thereby increasing the deintercalation rate of active substances during battery charging and discharging, and improving the battery's charging and discharging capacity and other kinetic properties. On the other hand, the present application controls the mass content of silicon in the negative electrode mixture layer to meet 36≤N4≤40, which can better cooperate with the negative electrode lanthanum element, improve the weight energy density of the electrochemical device, and enable electrochemical devices with higher weight energy density to be applied to high-rate charging and discharging equipment. Through the combination of the above-mentioned positive electrode titanium element and the negative electrode lanthanum element and silicon element, the heat generated during the lithium ion transmission process can be further reduced, which helps to improve the structural stability of the positive and negative electrode materials, especially in high temperature environments, and is not easy to react with the electrolyte or other battery components, thereby improving the thermal stability and high temperature storage performance of the electrochemical device.

[0007] In some embodiments, 0.005≤(N2+N3) / N4≤0.017. By adjusting the mass content of the above three elements, the first particle, the second particle and the third particle can be closely matched, and the conductive network system is constructed while improving the structural stability of the positive and negative electrodes, further improving the kinetics, thermal stability and high temperature storage performance of the electrochemical device.

[0008] In some embodiments, the first particle further includes neodymium, and based on the mass of the positive electrode mixture layer, the mass content of neodymium is N1%, 0.01≤N1≤0.05. Based on the above system, the present application dopes the first particle with neodymium, which can optimize the crystal structure of the ternary material, and cooperates with the titanium element in the second particle to construct a conductive network path inside and on the surface of the ternary material, improve its structural stability and conductive performance, and is conducive to the electrochemical device to obtain higher thermal stability and kinetic performance.

[0009] In some embodiments, 1.6≤N2 / N1≤10. By adjusting the mass ratio of the neodymium element in the first particle and the titanium element in the second particle, the conductive network of the positive electrode system can be further optimized, so that the electrochemical device can achieve better kinetics and thermal stability.

[0010] In some embodiments, in the first particle, the mass ratio of nickel, cobalt and manganese is (5-9):(0.5-3):(0.5-2). The present application controls the mass ratio of nickel, cobalt and manganese in the ternary material within this range, which helps to improve the conductivity of the ternary material after being combined with the titanium element in the second particle. In addition, the combination with the neodymium element can stabilize the crystal structure of the ternary material, reduce structural damage during high temperature or charging and discharging, and is conducive to improving the thermal stability and cycle performance of the electrochemical device.

[0011] Specifically, the first particle is lithium nickel cobalt manganese oxide, and the chemical formula of lithium nickel cobalt manganese oxide is LiNi a Co b Mn 1-a-b O2, where 0.5≤a≤0.9, 0.05≤b≤0.3, that is, 0.05≤(1-ab)≤0.2.

[0012] In some embodiments, the average particle size of the first particles is D1 μm; the average particle size of the second particles is D2 μm; 22.0≤D1 / D2≤50. When the particle size ratio of the first particles and the second particles is within this range, the distribution of nickel, cobalt, manganese and titanium in the positive electrode sheet can be optimized, a more excellent conductive network system and electrode structure can be obtained, and the kinetic performance and high temperature storage performance of the electrochemical device can be further improved.

[0013] In some embodiments, the third particles have an average particle size of D3 μm, 10≤D3≤15. The third particles with this average particle size can enhance the coordination effect of silicon and lanthanum, optimize the structural stability of the negative electrode, and enhance the kinetics, cycle and high temperature performance of the electrochemical device.

[0014] In some embodiments, 5≤D1≤9.5; and / or, 0.1≤D2≤0.8.

[0015] In some embodiments, the second particle is lithium aluminum titanium phosphate; the chemical formula of lithium aluminum titanium phosphate is Li 1+x Al x Ti 2-x (PO4)3, wherein 0≤x≤0.5; based on the mass of the positive electrode mixture layer, the mass content of lithium aluminum titanium phosphate is M1%, 0.4≤M1≤1.0.

[0016] In some embodiments, the third particle includes lithium lanthanum titanate; the chemical formula of lithium lanthanum titanate is La2 / 3-y Li 3y TiO3, where 0.17≤y≤0.5; based on the mass of the negative electrode mixture layer, the mass content of lithium lanthanum titanate is M2%, 0.5≤M2≤1.5. 1+x Al x Ti 2-x (PO4)3(LATP) is added to the negative electrode, which reacts with lithium ions at a low potential during charging, greatly reducing the initial efficiency of the battery. Therefore, Li-ion, which does not react with lithium ions, is added to the negative electrode side. 3x La 2 / 3-x TiO3(LLTO).

[0017] In some embodiments, the electrolyte includes a compound of formula I; in formula I, R1 is a substituted or unsubstituted C2-C8 cyclic ether group, R2 is a substituted or unsubstituted C1-C5 alkylene group, and R3 is hydrogen or a substituted or unsubstituted C1-C5 alkyl group. Based on the mass of the electrolyte, the mass content of the compound of formula I is N5%, 0.2≤N5≤0.6. In the present application, the addition of the compound of formula I to the electrolyte, in combination with the above-mentioned positive and negative electrode systems, is beneficial to improving the high temperature storage performance and safety performance of the electrochemical device. Although the specific mechanism is still unclear, it is speculated that the compound of formula I is beneficial to improving the film quality and stability of the SEI film and the CEI film, thereby achieving an improvement in the high temperature performance and safety performance of the electrochemical device.

[0018]

[0019] In some embodiments, to further improve the high temperature performance and safety performance of the electrochemical device, the compound shown in Formula I is selected from at least one of 2-tetrahydrofuranyl acrylate, 2-tetrahydrofuranyl methacrylate, and glycidyl acrylate. These compounds can further improve the high temperature performance and safety performance of the electrochemical device under the electrochemical device system of the present application.

[0020] In some embodiments, 0.4≤N5 / N3≤3. By adjusting N3 and N5 to satisfy this relationship, the film formation quality of the SEI film is optimized, thereby further improving the safety performance of the electrochemical device.

[0021] In a second aspect, the present application further provides an electronic device, comprising any one of the electrochemical devices provided in the first aspect of the present application. Since the electronic device comprises the electrochemical device provided in the present application, the electronic device has the same advantages as the electrochemical device.

[0022] Based on the electrochemical device and electronic device provided by the present application, by adding the second particle and the third particle to the positive and negative electrode sheets respectively, the inorganic components of the CEI film and the SEI film can be partially replaced after formation, on the one hand, the consumption of active materials in the film formation stage is reduced, which is conducive to maintaining a high energy density, and on the other hand, a conductive network path is constructed, so that the electrochemical device has a high kinetic performance and excellent rate cycle performance, and it also helps to improve the structural stability of the active material, reduce heat generation, and improve the thermal stability and high temperature storage performance of the electrochemical device. After being matched with the compound of formula I in the electrolyte, it is also conducive to further improving the high temperature stability and safety performance of the electrochemical device, and has an excellent application prospect. DETAILED DESCRIPTION

[0023] In order to make the purpose, technical solution and advantages of the present application more clear, the present application is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described here are only used to explain the present application and are not used to limit the present application.

[0024] The electrochemical device of the present application is not particularly limited, and may include any device in which an electrochemical reaction occurs, such as a secondary battery. The present application is described below using a secondary battery as an example in conjunction with the embodiments of the present application. In some embodiments of the present application, the secondary battery may include, but is not limited to: a lithium-ion secondary battery (lithium-ion battery) or a sodium-ion battery. It should be noted that in the specific embodiments of the present application, the present application is explained using a secondary battery as an example of an electrochemical device, but the electrochemical device of the present application is not limited to a secondary battery.

[0025] When improving the weight energy density of lithium-ion batteries, the prior art generally uses ternary materials combined with silicon-containing materials to construct a lithium-ion battery system. Ternary materials can increase the gram capacity of the positive electrode, and the introduction of high-capacity silicon-containing materials into the negative electrode can significantly increase the capacity of the negative electrode. However, the inventors found during the research process that the ternary combined with silicon system cannot achieve high-rate charge and discharge requirements due to the kinetic limitations of the positive and negative electrodes, and the cycle decay is fast. At present, conventional methods for improving kinetics include reducing the coating weight of the positive and negative electrodes, reducing the ratio of negative electrode silicon materials, and reducing the negative electrode adhesive. However, the methods of reducing the coating weight of the positive and negative electrodes and reducing the silicon negative electrode will lead to a decrease in the weight energy density of the battery, and reducing the negative electrode adhesive will cause the silicon negative electrode to expand cyclically and destroy the conductive network, resulting in accelerated decay.

[0026] In order to solve the above problems, the present application provides an electrochemical device, including a positive electrode plate and a negative electrode plate, the positive electrode plate includes a positive electrode mixture layer, the negative electrode plate includes a negative electrode mixture layer, wherein the positive electrode mixture layer includes a first particle and a second particle, the first particle contains nickel, cobalt and manganese, and the second particle contains titanium; based on the mass of the positive electrode mixture layer, the mass content of the titanium element is N2%, 0.08≤N2≤0.2; the negative electrode mixture layer includes a third particle, the third particle contains silicon and lanthanum; based on the mass of the negative electrode mixture layer, the mass content of the lanthanum element is N3%, 0.1≤N3≤0.5, and the mass content of the silicon element is N4%, 36≤N4≤40. The present application adds a second particle containing titanium to the positive electrode, which can improve the structural stability of the positive electrode material and reduce the structural changes of the positive electrode material during the cycle. The negative electrode uses lanthanum and silicon elements to increase the capacity of the negative electrode while improving the structural stability and thermal stability of the negative electrode material, slowing down the structural changes of the negative electrode material under high temperature or cycle conditions, reducing the thickness expansion of the secondary battery, and improving its safety and stability. On the other hand, after strengthening the positive and negative electrode materials respectively with titanium and lanthanum elements, a conductive network can be constructed to improve the rate performance of the secondary battery, and it is also beneficial to improve the film quality and stability of the solid electrolyte interface film (CEI film and SEI film), thereby slowing down the degradation rate of the electrolyte under high temperature or cycle conditions, and improving the high temperature performance and cycle performance of the secondary battery.

[0027] In some embodiments, N2 is 0.08, 0.09, 0.10, 0.11, 0.12, 0.13, 0.14, 0.15, 0.16, 0.17, 0.18, 0.19, 0.2, or a value within the range of any two of these values. Regulating the mass content of titanium in the positive electrode mixture layer within the above range can further optimize the ionic conductivity and structural stability of the positive electrode material, and improve the rate performance, cycle performance, and high temperature performance of the secondary battery.

[0028] In some embodiments, N3 is 0.1, 0.13, 0.14, 0.17, 0.19, 0.24, 0.25, 0.29, 0.33, 0.37, 0.40, 0.44, 0.46, 0.5 or a value within the range of any two of these values. The present application regulates the mass content of lanthanum in the negative electrode mixture layer within the above range, which is conducive to better coordination with silicon, optimizing the ionic conductivity and structural stability of the negative electrode material, and improving the rate performance, cycle performance, high temperature performance and expansion inhibition performance of the secondary battery.

[0029] In some embodiments, N4 is 36, 36.1, 36.5, 36.7, 37.0, 37.3, 37.7, 38.0, 38.2, 38.6, 38.8, 39.2, 39.5, 39.7, 40, or a value within the range of any two of these values. When the silicon content is within the above range, the energy density can be increased while improving the rate performance, cycle performance, high temperature performance and expansion inhibition performance of the secondary battery.

[0030] In some embodiments of the present application, the first particle is a ternary material of lithium nickel cobalt manganese oxide, and the second particle is lithium aluminum titanium phosphate (LATP).

[0031] In some embodiments of the present application, the chemical formula of lithium nickel cobalt manganese oxide is LiNi a Co b Mn 1-a-b O2, wherein 0.5≤a≤0.9, 0.05≤b≤0.3, that is, 0.05≤(1-ab)≤0.2. Exemplarily, lithium nickel cobalt manganese oxide is selected from LiNi 0.8 Mn 0.1 Co 0.1 O2(NCM811), LiNi 0.6 Mn 0.1 Co 0.3 O2(NCM613), LiNi 0.6 Mn 0.2 Co 0.2 O2、LiNi 0.5 Mn 0.2 Co 0.3 O2、LiNi 0.7 Mn 0.15 Co 0.15 At least one of O2.

[0032] In some embodiments, the second particle is lithium aluminum titanium phosphate; the chemical formula of lithium aluminum titanium phosphate is Li 1+x Al x Ti 2-x (PO4)3, where 0≤x≤0.5. Optionally, the ionic conductivity of LATP is in the range of 10 -3 to 10 -2 In the secondary battery system of the present application, LATP forms compounds such as Li2CO3 and LiOH on the surface of the positive electrode, which can form a stable interface layer on the positive electrode, improve the thermal stability and high-temperature storage performance of the positive electrode, and reduce the risk of thermal runaway or combustion of the battery.

[0033] The present application has no special requirements for the method of regulating the mass content of titanium in the positive electrode mixture layer, as long as it can meet the above-mentioned mass content range. For example, the amount of lithium titanium aluminum phosphate added can be adjusted, or lithium titanium aluminum phosphate with different titanium content can be added.

[0034] In some embodiments, 0.005≤(N2+N3) / N4≤0.017. In some embodiments, the value of (N2+N3) / N4 is 0.005, 0.006, 0.007, 0.008, 0.009, 0.010, 0.011, 0.012, 0.013, 0.014, 0.015, 0.016, 0.017 or a value in the range of any two of these values. By regulating the mass content of titanium, lanthanum and silicon to meet the above relationship, the elements can be closely matched to further improve the rate performance, cycle performance, high temperature performance and expansion inhibition performance of the secondary battery.

[0035] In some embodiments, the first particles further include neodymium, and based on the mass of the positive electrode mixture layer, the mass content of the neodymium is N1%, 0.01≤N1≤0.05. In some embodiments, N1 is 0.01, 0.013, 0.014, 0.017, 0.020, 0.024, 0.025, 0.031, 0.034, 0.037, 0.040, 0.043, 0.046, 0.049, 0.05, or a value within the range of any two of these values. Among them, the neodymium element can be added by doping. The present application does not specifically limit the method of adding the neodymium element, as long as the mass content of the neodymium element can be maintained within the above range. For example, during the preparation process, the oxide of the neodymium metal (such as neodymium oxide (Nd2O3)) can be mixed with the ternary material and then incorporated into the lattice of the ternary material during the sintering process. When the mass content of the neodymium element in the positive electrode mixture layer is regulated within the above range, the crystal structure of the ternary material can be optimized, the structural stability and conductivity of the latter can be improved, and the rate performance, cycle performance, high temperature performance and expansion inhibition performance of the secondary battery can be optimized.

[0036] In some embodiments, 1.6≤N2 / N1≤10. In some embodiments, the value of N2 / N1 is 1.6, 1.7, 2.3, 3.0, 3.7, 4.7, 5.0, 5.9, 6.7, 6.8, 7.8, 8.5, 9.3, 9.5, 10 or a value in the range of any two of these values. By further regulating the content of the neodymium element in the first particle and the titanium element in the second particle to meet the above range, the structural stability and conductivity of the positive electrode system can be optimized, thereby significantly improving the rate performance, cycle performance, high temperature performance and expansion inhibition performance of the secondary battery.

[0037] In some embodiments, the average particle size of the first particles is D1 μm; the average particle size of the second particles is D2 μm; 22.0≤D1 / D2≤50. In some embodiments, the value of D1 / D2 is 22, 23, 25, 28, 29, 31, 35, 36, 39, 41, 43, 44, 47, 49, 50 or a value within the range of any two of these values. The present application regulates the average particle size of the first particles and the second particles to satisfy the above relationship, which helps to optimize the distribution state of nickel, cobalt, manganese and titanium elements, obtain a more excellent conductive network system and electrode structure, and further improve the kinetic performance and high temperature storage performance of the secondary battery.

[0038] In some embodiments, 5≤D1≤9.5, 0.1≤D2≤0.8. In some embodiments, D1 is 5, 5.3, 5.4, 5.9, 6.3, 6.4, 6.9, 7.3, 7.5, 8.0, 8.4, 8.7, 9.0, 9.3, 9.5 or a value within the range of any two of these values. In some embodiments, D2 is 0.1, 0.11, 0.19, 0.23, 0.29, 0.33, 0.38, 0.42, 0.49, 0.57, 0.62, 0.64, 0.70, 0.78, 0.8 or a value within the range of any two of these values. The present application regulates the particle sizes of the first particles and the second particles to meet the above ranges respectively, which can better optimize the distribution of nickel, cobalt, manganese and titanium in the positive electrode, and improve the rate performance, thermal stability and cycle performance of the secondary battery.

[0039] In some embodiments, the ionic resistance of the positive electrode sheet is 20 mΩ / mm 2 Up to 100mΩ / mm 2 In some embodiments, the ionic resistance of the positive electrode sheet is 20 mΩ / mm 2 , 26mΩ / mm 2 , 27mΩ / mm 2 、38mΩ / mm 2 , 41mΩ / mm 2 、47mΩ / mm 2 、54mΩ / mm 2 、61mΩ / mm 2 、69mΩ / mm 2 、72mΩ / mm 2 、77mΩ / mm 2 、86mΩ / mm 2 、89mΩ / mm 2 、98mΩ / mm 2 , 100mΩ / mm 2Or a value within a range consisting of any two of these values. Optionally, the porosity of the positive electrode sheet is 20% to 35%. In some embodiments, the porosity of the positive electrode sheet is 20%, 20.7%, 22.3%, 23.1%, 23.5%, 25.7%, 26.6%, 27.4%, 28.6%, 30.2%, 30.8%, 32.5%, 33.5%, 34.1%, 35%, or a value within a range consisting of any two of these values. Exemplarily, the adhesion of the positive electrode sheet is 10N / m to 20N / m. In some embodiments, the adhesion force of the positive electrode sheet is 10 N / m, 10.1 N / m, 11.3 N / m, 12.2 N / m, 12.9 N / m, 13.1 N / m, 14.2 N / m, 15.3 N / m, 15.7 N / m, 16.3 N / m, 17.4 N / m, 17.9 N / m, 18.6 N / m, 19.5 N / m, 20 N / m or a value within the range formed by any two of these values.

[0040] The positive electrode sheet in the present application also includes a positive current collector. The present application has no particular restrictions on the positive current collector, as long as the purpose of the present application can be achieved. For example, the positive current collector may include aluminum foil, aluminum alloy foil or a composite current collector (such as an aluminum-carbon composite current collector). The present application has no particular restrictions on the thickness of the positive current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the positive current collector is 5μm to 20μm.

[0041] In the present application, the positive electrode mixture layer can be arranged on one side surface in the thickness direction of the positive electrode current collector, or on both side surfaces in the thickness direction of the positive electrode current collector. It should be noted that the "surface" can be the entire area of ​​the positive electrode current collector, or it can be a partial area of ​​the positive electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved.

[0042] In the present application, the positive electrode mixture layer also includes a positive electrode conductive agent. The present application has no special restrictions on the positive electrode conductive agent, as long as the purpose of the present application can be achieved. For example, it may include but is not limited to at least one of conductive carbon black (Super P), carbon nanotubes (CNTs), carbon fibers, graphene, metal materials or conductive polymers. The above-mentioned carbon nanotubes may include but are not limited to single-walled carbon nanotubes and / or multi-walled carbon nanotubes. The above-mentioned carbon fibers may include but are not limited to vapor-grown carbon fibers (VGCF) and / or nano-carbon fibers. The above-mentioned metal materials may include but are not limited to metal powders and / or metal fibers. Specifically, the metal may include but is not limited to at least one of copper, nickel, aluminum or silver. The above-mentioned conductive polymers may include but are not limited to at least one of polyphenylene derivatives, polyaniline, polythiophene, polyacetylene or polypyrrole.

[0043] In the present application, the positive electrode mixture layer also includes a positive electrode binder. The present application has no special restrictions on the positive electrode binder as long as the purpose of the present application can be achieved. For example, it may include but is not limited to at least one of polyacrylate, polyimide, polyamide, polyamideimide, polyvinylidene fluoride, polytetrafluoroethylene, polyvinyl alcohol, polyacrylonitrile, polystyrene butadiene copolymer, sodium alginate, sodium carboxymethyl cellulose, potassium carboxymethyl cellulose, sodium hydroxymethyl cellulose or potassium hydroxymethyl cellulose.

[0044] In some embodiments of the present application, the third particle is a mixture of a silicon-containing material and lithium lanthanum titanate (LLTO). In the present application, the chemical formula of lithium lanthanum titanate is La 2 / 3-y Li 3y TiO3, where 0.17≤y≤0.5.

[0045] In some embodiments, the average particle size of the third particles is D3 μm, 10≤D3≤15. Exemplarily, the average particle size D3 of the third particles is 10, 10.3, 10.7, 10.8, 11.2, 11.8, 12.1, 12.6, 12.9, 13.4, 13.5, 14.1, 14.4, 14.9, 15 or a value in the range of any two of these values. When the average particle size of the third particles is regulated within the above range, the structural stability of the negative electrode material can be optimized, while promoting the improvement of the negative electrode conductivity, and better improving the rate, cycle and high temperature performance of the secondary battery.

[0046] In some optional embodiments, the ionic conductivity of LLTO is in the range of 10 -6 S / cm to 10 -5 S / cm.

[0047] In some optional embodiments, the ionic resistance of the negative electrode plate is 20 mΩ / mm 2 Up to 50mΩ / mm 2 In some embodiments, the ionic resistance of the negative electrode plate is 20 mΩ / mm 2 , 22mΩ / mm 2 , 23mΩ / mm 2 , 26mΩ / mm 2 , 28mΩ / mm 2 、31mΩ / mm 2 、32mΩ / mm 2 、36mΩ / mm 2 、38mΩ / mm 2 , 40mΩ / mm 2 , 43mΩ / mm 2 、45mΩ / mm 2 、47mΩ / mm 2 , 48mΩ / mm 2, 50mΩ / mm 2 Or a value within the range consisting of any two of these values.

[0048] In some optional embodiments, the porosity of the negative electrode sheet is 15% to 35%. For example, the porosity of the negative electrode sheet is 15%, 16%, 17%, 18%, 21%, 22%, 24%, 25%, 26%, 29%, 29%, 32%, 33%, 34%, 35% or a value in the range composed of any two of these values. After 50 cycles of the cycle process in the cycle retention test of the present application, the increase in the porosity of the electrode sheet does not exceed 5%, and the pore size range corresponding to the maximum pore volume is 0.6 to 2 μm, and the proportion of the pore size volume above 1 μm to the total pore volume is 0 to 20%, indicating that the secondary battery system of the present application can reduce the expansion of silicon-based materials and improve structural stability through the coordination of various components, thereby helping to improve the cycle performance and inhibit expansion performance of the secondary battery.

[0049] Optionally, the adhesion of the negative electrode sheet is 20 N / m to 50 N / m. In some embodiments, the adhesion of the negative electrode sheet is 20 N / m, 21 N / m, 22 N / m, 25 N / m, 28 N / m, 30 N / m, 33 N / m, 35 N / m, 37 N / m, 39 N / m, 41 N / m, 44 N / m, 46 N / m, 49 N / m, 50 N / m, or a value in the range of any two of these values.

[0050] The negative electrode sheet of the present application also includes a negative electrode current collector. In the present application, the negative electrode mixture layer can be arranged on the surface on one side in the thickness direction of the negative electrode current collector, or on the surfaces on both sides in the thickness direction of the negative electrode current collector. It should be noted that the "surface" here can be the entire area of ​​the negative electrode current collector, or it can be a partial area of ​​the negative electrode current collector. This application has no special restrictions, as long as the purpose of this application can be achieved. This application has no special restrictions on the thickness of the negative electrode mixture layer, as long as the purpose of this application can be achieved. For example, the thickness of a single-sided negative electrode mixture layer can be 30μm to 160μm.

[0051] The present application has no particular restrictions on the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the negative electrode current collector may include copper foil, copper alloy foil, nickel foil, stainless steel foil, titanium foil, nickel foam, copper foam or composite current collector (such as carbon copper composite current collector, nickel copper composite current collector, titanium copper composite current collector), etc. The present application has no particular restrictions on the thickness of the negative electrode current collector, as long as the purpose of the present application can be achieved. For example, the thickness of the negative electrode current collector is 4μm to 10μm.

[0052] In the present application, the negative electrode mixture layer may also include a negative electrode binder. The present application has no particular limitation on the negative electrode binder as long as the purpose of the present application can be achieved. For example, it may include but is not limited to at least one of polyvinyl alcohol, carboxymethyl cellulose, hydroxypropyl cellulose, diacetyl cellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene oxide-containing polymers, polyvinyl pyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyacrylic acid, styrene-butadiene rubber, acrylic (ester) styrene-butadiene rubber, epoxy resin or nylon.

[0053] In the present application, the electrochemical device also includes an electrolyte, and the electrolyte includes a lithium salt and a non-aqueous solvent. The lithium salt may include at least one of LiPF6, LiBF4, LiAsF6, LiClO4, LiB(C6H5)4, LiCH3SO3, LiCF3SO3, LiN(SO2CF3)2, LiC(SO2CF3)3, Li2SiF6, lithium bis(oxalate borate) (LiBOB) or lithium difluoroborate. The present application does not particularly limit the concentration of the lithium salt in the electrolyte, as long as the purpose of the present application can be achieved. For example, the concentration of the lithium salt in the electrolyte is 0.9mol / L to 1.5mol / L. For example, the concentration of the lithium salt in the electrolyte can be 0.9mol / L, 1.0mol / L, 1.1mol / L, 1.3mol / L, 1.5mol / L or a range consisting of any two of the above values. The present application has no particular restrictions on non-aqueous solvents, as long as the purpose of the present application can be achieved, for example, it may include but is not limited to at least one of carbonate compounds, carboxylate compounds, ether compounds or other organic solvents. The above-mentioned carbonate compounds may include but are not limited to at least one of linear carbonate compounds, cyclic carbonate compounds or fluorinated carbonate compounds. The above-mentioned linear carbonate compounds may include but are not limited to at least one of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC) or ethyl methyl carbonate (MEC). The above-mentioned cyclic carbonate may include but is not limited to at least one of ethylene carbonate (EC), propylene carbonate (PC), butylene carbonate (BC) or vinyl ethylene carbonate (VEC). The fluorinated carbonate compound may include, but is not limited to, at least one of fluoroethylene carbonate (FEC), 1,2-difluoroethylene carbonate, 1,1-difluoroethylene carbonate, 1,1,2-trifluoroethylene carbonate, 1,1,2,2-tetrafluoroethylene carbonate, 1-fluoro-2-methylethylene carbonate, 1-fluoro-1-methylethylene carbonate, 1,2-difluoro-1-methylethylene carbonate, 1,1,2-trifluoro-2-methylethylene carbonate, or trifluoromethylethylene carbonate. The above-mentioned carboxylate compound may include, but is not limited to, at least one of methyl formate, methyl acetate, ethyl acetate, n-propyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, γ-butyrolactone, decalactone, valerolactone, or caprolactone. The ether compound may include, but is not limited to, at least one of dibutyl ether, tetraglyme, diglyme, 1,2-dimethoxyethane, 1,2-diethoxyethane, 1-ethoxy-1-methoxyethane, 2-methyltetrahydrofuran or tetrahydrofuran.The above-mentioned other organic solvents may include but are not limited to at least one of dimethyl sulfoxide, 1,2-dioxolane, sulfolane, methyl sulfolane, 1,3-dimethyl-2-imidazolidinone, N-methyl-2-pyrrolidone, dimethylformamide, acetonitrile, trimethyl phosphate, triethyl phosphate or trioctyl phosphate.

[0054] In some embodiments, the electrolyte includes a compound shown in Formula I; in Formula I, R1 is a substituted or unsubstituted C2-C8 cyclic ether group, R2 is a substituted or unsubstituted C1-C5 alkylene group, and R3 is hydrogen or a substituted or unsubstituted C1-C5 alkyl group. Based on the mass of the electrolyte, the mass content of the compound shown in Formula I is N5%, 0.2≤N5≤0.6. In some embodiments, N5 is 0.2, 0.22, 0.24, 0.27, 0.30, 0.34, 0.37, 0.39, 0.45, 0.45, 0.49, 0.54, 0.55, 0.57, 0.6 or a value within the range composed of any two of these values. The present application adds the compound shown in Formula I to the electrolyte, and further regulates the mass content of the compound of Formula I in the electrolyte within the above range, which can improve the high temperature performance and safety performance of the secondary battery.

[0055]

[0056] In some embodiments, the compound represented by formula I is selected from at least one of 2-tetrahydrofuranyl acrylate, 2-tetrahydrofuranyl methacrylate, and glycidyl acrylate. The use of these compounds in the electrolyte in combination with the positive and negative electrode systems of the present application can further improve the high temperature performance and safety performance of the secondary battery.

[0057] In some embodiments, 0.4≤N5 / N3≤3. In some embodiments, the value of N5 / N3 is 0.4, 0.6, 0.7, 0.9, 1.0, 1.3, 1.6, 1.7, 1.8, 2.2, 2.3, 2.5, 2.7, 2.8, 3 or a value in the range of any two of these values. By regulating the mass content of the compound of formula I in the electrolyte and the mass content of the lanthanum element in the negative electrode mixture layer to meet the above relationship, the high temperature performance and safety performance of the secondary battery can be significantly improved.

[0058] The secondary battery of the present application also includes a separator. The present application has no special restrictions on the separator, as long as the purpose of the present application can be achieved. For example, the material of the separator may include but is not limited to polyethylene (PE), polypropylene (PP), polytetrafluoroethylene-based polyolefin (PO) separators, polyester films (such as polyethylene terephthalate (PET) films), cellulose films, polyimide films (PI), polyamide films (PA), spandex or aramid films, etc. At least one of the types of separators may include but is not limited to woven membranes, non-woven membranes (non-woven fabrics), microporous membranes, composite membranes, rolled membranes or spinning membranes, etc. The separator of the present application may have a porous structure, and the size of the pore size is not particularly limited, as long as the purpose of the present application can be achieved. For example, the size of the pore size can be 0.01 μm to 1 μm. In the present application, the thickness of the separator is not particularly limited, as long as the purpose of the present application can be achieved. For example, the thickness can be 5 μm to 500 μm.

[0059] The secondary battery of the present application also includes a packaging bag for containing a positive electrode sheet, a separator, a negative electrode sheet and an electrolyte, as well as other components known in the art in the secondary battery, and the present application does not limit the above other components. The present application does not specifically limit the packaging bag, and it can be a packaging bag known in the art, as long as it can achieve the purpose of the present application.

[0060] The secondary battery of the present application is not particularly limited, and may include any device that undergoes an electrochemical reaction. In one embodiment of the present application, the secondary battery may include, but is not limited to, a lithium ion secondary battery (lithium ion battery), a lithium metal secondary battery, a lithium polymer secondary battery, or a lithium ion polymer secondary battery. In one embodiment, the structure of the electrode assembly includes a winding structure or a laminated structure.

[0061] The preparation process of the secondary battery of the present application is well known to those skilled in the art, and the present application has no special restrictions. For example, it may include but is not limited to the following steps: stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and winding, folding and other operations as needed to obtain an electrode assembly of a winding structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain a secondary battery; or stacking the positive electrode sheet, the separator and the negative electrode sheet in order, and then fixing the four corners of the entire stacked structure with tape to obtain an electrode assembly of a stacked structure, placing the electrode assembly in a packaging bag, injecting the electrolyte into the packaging bag and sealing it to obtain a secondary battery. In addition, overcurrent protection elements, guide plates, etc. may also be placed in the packaging bag as needed to prevent the pressure inside the secondary battery from rising and overcharging and discharging.

[0062] The present application has no limitation on the packaging bag, and those skilled in the art can select it according to actual needs, as long as the purpose of the present application can be achieved. For example, an aluminum-plastic film packaging bag can be used.

[0063] In a second aspect, the present application further provides an electronic device, comprising the electrochemical device provided in the first aspect of the present application.

[0064] The electronic device of the present application is not particularly limited, and it can be used for any electronic device known in the prior art. In some embodiments, the electrochemical device of the present application can be used for, but not limited to, laptop computers, pen-input computers, mobile computers, e-book players, portable phones, portable fax machines, portable copiers, portable printers, head-mounted stereo headphones, video recorders, LCD televisions, portable cleaners, portable CD players, mini-discs, transceivers, electronic notepads, calculators, memory cards, portable recorders, radios, backup power supplies, motors, cars, motorcycles, power-assisted bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household batteries and lithium-ion capacitors, etc.

[0065] The scheme of the present application is described below in conjunction with the following specific examples. Unless otherwise specified, the raw materials used in the following examples are all from common commercial products, and the devices or equipment used are all purchased from conventional market sales channels. Various tests and evaluations are carried out according to the following methods. In addition, unless otherwise specified, "parts" and "%" are mass references.

[0066] Example 1

[0067] The present embodiment provides a lithium-ion battery, including a positive electrode plate and a negative electrode plate, wherein the positive electrode plate includes a positive electrode mixture layer, and the negative electrode plate includes a negative electrode mixture layer, wherein the positive electrode mixture layer includes a first particle and a second particle, and the first particle is a lithium nickel cobalt manganese oxide NCM811 doped with neodymium, containing neodymium, nickel, cobalt and manganese, and the chemical formula of the lithium nickel cobalt manganese oxide is LiNi 0.8 Co 0.1 Mn 0.1 O2, the mass ratio of nickel, cobalt and manganese is 8:1:1. The second particle is lithium aluminum titanium phosphate, and the chemical formula of lithium aluminum titanium phosphate is Li 1.1 Al 0.1 Ti 1.9 (PO4)3. Based on the mass of the positive electrode mixture layer, the mass content of neodymium is N1%=0.02%, the mass content of titanium is N2%, N2=0.1, and N2 / N1=5. The average particle size D1μm of the first particles is 5.5μm; the average particle size D2μm of the second particles is 0.2μm; 10≤D1 / D2≤47.

[0068] The negative electrode mixture layer includes a third particle, the third particle includes silicon and lithium lanthanum titanate, and the chemical formula of lithium lanthanum titanate is La 2 / 3-y Li 3yTiO3. Based on the mass of the negative electrode mixture layer, the mass content of lanthanum is N3%, N3=0.1, and the mass content of silicon is N4%, N4=36. The average particle size D3μm of the third particles is 11μm. (N2+N3) / N4=0.56.

[0069] The preparation process of the lithium ion battery of this embodiment includes the following steps:

[0070] 1) Positive electrode

[0071] The positive electrode active material, lithium nickel cobalt manganese oxide (NCM811), conductive agent Super P and CNT, binder polyvinylidene fluoride (PVDF), and LATP are mixed, wherein the positive electrode active material, conductive agent Super P, conductive agent CNT, PVDF, and LATP are in a weight ratio of 97.0:0.8:0.5:1.3:0.4, the positive electrode material and LATP are first blended, and then all the materials are fully stirred and mixed in an appropriate amount of N-methylpyrrolidone (NMP) solvent to form a uniform positive electrode slurry, wherein the solid content of the positive electrode slurry is 75wt%. The slurry is coated on the positive electrode current collector aluminum foil, dried at 85°C, and then cold pressed, cut, and cut, and then dried under vacuum conditions at 85°C for 4 hours to obtain a positive electrode sheet.

[0072] 2) Negative electrode

[0073] Graphite, silicon-carbon material, LLTO, styrene-butadiene rubber (SBR) and sodium carboxymethyl cellulose (CMC) were fully stirred and mixed in a proper amount of deionized water in a weight ratio of 44:50:1:4:1 to form a uniform negative electrode slurry, wherein the solid content of the negative electrode slurry was 50wt%. The slurry was coated on the negative electrode current collector (copper foil), dried at 85°C, and then cold pressed, cut and slit, and dried under vacuum conditions at 120°C for 12 hours to obtain a negative electrode sheet.

[0074] 3) Electrolyte

[0075] Ethylene carbonate (EC), propylene carbonate (PC) and diethyl carbonate (DEC) are mixed in a mass ratio of EC:PC:DEC=50:20:30 to obtain a solvent, and then lithium salt LiPF6 is added to the solvent. After mixing evenly, an electrolyte is obtained, wherein the mass content of LiPF6 is 1.15% based on the mass of the electrolyte.

[0076] 4) Isolation film

[0077] A 5 μm thick polyethylene (PE) porous polymer film was used as the isolation membrane.

[0078] The positive electrode sheet, the separator, and the negative electrode sheet are stacked in order, so that the separator is between the positive and negative electrodes to play an isolating role. Then they are wound, the pole ears are welded, and placed in the outer packaging foil aluminum-plastic film. The electrolyte is injected, and after vacuum packaging, standing, formation, capacity testing and degassing, a soft-pack lithium-ion battery is obtained.

[0079] Test method:

[0080] Average particle size test:

[0081] The particle size distribution of the particles to be tested (e.g., the first particles, the second particles, or the third particles) is tested using a Malvern particle size tester (the instrument model is Master Sizer 2000). The sample preparation method is as follows: 0.02 g of the powder sample of the particles to be tested is added to a 50 mL clean beaker, and about 20 mL of deionized water is added, and ultrasonic cleaning is performed in a 120 W ultrasonic cleaning machine for 5 minutes to uniformly disperse the powder in the water to obtain the particle size test sample of the particles to be tested.

[0082] Alternatively, after the electrode (positive electrode or negative electrode) is subjected to argon ion polishing, a SEM photo of the sample is taken by a scanning electron microscope, and then 20 particles to be tested are randomly selected from the SEM photo using image analysis software, and the cross-sectional area S of the particles to be tested is counted. Then, assuming that the particles to be tested are spherical, the particle size R (diameter) of each particle is calculated by the following formula: R = 2 × (S / π) 1 / 2 ; Take the arithmetic average of the particle sizes R of each particle to obtain the average particle size of the particles to be measured.

[0083] Element content test:

[0084] After the electrode (positive electrode or negative electrode) is subjected to argon ion polishing and sample preparation, elemental analysis is performed using an energy dispersive spectrometer (EDS) coupled to a field emission scanning electron microscope to test the content of the element to be tested.

[0085] Cycle performance test (400 cycles capacity retention rate):

[0086] Place the lithium-ion battery in a constant temperature box at 25°C ± 1°C for 30 minutes, charge it to 4.3V at a constant current of 0.5C, charge it to 0.025C at a constant voltage of 4.3V, place it for 5 minutes, and then discharge it to 2.8V at 0.5C. This is a charge and discharge cycle. Record the first cycle discharge capacity C0 of the lithium-ion battery. After that, cycle it 400 times according to the above cycle process. Record the cycle discharge capacity C1 of the 400th cycle. 400 cycle capacity retention rate = C1 / C0×100%.

[0087] 4C rate discharge capacity retention rate:

[0088] The lithium-ion battery was placed in a constant temperature box at 25℃±1℃ for 30 minutes, charged to 4.3V at 0.5C constant current, then charged to 0.025C at 4.3V constant voltage, allowed to stand for 5 minutes, then discharged to 2.8V at 0.5C, and the discharge capacity was recorded as C2. The battery was then charged to 4.3V at 0.5C constant current, then charged to 0.025C at 4.3V constant voltage, allowed to stand for 5 minutes, then discharged to 2.8V at 4C, and the discharge capacity was recorded as C3. 4C discharge capacity retention rate = C3 / C2×100%.

[0089] Cyclic expansion rate (thickness expansion rate):

[0090] The initial thickness of the lithium-ion battery before cycling is measured by a spiral micrometer as H0. When the lithium-ion battery is cycled 400 times according to the above cycle performance test process, the thickness of the lithium-ion battery is measured by a spiral micrometer in a fully charged state (charged to 0.025C at a constant voltage of 4.3V). The expansion rate of 400 cycles = (H1-H0) / H0×100%.

[0091] High temperature storage performance (80℃24h storage thickness expansion rate test):

[0092] The lithium-ion battery was placed in a constant temperature box at 25°C ± 1°C for 30 minutes, charged to 4.3V at a constant current of 0.5C, and then charged to 0.025C at a constant voltage of 4.3V, and placed for 5 minutes. The initial thickness of the lithium-ion battery before cycling was measured with a screw micrometer, which was H0; then the temperature was raised to 80°C and maintained for 24h, and the thickness of the lithium-ion battery was measured with a screw micrometer, which was H1. The thickness expansion rate after 24h storage at 80°C = (H1-H0) / H0×100%.

[0093] Hot box test:

[0094] The specific method of the hot box test is as follows: (a) adjust the furnace temperature to 25°C, take 10 lithium-ion batteries of the embodiment or comparative example to be tested as samples and place them in the furnace for 5 minutes; (b) 0.2C constant current discharge (DC) to 2.8V; (c) stand for 10 minutes; (d) 0.7C constant current charge (CC) to 4.3V, and then charge to 0.025C at 4.3V constant voltage (CV); (e) stand for 10 minutes; (f) take pictures before the test, measure the voltage internal resistance, and attach the temperature sensing wire to the surface of the battery, then put the sample into the heating furnace box, and heat it to the target temperature of 130°C at a heating rate of 5±2°C / min and keep it for 60 minutes. After the test, take pictures and measure the voltage internal resistance. If the battery does not catch fire or explode, it means that it has passed the hot box test, which is recorded as P.

[0095] Repeat the above (a)-(e) and (f) before the test, take photos, measure the voltage and internal resistance, and stick the temperature-sensing wire on the battery surface, then put the sample into the heating furnace, and heat it to the target temperature of 132°C at a rate of 5±2°C / min and keep it for 60 minutes. After the test, take photos and measure the voltage and internal resistance. If the battery does not catch fire or explode, it means that it has passed the hot box test, which is recorded as P. For example, 4P / 10T means that four out of 10 tested lithium-ion batteries have passed the hot box test.

[0096] The lithium-ion batteries of the embodiments and comparative examples in Table 1 differ from those of Embodiment 1 only in that the mass content of titanium in the positive electrode mixture layer is N2%, the mass content of lanthanum in the negative electrode mixture layer is N3%, and the mass content of silicon is N4%, and the mathematical relationship of (N2+N3) / N4 is different. The specific differences and corresponding test results are shown in Table 1 below.

[0097] Table 1

[0098]

[0099] As can be seen from Table 1, the present application adds titanium to the positive electrode and adjusts its mass content N2% to meet 0.08≤N2≤0.2, and adds lanthanum and silicon to the negative electrode, and adjusts the mass content of the two to meet 0.1≤N3≤0.5 and 36≤N4≤40 respectively. Through the coordination of the three, it is possible to improve the energy density while improving the cycle performance, rate performance, expansion inhibition performance and high temperature storage performance of the lithium-ion battery. In particular, when the mass contents of the three meet the ranges of Table 1 respectively, the cycle performance, rate performance, expansion inhibition performance and high temperature storage performance of the lithium-ion battery can be further improved.

[0100] In particular, when the mass contents of the three elements meet the relationship of 0.005≤(N2+N3) / N4≤0.017, the coordination effect of the three can be further enhanced, thereby significantly improving the cycle performance, rate performance, expansion inhibition performance and high-temperature storage performance of lithium-ion batteries.

[0101] The lithium-ion batteries of each embodiment in Table 2 are different from those of Embodiment 1 only in that neodymium is added to lithium nickel cobalt manganese oxide and the average particle size of each particle is different. The mass content of neodymium in the positive electrode mixture layer is N1% and the specific particle size of each particle is shown in Table 2.

[0102] Table 2

[0103]

[0104] As can be seen from Table 2, the present application adds neodymium to the positive electrode on the basis of the above-mentioned combination of titanium, lanthanum and silicon elements, and regulates its mass content to meet 0.01≤N1≤0.05, which is conducive to further improving the cycle performance, rate performance, expansion inhibition performance and high-temperature storage performance of lithium-ion batteries. Among them, the mass content of neodymium and titanium in the positive electrode mixture layer is controlled to meet 1.6≤N2 / N1≤10, which can significantly improve the cycle performance, rate performance, expansion inhibition performance and high-temperature storage performance of lithium-ion batteries. In particular, when the mass content of the two is regulated to meet 2.4≤N2 / N1≤8, it can better promote the coordination of the two elements, so that the lithium-ion battery exhibits more excellent cycle performance, rate performance, expansion inhibition performance and high-temperature storage performance.

[0105] The lithium ion batteries of the embodiments in Table 3 are different from those of Embodiment 1 only in that the average particle sizes of the particles are different. The specific average particle sizes are shown in Table 3.

[0106] Table 3

[0107]

[0108] As can be seen from Table 3, further regulating the average particle size of the first particle and the second particle in the lithium-ion battery to meet 22.0≤D1 / D2≤50 can optimize the coordination effect of each element in the positive electrode and improve the cycle performance, rate performance, expansion inhibition performance and high-temperature storage performance of the lithium-ion battery. In particular, when the average particle size of the first particle and the second particle are respectively regulated to meet the range of Table 3, the cycle performance, rate performance, expansion inhibition performance and high-temperature storage performance of the lithium-ion battery can be better optimized. On this basis, regulating the particle size of the third particle to meet 10≤D3≤15 can further improve the cycle performance, rate performance, expansion inhibition performance and high-temperature storage performance of the lithium-ion battery.

[0109] The lithium ion batteries of the embodiments in Table 4 are different from those in Embodiment 1 only in that a first compound is added to the solvent in the electrolyte. The specific addition type and the mass content N5% of the first compound in the electrolyte are shown in Table 4 below.

[0110] Table 4

[0111]

[0112]

[0113] As can be seen from Table 4, the present application further adds the compound shown in formula I to the electrolyte, which can improve the high temperature storage performance and safety performance of the lithium-ion battery after cooperating with the positive and negative electrode systems. In particular, when the mass content N5 of the compound shown in formula I in the electrolyte is regulated to meet 0.2≤N5≤0.6, the high temperature stability of the lithium-ion battery can be further improved, and the safety performance of the lithium-ion battery in high temperature extreme environments can be improved. Among them, when N5 and the content of lanthanum in the negative electrode N3 are regulated to meet 0.4≤N5 / N3≤3, the high temperature stability and safety performance of the lithium-ion battery can be further improved.

[0114] The above description is only a preferred embodiment of the present application and is not intended to limit the present application. Any modifications, equivalent substitutions and improvements made within the principles of the present application should be included in the protection scope of the present application.

Claims

1. An electrochemical device, comprising a positive electrode sheet and a negative electrode sheet, wherein the positive electrode sheet comprises a positive electrode mixture layer, and the negative electrode sheet comprises a negative electrode mixture layer, characterized in that: The positive electrode mixture layer includes first particles and second particles, the first particles contain nickel, cobalt and manganese, and the second particles contain titanium; Based on the mass of the positive electrode mixture layer, the mass content of titanium element is N2%, 0.08≤N2≤0.2; The negative electrode mixture layer includes third particles, and the third particles contain silicon and lanthanum; Based on the mass of the negative electrode mixture layer, the mass content of the lanthanum element is N3%, 0.1≤N3≤0.5, and the mass content of the silicon element is N4%, 36≤N4≤40.

2. The electrochemical device according to claim 1, characterized in that 0.005≤(N2+N3) / N4≤0.

017.

3. The electrochemical device according to claim 1, wherein the first particles further comprise neodymium, and the mass content of the neodymium is N1% based on the mass of the positive electrode mixture layer, 0.01≤N1≤0.05; and / or, 1.6≤N2 / N1≤10.

4. The electrochemical device according to claim 1, characterized in that In the first particles, the mass ratio of the nickel element, the cobalt element and the manganese element is (5-9):(0.5-3):(0.5-2); and / or, The first particle is lithium nickel cobalt manganese oxide, and the chemical formula of the lithium nickel cobalt manganese oxide is LiNi a Co b Mn 1-a-b O2, where 0.5≤a≤0.9, 0.05≤b≤0.

3.

5. The electrochemical device according to any one of claims 1 to 4, characterized in that The average particle size of the first particles is D1 μm; the average particle size of the second particles is D2 μm; 10≤D1 / D2≤47; and / or, The average particle size of the third particles is D3 μm, 10≤D3≤15.

6. The electrochemical device according to claim 5, characterized in that 5≤D1≤9.5; and / or, 0.2≤D2≤0.

6.

7. The electrochemical device according to any one of claims 1 to 4, characterized in that: The second particle is lithium aluminum titanium phosphate; the chemical formula of the lithium aluminum titanium phosphate is Li 1+x Al x Ti 2-x (PO4)3, wherein 0<x≤0.5; based on the mass of the positive electrode mixture layer, the mass content of the lithium aluminum titanium phosphate is M1%, 0.4≤M1≤1.0; and / or, The third particle includes lithium lanthanum titanate; the chemical formula of the lithium lanthanum titanate is La 2 / 3-y Li 3y TiO3, wherein 0.17≤y≤0.5; based on the mass of the negative electrode mixture layer, the mass content of the lithium lanthanum titanate is M2%, 0.5≤M2≤1.

5.

8. The electrochemical device according to any one of claims 1 to 4, characterized in that: The electrochemical device further comprises an electrolyte; the electrolyte comprises a compound represented by formula I; In Formula I, R1 is a substituted or unsubstituted C2-C8 cyclic ether group, R2 is a substituted or unsubstituted C1-C5 alkylene group, and R3 is hydrogen or a substituted or unsubstituted C1-C5 alkyl group; Based on the mass of the electrolyte, the mass content of the compound represented by formula I is N5%, 0.2≤N5≤0.

6.

9. The electrochemical device according to claim 8, characterized in that The compound represented by formula I is selected from at least one of 2-tetrahydrofuranyl acrylate, 2-tetrahydrofuranyl methacrylate and glycidyl acrylate; and / or, 0.4≤N5 / N3≤3.

10. An electronic device, characterized in that: An electrochemical device comprising any one of claims 1 to 9.

Citation Information

Patent Citations

  • Negative electrode for all-solid-state battery, and all-solid-state battery

    CN114342118A

  • Electrochemical device and electronic device

    CN116031411A

  • Lithium ion battery, battery and electric device

    CN117154188A

  • Positive electrode active material, and electrochemical apparatus and electronic apparatus using same

    US20240021815A1

  • Negative electrode sheet, electrochemical device, and electronic device

    WO2024050714A1

Cited By

  • Electrochemical device and electronic device

    CN119965271A

  • Electrochemical device and electronic device

    WO2026183729A1