Negative active material as well as preparation method and application thereof
By using silicon/phosphorus/carbon composite materials in lithium and sodium batteries, the problem of poor battery circulation and rate performance is solved, and higher energy density and electrochemical performance are achieved, especially under low temperature and fast charging conditions. More stable performance.
Patent Information
- Application Number
- CN202411093653.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-09
- Publication Date
- 2024-11-12
AI Technical Summary
The circulation and rate performance of existing lithium and sodium batteries are poor, which affects the application effect of the battery.
A negative electrode active material, including a carbon ball embedded with silicon-based materials and phosphorus-based materials, is used to form silicon/phosphorus/carbon composite materials by regulating the content and electronic conductivity of the silox-based materials and phosphorus-based materials to improve the conductivity of the material. and ion diffusion capability, satisfying specific mass fraction and conductivity relationships to improve the energy density and electrochemical properties of the battery.
It significantly improves the battery's low-temperature discharge performance, charging temperature rise and circulation performance, reduces polarization phenomenon and lithium evolution risks, and improves the battery's rate performance and energy density.
Smart Images

Figure CN118943335A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of battery materials, and in particular relates to a negative electrode active material and a preparation method and application thereof. Background Art
[0002] As a new type of secondary battery, lithium and sodium batteries have the advantages of high operating voltage, high energy density, long life, wide operating temperature range and environmental friendliness, and have become the main energy storage devices for mainstream electronic products. As the market demand for battery performance gradually increases, lithium batteries and sodium batteries with excellent performance not only need to have high energy density, but also excellent charging and discharging capabilities. In the traditional electrode sheet preparation method, the content of active material coated on the surface of the current collector is increased to achieve the purpose of improving the energy density of the battery. However, the current battery cycle performance and rate performance are poor, which to a certain extent affects the application of the battery. Summary of the invention
[0003] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a negative electrode active material, which has good cycle performance and rate performance and good application prospects when used in a secondary battery.
[0004] The invention also provides a method for preparing the negative electrode active material.
[0005] The invention also provides a negative electrode material.
[0006] The invention also provides a negative electrode.
[0007] The invention also provides an electrochemical energy storage device.
[0008] The invention also provides an electrical device.
[0009] In a first aspect of the present invention, a negative electrode active material is provided, including a carbon ball, wherein the carbon ball includes a silicon-based material and a phosphorus-based material, and the mass fraction of the silicon-based material in the carbon ball is M si %, the mass fraction of the phosphorus-based material in the carbon sphere is M P %, the electronic conductivity of the silicon-based material is σ si S / cm, the electronic conductivity of the phosphorus-based material is σ P S / cm,M si 、M P , σ si and σ P Between: 1≤(M Si *σ P ) / (1000*M P *σ Si )≤100,1≤M P / M Si≤3.
[0010] The negative electrode active material according to the embodiment of the present invention has at least the following beneficial effects:
[0011] The negative electrode active material in the present invention is a silicon / phosphorus / carbon composite material. The phosphorus material has a high theoretical specific capacity and excellent electrical conductivity (electronic conductivity). When used in an electrochemical energy storage device (such as a secondary battery), the lithium (sodium) phosphorus compound formed during the lithium (sodium) process of phosphorus has a positive effect on ion diffusion. In the present invention, the silicon of the silicon-based material and the phosphorus of the phosphorus-based material can both provide lithium (sodium) insertion sites. The conductivity of the material can be improved by combining the silicon-based material and the phosphorus-based material with the carbon material, and the volume expansion effect caused by ion insertion can be restrained. The content of the silicon-based material and the phosphorus-based material satisfies the relationship: 1≤M P / M Si ≤3, which is conducive to the formation of PC bonds between phosphorus-based materials and carbon materials. The formation of PC bonds can further improve the conductivity of negative electrode active materials. At the same time, because the content and conductivity of silicon-based materials and phosphorus-based materials affect the electron transfer rate, when the relationship is satisfied: 1≤(M Si *σ P ) / (1000*M P *σ Si )≤100, the silicon and phosphorus contents can not only meet the capacity requirements, but also improve the electronic conductivity of the negative electrode active materials.
[0012] In summary, using the negative electrode active material (silicon / phosphorus / carbon composite material) in the present invention for an electrochemical energy storage device can not only ensure the energy density of the electrochemical energy storage device, but also increase the electron transmission rate, improve the electrochemical performance, reduce the charging temperature rise of the electrochemical energy storage device, and relatively losslessly reduce the polarization of the electrochemical energy storage device, improve the low-temperature discharge and rate performance of the electrochemical energy storage device, and reduce the risk of lithium plating during fast charging.
[0013] In some embodiments of the present invention, 1≤(M Si *σ P ) / (1000*M P *σ Si )≤5,2≤M P / M Si ≤3.
[0014] Through the above implementation, the obtained negative electrode active material is used in a secondary battery, and the low-temperature discharge performance, charging temperature rise and cycle performance of the battery are greatly improved, and the battery performance is better.
[0015] In some embodiments of the present invention, 1≤(M Si *σ P ) / (1000*M P *σSi )≤4.
[0016] In some embodiments of the present invention, the carbon sphere has a D 50 It is 0.5 to 20 μm, preferably 2 to 6 μm.
[0017] Through the above implementation, compared with the D 50 Less than 2μm, the D 50 2-6 μm is more conducive to the composite effect of phosphorus-based materials, phosphorus-based materials and carbon materials in the material preparation process, and is less likely to cause agglomeration of phosphorus-based materials and phosphorus-based materials. 50 Larger than 6μm, the D 50 The thickness of the negative electrode is 2 to 6 μm. In the subsequent rolling process of preparing the negative electrode sheet, it is less likely to cause the material to break due to large external mechanical stress, and the electrochemical performance of the resulting battery is more stable.
[0018] In some embodiments of the present invention, the carbon sphere includes a carbon shell and a porous carbon core disposed in the carbon shell, and the silicon-based material is located in the pores of the porous carbon core or / and between the carbon shell and the porous carbon core.
[0019] In some embodiments of the present invention, the phosphorus-based material is located in the pores of the porous carbon core or / and between the carbon shell and the porous carbon core.
[0020] In some embodiments of the present invention, the thickness of the carbon shell is 10 to 900 nm, such as 100 to 300 nm.
[0021] In some embodiments of the present invention, the pores contained in the porous carbon core have a pore diameter of 5 to 200 nm, such as 50 to 150 nm.
[0022] In some embodiments of the present invention, the carbon shell and the porous carbon core may be connected, partially connected, or fully connected.
[0023] In some embodiments of the present invention, the silicon-based material comprises silicon. Optionally, the silicon comprises silicon particles.
[0024] In some embodiments of the present invention, the phosphorus-based material comprises phosphorus. Optionally, the phosphorus comprises phosphorus particles.
[0025] In some embodiments of the present invention, the phosphorus is black phosphorus.
[0026] Through the above implementation, the phosphorus material is black phosphorus, which has a high specific capacity, good conductivity and interlayer spacing, is conducive to the shuttle of ions and electrons, and is a very promising fast-charging negative electrode material. By combining black phosphorus with good conductivity with silicon with high specific capacity, the composite material has high capacity and good fast-charging capability. Regulate the content ratio of silicon and phosphorus materials and electronic conductivity to satisfy the relationship: 1≤(M Si *σ P ) / (1000*M P *σ Si )≤100,1≤M P / M Si ≤3, the negative electrode active material can have high energy density and good charging capacity. Good electronic conductivity can reduce polarization, reduce battery temperature rise, and help improve high temperature performance. In addition, phosphorus has better conductivity. During the lithium insertion process, lithium ions are preferentially embedded in phosphorus materials. The lithium insertion expansion of phosphorus materials will further limit the lithium insertion expansion of silicon materials. With the help of porous carbon coating restrictions, it helps to reduce the long-term cycle thickness expansion rate of the battery.
[0027] In some embodiments of the present invention, the M si % is 1% to 25%, and can be optionally 5% to 20%.
[0028] Through the above implementation, compared with M si % greater than 25%, M si % is 1% to 25%, and the conductivity of the obtained negative electrode active material is better; compared with M si % less than 1%, M si % of 1% to 25% is more conducive to the specific capacity of the obtained negative electrode active material.
[0029] In some embodiments of the present invention, the M P % is 5% to 60%, and can be optionally 10% to 50%.
[0030] Through the above implementation, the phosphorus-based material has a higher theoretical specific capacity, and its conductivity (electronic conductivity) is much better than that of silicon materials. P % greater than 60%, M P % of 5% to 60% is more conducive to the formation of PC bonds between the phosphorus-based material and the carbon material, thereby further improving the conductivity of the negative electrode active material.
[0031] And because phosphorus materials and silicon materials have certain lithiation expansion rates, the present invention uses M si % is 1% to 25% of silicon-based materials and M P The composite of 5% to 60% phosphorus-based materials and carbon materials can better improve the electrical conductivity of the material and better restrain the volume expansion effect caused by ion embedding.
[0032] In some embodiments of the present invention, the electronic conductivity of the silicon-based material is 10 -6 ~10 -2 S / cm, if optional, 10 -5 ~10 -3 S / cm.
[0033] In some embodiments of the present invention, the electronic conductivity of the phosphorus-based material is 0.1 to 10 S / cm, such as 1 to 3 S / cm.
[0034] The second aspect of the present invention proposes a method for preparing a negative electrode active material, comprising the following steps: first heat treating a mixture containing a porous carbon material, a phosphorus-based material and a silicon-based material at 300 to 800°C in a vacuum environment for 0.5 to 20 hours, and then calcining it at 100 to 800°C in a hydrogen-containing atmosphere for 0.5 to 20 hours to obtain the negative electrode active material.
[0035] In some embodiments of the present invention, the mass ratio of the porous carbon material, phosphorus-based material and silicon-based material is (25-94):(1-25):(5-60), such as (40-85):(5-20):(10-40), and further (46-82):(6-18):(12-36).
[0036] In some embodiments of the present invention, the vacuum degree of the vacuum environment is less than -0.075 MPa.
[0037] In some embodiments of the present invention, the mixture is first heat treated at 400-600° C. for 3-5 h in a vacuum environment, and then calcined at 300-500° C. for 3-5 h in an atmosphere containing hydrogen and an inert gas to obtain the negative electrode active material.
[0038] In some embodiments of the present invention, the volume ratio of hydrogen to inert gas is 1:(15-18).
[0039] In some embodiments of the present invention, the preparation method also includes preparing a porous carbon material, which specifically includes the following steps: mixing the MOF material with a monomer, an initiator and a solvent, heat treating in a water bath, filtering, grinding, calcining at 150 to 400° C. for 0.5 to 10 hours in a mixed atmosphere of oxygen and inert gas, and acid washing to obtain the porous carbon material; wherein the monomer includes at least one of pyrrole or aniline.
[0040] Compared with graphite, the conductivity of silicon and phosphorus is slightly poor. By embedding silicon and phosphorus particles inside porous carbon materials, the expansion of lithium insertion is limited on the one hand, and the conductivity is improved on the other hand. MOFs have rich pore structures, large specific surface areas and excellent chemical stability. The monomers and initiators generate polypyrrole or polyaniline, which can enhance the conductivity of the material. At the same time, during the carbonization process, the organic units of MOFs can synthesize porous carbon materials with high surface areas under the influence of the original pore skeleton, thus providing storage space for silicon and phosphorus, further improving the conductivity of the material.
[0041] Among them, polypyrrole or polyaniline is coated on the surface of MOFs material and then carbonized, similar to the double carbon layer structure, which can better limit the expansion of silicon and phosphorus particles and increase conductivity. In addition, the spherical structure of polypyrrole is destroyed by the carbonization process, resulting in a rough surface of the material, an increase in the surface area of the rough surface, and an increase in porosity, which is conducive to the penetration and infiltration of the electrolyte.
[0042] In some embodiments of the present invention, the initiator includes at least one of ammonium persulfate, ferric oxide or cerium ammonium nitrate.
[0043] In some embodiments of the present invention, the water bath heat treatment is performed at a temperature of 50 to 90° C. for a time of 3 to 15 hours.
[0044] In some embodiments of the invention, the solvent comprises ethanol.
[0045] In some embodiments of the present invention, the volume ratio of oxygen to inert gas is (1-10):1.
[0046] In some embodiments of the present invention, the mass ratio of the MOF material to the monomer and the initiator is 1:(20-100):(0.1-1).
[0047] In some embodiments of the present invention, the pickling is performed by using 0.2-0.6 mol / L hydrochloric acid at 40-70°C for 1-3 hours. For example, the pickling may be performed by using 0.4 mol / L hydrochloric acid at 60°C for 2 hours.
[0048] According to a third aspect of the present invention, a negative electrode material is provided, comprising the negative electrode active material described above.
[0049] In some embodiments of the present invention, the negative electrode material further comprises graphite. Optionally, the graphite is selected from natural graphite or artificial graphite.
[0050] In some embodiments of the present invention, the mass ratio of the graphite to the negative electrode active material is (60-99):(2-20).
[0051] In some embodiments of the present invention, the negative electrode material further includes a negative electrode conductor and a negative electrode binder.
[0052] In some embodiments of the present invention, the negative electrode conductive agent includes at least one of conductive carbon black (SP) or carbon nanotubes (CNT).
[0053] In some embodiments of the present invention, in the negative electrode conductive agent, the mass ratio of conductive carbon black to carbon nanotubes is (5-20):1.
[0054] In some embodiments of the present invention, the negative electrode binder includes at least one of SBR or PAALi.
[0055] In some embodiments of the present invention, in the negative electrode binder, the mass ratio of SBR to PAALi is 1:(1-10).
[0056] In some embodiments of the present invention, the mass ratio of the negative electrode active material, the negative electrode conductive agent and the negative electrode binder is (80-99.8):(0.1-5):(0.1-5).
[0057] According to a fourth aspect of the present invention, a negative electrode is provided, comprising the negative electrode material mentioned above.
[0058] In some embodiments of the present invention, the negative electrode includes a negative electrode current collector and a negative electrode active layer, and the negative electrode active layer includes the negative electrode material.
[0059] In some embodiments of the present invention, the negative electrode active layer is disposed on at least one side of the negative electrode current collector.
[0060] In some embodiments of the present invention, the thickness of the negative electrode active layer is 10 to 200 μm.
[0061] In some embodiments of the present invention, the thickness of the negative electrode current collector is 1 to 20 μm.
[0062] In some embodiments of the present invention, the negative electrode current collector includes but is not limited to copper foil, foam copper, nickel foil, foam nickel, stainless steel foil, tin foil or a composite current collector.
[0063] In some embodiments of the present invention, the negative electrode further includes but is not limited to negative electrode film-forming additives or cycle-improving and low-temperature additives.
[0064] In a fifth aspect of the present invention, an electrochemical energy storage device is provided, comprising the above-mentioned negative electrode.
[0065] In some embodiments of the present invention, the electrochemical energy storage device is a secondary battery.
[0066] In some embodiments of the present invention, the secondary battery further includes a positive electrode and a separator.
[0067] In some embodiments of the present invention, the positive electrode includes a positive electrode current collector and a positive electrode active layer.
[0068] In some embodiments of the present invention, the positive electrode active layer comprises a positive electrode active material, a positive electrode conductive agent and a positive electrode binder, wherein the specific types and compositions of the positive electrode active material, the positive electrode conductive agent and the positive electrode binder are not subject to specific restrictions.
[0069] In some embodiments of the present invention, the positive electrode active material includes but is not limited to lithium cobalt oxide, ternary materials or lithium-rich materials.
[0070] In some embodiments of the present invention, the positive electrode conductive agent includes at least one of acetylene black or carbon nanotubes.
[0071] In some embodiments of the present invention, the positive electrode binder includes polyvinylidene fluoride (PVDF).
[0072] In some embodiments of the present invention, the mass ratio of the positive electrode active material, the positive electrode conductor and the positive electrode binder is (80-99.8):(0.1-5):(0.1-5).
[0073] In some embodiments of the present invention, the positive electrode further includes but is not limited to positive electrode film-forming additives or cycle-improving and low-temperature additives.
[0074] In some embodiments of the present invention, the separator includes but is not limited to polyethylene, polypropylene or polyvinylidene fluoride, etc., and can be a single-layer film or a multi-layer film.
[0075] In some embodiments of the present invention, the secondary battery further comprises an electrolyte. Optionally, the electrolyte comprises an electrolyte salt and an organic solvent, wherein the specific types and compositions of the electrolyte salt and the organic solvent are not subject to specific restrictions.
[0076] According to a sixth aspect of the present invention, an electrical device is provided, wherein the electrochemical energy storage device is used as a power source for the electrical device. BRIEF DESCRIPTION OF THE DRAWINGS
[0077] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:
[0078] Figure 1 Schematic diagram of the structure of the negative electrode active material of Example 1 of the present invention.
[0079] Figure symbols: 1. Silicon particles; 2. Phosphorus particles; 3. Porous carbon. DETAILED DESCRIPTION
[0080] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0081] The experimental methods in the following examples without specifying specific conditions are generally carried out according to conventional conditions in the art or conditions recommended by the manufacturers; the raw materials and reagents used, unless otherwise specified, are all raw materials and reagents that can be obtained from commercial channels such as conventional markets.
[0082] Pyrrole, ammonium persulfate, and hydrochloric acid were purchased from Aladdin Biochemical Technology Co., Ltd. or other manufacturers.
[0083] Artificial graphite: purchased from Jiangxi Zichen Technology Co., Ltd. 50 :10.5±2.0μm, BET: 1.30±0.30m 2 g -1 , TD: ≥0.85g / cm 3 ;
[0084] The Co-MOF is ZIF-67, the metal source is Co, and the ligand is dimethylimidazole, which are purchased from Aladdin Biochemical Technology Co., Ltd.; MOF materials produced by other manufacturers can also be purchased.
[0085] Example 1
[0086] This embodiment discloses a negative electrode active material, which is a silicon / phosphorus / carbon composite material, including a carbon shell, a porous carbon sphere located in the carbon shell, phosphorus and silicon (the phosphorus is located in the pores of the porous carbon core or / and between the carbon shell and the porous carbon core; the silicon is located in the pores of the porous carbon core or / and between the carbon shell and the porous carbon core). The schematic diagram can be shown as follows Figure 1 The preparation process of the negative electrode active material includes:
[0087] (Ⅰ) Preparation of porous carbon, including: taking 0.05g Co-MOF (ZIF-67, Mn-MOF or Ni-MOF can also be used), 2.5g pyrrole, 0.025g ammonium persulfate dispersed in 15mL ethanol, 70℃ water bath for 8h. Then the above mixture is filtered, dried and ground. The ground material is placed in a tube furnace and calcined at 280℃ for 3h in a mixed atmosphere of oxygen and argon (volume ratio 3:1). The sintered powder is acid-washed with 0.4mol / L hydrochloric acid at 60℃ for 2h, the solid matter is filtered out and dried to obtain porous carbon spheres. The shell thickness of the carbon sphere formed by sintering the MOF material is about 150nm, and the pore size of the carbon core is about 80nm. There is no gap between the shell and the core of the prepared carbon sphere, and the shell and the core of the carbon sphere are integrated. The D of the carbon sphere 50 In some other embodiments of the present invention, the shell thickness of the carbon sphere can be 100 to 300 nm, the pore diameter of the carbon core can be 50 to 150 nm, and the D 50 Any size between 2 and 6 μm is acceptable.
[0088] (II) Preparation of silicon / phosphorus / carbon composite material: Porous carbon is mixed with silicon material (silicon) and phosphorus material (black phosphorus) in a mass ratio of 12.7:1:3, placed in a tube furnace, kept at 500°C and vacuum degree <-0.075Mpa for 3h (3-5h is acceptable), and then calcined at 300°C (300-500°C is acceptable) for 3h (3-5h is acceptable) in a mixed atmosphere of hydrogen and argon (volume ratio 1:15) to obtain a silicon / phosphorus / carbon composite material. The volume ratio of hydrogen to argon is 1:15-18.
[0089] The electronic conductivity of the silicon material and phosphorus material used is 4.23x10 -4 S / cm, 1.76S / cm.
[0090] This embodiment also discloses a negative electrode material, comprising the negative electrode active material prepared in this embodiment and artificial graphite, a negative electrode conductive agent and a negative electrode binder. The negative electrode conductive agent comprises a mixture of SP and CNT, and the mass ratio of SP to CNT is 0.45:0.05. The binder is a mixture of SBR and PAALi, and the mass ratio of SBR to PAALi is 0.5:1.8.
[0091] This embodiment also discloses a negative electrode sheet, the preparation steps of which include:
[0092] SP and CNT were mixed in a mass ratio of 0.45:0.05 to obtain a negative electrode conductive agent; SBR and PAALi were mixed in a mass ratio of 0.5:1.8 to obtain a negative electrode binder;
[0093] The negative electrode active material (including negative electrode active material and artificial graphite, the mass ratio of the two is 10:90), the negative electrode conductive agent, and the negative electrode binder are mixed in a weight ratio of 97.7:1.1:1.2 to prepare the negative electrode active material slurry, and the slurry is evenly coated on the negative electrode collector (copper foil), and then cold pressed and stripped to obtain the negative electrode sheet. The thickness of the negative electrode sheet is 90μm, and the thickness of the negative electrode collector is 5μm.
[0094] This embodiment also discloses a lithium-ion battery, including the negative electrode sheet prepared in this embodiment. The lithium-ion battery also includes a positive electrode sheet, a separator and an electrolyte. Among them:
[0095] Preparation of positive electrode sheet: The positive electrode active material LiCoO2, the conductive agent acetylene black, the conductive carbon nanotubes, and the binder polyvinylidene fluoride (PVDF) are fully dispersed and uniformly coated on the positive electrode collector (aluminum foil) in the N-methylpyrrolidone solvent system at a weight ratio of 97.6:0.5:0.6:1.3, and then cold pressed and cut into strips to obtain the positive electrode sheet. The thickness of the positive electrode sheet is 70μm, and the thickness of the positive electrode collector is 8μm.
[0096] Isolation membrane: The surfaces of both sides of the PE layer are coated with a ceramic mixture as an isolation membrane, wherein the ceramic mixture includes PVDF and alumina. The thickness of the isolation membrane is 6μm, and the thickness of the PE layer is 4μm. Purchased from Huizhou Liwei Electronic Technology Co., Ltd. (YC-SCD-6814F4-004);
[0097] Electrolyte: Ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), and propyl propionate (PP) are mixed in a volume ratio of 1.2:1:4:4, and then fully dried lithium salt LiPF6 is dissolved in a mixed organic solvent at a ratio of 1 mol / L to prepare an electrolyte.
[0098] Preparation of a full battery: The negative electrode sheet, separator, and positive electrode sheet are wound or stacked to produce a bare cell, which is then packaged and injected with electrolyte to produce a finished lithium-ion battery.
[0099] This embodiment also discloses a sodium ion battery, including the negative electrode sheet prepared in this embodiment.
[0100] Examples 2 to 8 and Comparative Examples 1 to 7
[0101] Examples 2 to 8 and Comparative Examples 1 to 7 disclose a series of negative electrode active materials, which differ from Example 1 in that: the electronic conductivity of the silicon material and the phosphorus material used is different (the lattice defects and impurity concentration of the silicon material will affect the conductivity of the material; the purity and nano-size of the phosphorus material will affect the conductivity of the material), the mass fractions of the silicon material and the phosphorus material in the negative electrode active material are different, and whether pyrrole and ammonium persulfate are added during the preparation; the specific information is shown in Table 1 below, where the electronic conductivity is measured by a four-probe measurement method.
[0102] Among them, silicon materials were purchased from Lanxi Zhide Energy Materials Co., Ltd.:
[0103] Examples 1 to 5 / 8, Comparative Examples 1 / 3 / 5 to 7: YP-APS-0090-0000;
[0104] Examples 6-7: YP-APS-0083-0000; Comparative Example 4: YP-APS-0121-0000;
[0105] Phosphorus materials were purchased from Solid Lithium New Energy Technology Co., Ltd.:
[0106] Examples 1 to 6 / 8, Comparative Examples 2 to 5 / 7: YP-APG-0058-0000;
[0107] Example 7: YP-APG-0014-0000; Comparative Example 6: YP-APG-0021-0000;
[0108] Examples 2 to 8 and Comparative Examples 1 to 7 further disclose a series of negative electrode materials, which differ from Example 1 only in that the corresponding negative electrode active materials in Examples 2 to 8 and Comparative Examples 1 to 7 are respectively used.
[0109] Examples 2 to 8 and Comparative Examples 1 to 7 further disclose a series of negative electrode sheets, which differ from Example 1 only in that the corresponding negative electrode materials in Examples 2 to 8 and Comparative Examples 1 to 7 are respectively used.
[0110] Examples 2 to 8 and Comparative Examples 1 to 7 further disclose a series of lithium-ion batteries, which differ from Example 1 only in that the corresponding negative electrode plates in Examples 2 to 8 and Comparative Examples 1 to 7 are respectively used.
[0111] Examples 2 to 8 and Comparative Examples 1 to 7 further disclose a series of sodium ion batteries, which differ from Example 1 only in that the corresponding negative electrode plates in Examples 2 to 8 and Comparative Examples 1 to 7 are respectively used.
[0112] Table 1
[0113]
[0114]
[0115] Test example
[0116] This test example conducted a performance test on the lithium ion batteries prepared in the examples and comparative examples, specifically including:
[0117] Low temperature performance test: In a 25℃ environment, the charging test is carried out according to the following method, and the charging system is: 0.5C CC to 4.5V, CV to 0.02C; in a -10℃ environment, the discharge test is carried out according to the following method, and the discharge system is: 0.2C DC to 3.2V.
[0118] Rate performance test: In a 25℃ environment, perform charging test according to the following method, charging mode: 0.5C CC to 4.5V, CV to 0.02C; discharge mode: 1.5C DC to 3.0V;
[0119] Temperature rise test: In a 25℃ environment, perform charging test according to the following method, charging mode: 2.8C CC to 4.27V, 2.5CCC to 4.35V, CV to 1.8C, 1.8C CC to 4.4V, CV to 1.5C, 1.5C CC to 4.5V, CV to1.2C, 1.2CCC to 4.55V, CV to 0.26C; discharge mode: 0.2C DC to 3.0V. Use a temperature rise tester to monitor the temperature at the center of the battery surface.
[0120] Cycle test: In 45℃ environment, charge test was performed according to the following method. Charging mode: 2.8C CC to 4.27V, 2.5CCC to 4.35V, CV to 1.8C, 1.8C CC to 4.4V, CV to 1.5C, 1.5C CC to 4.5V, CV to1.2C, 1.2CCC to 4.55V, CV to 0.26C; Discharge mode: 0.7C DC to 3.2V.
[0121] 300-cycle capacity retention rate = 300-cycle full-charge capacity / initial full-charge capacity;
[0122] 300-week thickness expansion rate = (300-week full-charge thickness - initial half-charge thickness) / initial half-charge thickness; battery thickness is measured using 600PPG.
[0123] The test results are shown in Table 2 below:
[0124] Table 2
[0125]
[0126] It can be seen from Examples 1 to 8 and Comparative Examples 1 to 7 that the negative electrode material of the present invention has significantly better electrochemical performance; based on low-temperature discharge and rate performance, the conductivity of the electrochemical energy storage device of the present invention is significantly improved, and it still performs well under low temperature or high current density conditions. From the temperature rise results, the electrode polarization of the electrochemical energy storage device is reduced, and the temperature rise is reduced, which is conducive to improving the performance of the electrochemical energy storage device in a high temperature environment.
[0127] If there is no special explanation, the actual meaning of "about" in the present invention is that the error is allowed within the range of ±2%, for example, about 100 is actually 100±2%×100. The "normal temperature" or "room temperature" in the present invention, unless otherwise specified, is about 20-30°C.
[0128] Unless otherwise specified, “between” in the present invention includes the number itself, for example, “between 2-3” includes the endpoint values 2 and 3.
[0129] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A negative electrode active material, characterized in that: The carbon sphere includes a silicon-based material and a phosphorus-based material, and the mass fraction of the silicon-based material in the carbon sphere is M si %, the mass fraction of the phosphorus-based material in the carbon sphere is M P %, the electronic conductivity of the silicon-based material is σ si S / cm, the electronic conductivity of the phosphorus-based material is σ P S / cm,M si 、M P , σ si and σ P Between: 1≤(M Si *σ P ) / (1000*M P *σ Si )≤100,1≤M P / M Si ≤3.
2. The negative electrode active material according to claim 1, characterized in that 1≤(M Si *s P ) / (1000*M P *s Si )≤5,2≤M P / M Si ≤3。 3. The negative electrode active material according to claim 1, characterized in that The D 50 The carbon sphere comprises a carbon shell and a porous carbon core disposed in the carbon shell, and the silicon-based material is located in the pores of the porous carbon core or / and between the carbon shell and the porous carbon core.
4. The negative electrode active material according to claim 1, characterized in that The silicon-based material includes silicon; and / or, the phosphorus-based material includes phosphorus; and / or, the M si % is 1% to 25%; and / or, the M P % is 5% to 60%; and / or the electronic conductivity of the silicon-based material is 10 -6 ~10 -2 S / cm; and / or, the electronic conductivity of the phosphorus-based material is 0.1-10 S / cm.
5. A method for preparing a negative electrode active material, characterized in that: The method comprises the following steps: firstly heat treating a mixture containing porous carbon material, phosphorus-based material and silicon-based material at 300-800° C. for 0.5-20 h in a vacuum environment, and then calcining at 100-800° C. for 0.5-20 h in a hydrogen-containing atmosphere to obtain the negative electrode active material.
6. A negative electrode material, characterized in that: The negative electrode active material comprises the negative electrode active material according to any one of claims 1 to 4 or the negative electrode active material prepared by the method according to claim 5.
7. The negative electrode material according to claim 6, characterized in that The negative electrode material also includes graphite; Preferably, the mass ratio of the graphite to the negative electrode active material is (60-99):(2-20).
8. A negative electrode, characterized in that The negative electrode material comprises the negative electrode material according to any one of claims 6 to 7.
9. An electrochemical energy storage device, characterized in that: Comprising the negative electrode as claimed in claim 8.
10. An electrical device, characterized in that: The electrochemical energy storage device according to claim 9 is used as a power source for the electrical equipment.