Preparation method of iodine-loaded porous positive electrode material for zinc battery

Through the preparation method of iodine-loaded porous cathode material, the problem of low energy density of aqueous zinc ion batteries is solved, and a stable dispersion system is formed through ball milling and adsorption processes, which improves the specific capacity and circulation performance of the battery and achieves improvement in performance.

CN118943369APending Publication Date: 2024-11-12SUZHOU PUCHANG NEW ENERGY CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202410987613.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12

Smart Images

  • Figure BDA0004957906920000101
    Figure BDA0004957906920000101
Patent Text Reader

Abstract

The invention discloses a preparation method of an iodine-loaded porous positive electrode material for a zinc battery, and relates to the technical field of aqueous zinc ion battery positive electrode materials. The method comprises the following steps: weighing precursor manganese carbonate, a carbon source and a dispersing agent, carrying out ball milling, transferring mixed powder into a tubular furnace for sintering after ball milling, cooling to room temperature, repeatedly cleaning with diluted hydrochloric acid and deionized water respectively, drying, carrying out ball milling and mixing with elemental iodine by using a ball mill, transferring into a reaction kettle, heating the reaction kettle for adsorption, and cooling to room temperature; and after adsorption is completed, preserving heat and slowly cooling to obtain the iodine-loaded porous positive electrode material for the zinc battery. The positive electrode material prepared by the method effectively improves the specific capacity, the cycle performance and the rate performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of positive electrode materials for aqueous zinc ion batteries, in particular to a method for preparing an iodine-loaded porous positive electrode material for zinc batteries. Background Art

[0002] With the increasing depletion of fossil energy and the serious environmental problems it brings, the development of environmentally friendly clean renewable energy has attracted more and more attention. Secondary batteries have attracted widespread attention due to their relatively simple system and relatively high energy storage efficiency. Among them, aqueous zinc-ion batteries (AZIBs) with high specific capacity (820mAh g -1 ), low redox potential (-0.76Vvs.SHE), cheap and stable metal zinc as the negative electrode, so it has its irreplaceable advantages. It stands out among many new aqueous rechargeable metal ion batteries and becomes the most popular research object in aqueous metal batteries.

[0003] A positive electrode material for an aqueous zinc ion battery and a preparation method thereof (Chinese patent application number: CN202111164599.9) comprises the following steps: (1) dissolving a manganese source in water, adding an oxidant and sulfur, stirring evenly, and transferring the mixture to a hydrothermal reactor for hydrothermal reaction to obtain a precipitate; (2) stirring the precipitate and an organic additive solution evenly, and then spray drying the mixture to obtain a precursor, and calcining the precursor in a muffle furnace at 300 to 1000° C. to obtain Mn 3 O 4 / S precursor material; (3) Mn 3 O 4 The / S material and the carbon source are dispersed in water to obtain a dispersion, and the dispersion is dried and calcined in a tube furnace at 300-800°C under an inert gas atmosphere to finally obtain Mn 3 O 4 / S / C composite material.

[0004] A method for preparing a manganese trioxide / iron oxide composite positive electrode material for an aqueous zinc ion battery using manganese ore tailings leachate (Chinese patent application number: CN202311046972.X) is firstly to use manganese ore tailings as a raw material, glucose as a reducing agent, and hydrochloric acid as a leaching agent to carry out a reduction leaching reaction to obtain a manganese ore tailings leachate, appropriately adjust the molar ratio of manganese ions to glucose in the leachate, and then place the leachate in a muffle furnace for heat treatment to obtain Mn 2 O 3 / Fe 2 O 3 Composite electrode materials.

[0005] A positive electrode material for an aqueous zinc-ion secondary battery, a preparation method and an application thereof (Chinese patent application number: CN202211050005.6) uses organic matter and graphite materials as carbon sources, and adopts in-situ solid-phase synthesis technology to prepare a MnO / MnOS / C composite material. The cycle stability and rate performance of the composite material are effectively improved by further doping with functional metal elements.

[0006] At present, the positive electrode materials available for aqueous zinc ion batteries are limited and the energy density of aqueous batteries is low, which is a problem and bottleneck link that restricts their widespread application. Based on this, in order to obtain an aqueous zinc ion battery positive electrode material with excellent performance, the present invention provides a method for preparing an iodine-loaded porous positive electrode material for zinc batteries. Summary of the invention

[0007] In view of the problems pointed out in the background technology and the shortcomings of the prior art, the purpose of the present invention is to provide a method for preparing an iodine-loaded porous positive electrode material for zinc batteries to improve the performance of aqueous zinc ion batteries.

[0008] The above invention object is achieved through the following scheme:

[0009] A method for preparing an iodine-loaded porous positive electrode material for a zinc battery, the operating steps of which are as follows:

[0010] Step 1: Weigh 45-60 parts of precursor manganese carbonate, 30-50 parts of carbon source and 0.007-0.07 parts of dispersant by mass, use a planetary ball mill for ball milling, transfer the mixed powder after ball milling to a tube furnace for sintering for 1-3 hours, cool to room temperature, and wash repeatedly with dilute hydrochloric acid and deionized water, and then dry;

[0011] Step 2: Weigh 50-75 parts of the mixture prepared in step 1 and 90-180 parts of iodine, use a planetary ball mill to mix them, transfer the mixed powder after ball milling to a reactor, heat the reactor for adsorption for 8-12 hours, evacuate the reactor, continue to keep warm for 2-5 hours, and slowly cool down to obtain an iodine-loaded porous positive electrode material for zinc batteries.

[0012] Preferably, in step 1, the carbon source is selected from at least one of sucrose, maltose, glucose and citric acid.

[0013] Preferably, in the steps 1 and 2, the ball milling jar is made of agate, the ball milling beads are made of zirconium beads, the ball milling speed is 200-400 rpm, and the ball milling time is 0.5-2 hours.

[0014] Preferably, inert gas is used for protection during the sintering in step 1 and the adsorption in step 2, and the inert gas is selected from one of argon, helium or nitrogen.

[0015] Preferably, in step 1, the sintering temperature is 650-850° C., and the heating rate of the tubular furnace is 2-5° C. / min.

[0016] Preferably, the preparation method of the dispersant in step 1 is:

[0017] H1: 0.18-0.36 parts of manganese nitrate and 0.3-0.6 parts of 10,13-epoxy-10,12-octadecadienoic acid were weighed and placed in 100-150 parts of water, reacted at 20-30°C for 100-150 minutes, and the water was distilled off;

[0018] H2: Continue to add 11-22 parts of 3-mercaptothiophene, 100-150 parts of N-methylpyrrolidone, and 3-6 parts of sodium ethoxide, react at 60-70°C for 100-150 minutes, then add 10-20 parts of isosorbide divinyl ether, react at 60-70°C for 30-50 minutes to obtain a dispersant.

[0019] Preferably, the reaction temperature in step H1 is 20-30°C, and the reaction temperature in step H2 is 60-70°C.

[0020] Preferably, the adsorption temperature of the reactor in step 2 is 65-85°C.

[0021] The reaction mechanism is:

[0022] Manganese nitrate reacts with 10,13-epoxy-10,12-octadecadienoic acid to generate 10,13-epoxy-10,12-octadecadienoic acid / manganese complex, which then reacts with 3-mercaptothiophene to undergo mercapto-epoxy reaction to obtain component 1;

[0023] Isosorbide divinyl ether and 3-mercaptothiophene undergo a mercapto-ene addition reaction to obtain component 2;

[0024] N-methylpyrrolidone, component 3;

[0025] The above three components obtain a dispersant containing manganese complex, thiophene and isosorbide; the uniform mixing of zinc battery positive electrode material precursor manganese carbonate and carbon source can be improved, as well as a more uniform particle size distribution, a smaller particle size, and no influence on the conductive performance.

[0026] Technical effects:

[0027] The manganese complex, thiophene and isosorbide dispersant form a stable dispersion system in manganese carbonate and carbon source. This dispersion system can effectively disperse manganese carbonate and carbon source evenly and avoid agglomeration and accumulation. The thiophene and isosorbide functional groups in the dispersant interact with the surface of manganese carbonate and carbon source, increase their surface activity, make them easier to mix with other materials, and help disperse and evenly distribute particles. Isosorbide is conducive to the dissolution and mixing of reactants, provides stability to the system, and prevents the occurrence of agglomeration and precipitation.

[0028] The dispersant containing manganese complex, thiophene and isosorbide can improve the uniform mixing of zinc battery positive electrode material precursor manganese carbonate and carbon source through the above mechanism, achieve more uniform particle size distribution and smaller particle size, and do not affect the conductivity. It helps to improve the specific capacity, cycle and rate performance of the battery. DETAILED DESCRIPTION

[0029] In view of the deficiencies in the prior art, the inventor of this case, after long-term research and extensive practice, was able to propose the technical solution of the present invention. The technical solution, its implementation process and principle, etc. will be further explained as follows.

[0030] Example 1

[0031] A method for preparing an iodine-loaded porous positive electrode material for a zinc battery, the operating steps of which are as follows:

[0032] Step 1: Weigh 45g of precursor manganese carbonate and 30g of carbon source, 0.01g of dispersant, use a planetary ball mill for ball milling, transfer the mixed powder after ball milling to a tube furnace for sintering for 1h, cool to room temperature, and wash repeatedly with dilute hydrochloric acid and deionized water, and then dry;

[0033] Step 2: Weigh 50g of the mixture prepared in step 1 and 90g of iodine, use a planetary ball mill to mix them, transfer the mixed powder after ball milling to a reactor, heat the reactor for adsorption for 8h, evacuate the reactor, continue to keep warm for 2h, and slowly cool down to obtain an iodine-loaded porous positive electrode material for zinc batteries.

[0034] In the step 1, the carbon source is selected from sucrose.

[0035] In the steps 1 and 2, the ball mill jar is made of agate, the ball mill beads are made of zirconium beads, the ball mill speed is 200 rpm, and the ball mill time is 0.5 hours.

[0036] In the sintering process in step 1 and the adsorption process in step 2, an inert gas is used for protection, and the inert gas is selected from argon.

[0037] In the step 1, the sintering temperature is 650° C., and the heating rate of the tubular furnace is 2° C. / min.

[0038] The preparation method of the dispersant in step 1 is:

[0039] H1: Weigh 0.18 g of manganese nitrate and 0.3 g of 10,13-epoxy-10,12-octadecadienoic acid into 100 g of water, react at 20°C for 100 minutes, and distill off the water;

[0040] H2: Continue to add 11 g of 3-mercaptothiophene, 100 g of N-methylpyrrolidone, and 3 g of sodium ethoxide, react at 60° C. for 100 minutes, then add 10 g of isosorbide divinyl ether, react at 60° C. for 30 minutes to obtain a dispersant.

[0041] The reaction temperature in step H1 is 20°C, and the reaction temperature in step H2 is 60°C.

[0042] The adsorption temperature of the reactor in step 2 is 65°C.

[0043] Example 2

[0044] A method for preparing an iodine-loaded porous positive electrode material for a zinc battery, the operating steps of which are as follows:

[0045] Step 1: Weigh 50g of precursor manganese carbonate and 35g of carbon source, 0.03g of dispersant, use a planetary ball mill for ball milling, transfer the mixed powder after ball milling to a tube furnace for sintering for 2h, cool to room temperature, and wash repeatedly with dilute hydrochloric acid and deionized water, and then dry;

[0046] Step 2: Weigh 55g of the mixture prepared in step 1 and 120g of iodine, use a planetary ball mill to mix them, transfer the mixed powder after ball milling to a reactor, heat the reactor for adsorption for 10 hours, evacuate the reactor, continue to keep warm for 3 hours, and slowly cool down to obtain an iodine-loaded porous positive electrode material for zinc batteries.

[0047] In the step 1, the carbon source is selected from maltose.

[0048] In the steps 1 and 2, the ball milling jar is made of agate, the ball milling beads are made of zirconium beads, the ball milling speed is 300 rpm, and the ball milling time is 1 hour.

[0049] Inert gas is used for protection during the sintering in step 1 and the adsorption in step 2, and the inert gas is selected from helium.

[0050] In the step 1, the sintering temperature is 700° C., and the heating rate of the tubular furnace is 3° C. / min.

[0051] The preparation method of the dispersant in step 1 is:

[0052] H1: 0.24 g of manganese nitrate and 0.45 g of 10,13-epoxy-10,12-octadecadienoic acid were placed in 110 g of water, reacted at 25°C for 115 minutes, and the water was distilled off;

[0053] H2: Continue to add 15 g of 3-mercaptothiophene, 115 g of N-methylpyrrolidone, and 4 g of sodium ethoxide, react at 65° C. for 115 minutes, then add 13 g of isosorbide divinyl ether, and react at 65° C. for 40 minutes to obtain a dispersant.

[0054] The reaction temperature in step H1 is 25°C, and the reaction temperature in step H2 is 65°C.

[0055] The adsorption temperature of the reactor in step 2 is 70°C.

[0056] Example 3

[0057] A method for preparing an iodine-loaded porous positive electrode material for a zinc battery, the operating steps of which are as follows:

[0058] Step 1: Weigh 55g of precursor manganese carbonate and 42g of carbon source, 0.05g of dispersant, use a planetary ball mill for ball milling, transfer the mixed powder after ball milling to a tube furnace for sintering for 2h, cool to room temperature, and wash repeatedly with dilute hydrochloric acid and deionized water, and then dry;

[0059] Step 2: Weigh 65g of the mixture prepared in step 1 and 150g of iodine, use a planetary ball mill to mix them, transfer the mixed powder after ball milling to a reactor, heat the reactor for adsorption for 10 hours, evacuate the reactor, continue to keep warm for 4 hours, and slowly cool down to obtain an iodine-loaded porous positive electrode material for zinc batteries.

[0060] In the step 1, the carbon source is selected from glucose.

[0061] In the steps 1 and 2, the ball mill jar is made of agate, the ball mill beads are made of zirconium beads, the ball mill speed is 300 rpm, and the ball mill time is 1.5 hours.

[0062] Inert gas is used for protection during the sintering in step 1 and the adsorption in step 2, and the inert gas is selected from helium.

[0063] In the step 1, the sintering temperature is 800° C., and the heating rate of the tubular furnace is 4° C. / min.

[0064] The preparation method of the dispersant in step 1 is:

[0065] H1: 0.32 g of manganese nitrate and 0.5 g of 10,13-epoxy-10,12-octadecadienoic acid were placed in 140 g of water, reacted at 25° C. for 140 minutes, and the water was distilled off;

[0066] H2: 19 g of 3-mercaptothiophene, 135 g of N-methylpyrrolidone, and 5 g of sodium ethoxide were added, and the mixture was reacted at 65° C. for 135 minutes. Then, 17 g of isosorbide divinyl ether was added, and the mixture was reacted at 65° C. for 40 minutes to obtain a dispersant.

[0067] The reaction temperature in step H1 is 25°C, and the reaction temperature in step H2 is 65°C.

[0068] The adsorption temperature of the reactor in step 2 is 75°C.

[0069] Example 4

[0070] A method for preparing an iodine-loaded porous positive electrode material for a zinc battery, the operating steps of which are as follows:

[0071] Step 1: Weigh 60g of precursor manganese carbonate and 50g of carbon source, 0.07g of dispersant, use a planetary ball mill for ball milling, transfer the mixed powder after ball milling to a tube furnace for sintering for 3h, cool to room temperature, and wash repeatedly with dilute hydrochloric acid and deionized water, and then dry;

[0072] Step 2: Weigh 75g of the mixture prepared in step 1 and 180g of iodine, use a planetary ball mill to mix them, transfer the mixed powder after ball milling to a reactor, heat the reactor for adsorption for 12h, evacuate the reactor, continue to keep warm for 5h, and slowly cool down to obtain an iodine-loaded porous positive electrode material for zinc batteries.

[0073] In the step 1, the carbon source is selected from citric acid.

[0074] In the steps 1 and 2, the ball mill jar is made of agate, the ball mill beads are made of zirconium beads, the ball mill speed is 400 rpm, and the ball mill time is 2 hours.

[0075] Inert gas is used for protection during the sintering in step 1 and the adsorption in step 2, and the inert gas is selected from nitrogen.

[0076] In the step 1, the sintering temperature is 850° C., and the heating rate of the tubular furnace is 5° C. / min.

[0077] The preparation method of the dispersant in step 1 is:

[0078] H1: 0.36 g of manganese nitrate and 0.6 g of 10,13-epoxy-10,12-octadecadienoic acid were placed in 150 g of water, reacted at 30° C. for 150 minutes, and the water was distilled off;

[0079] H2: Continue to add 22 g of 3-mercaptothiophene, 150 g of N-methylpyrrolidone, and 6 g of sodium ethoxide, react at 70° C. for 150 minutes, then add 20 g of isosorbide divinyl ether, and react at 70° C. for 50 minutes to obtain a dispersant.

[0080] The reaction temperature in step H1 is 30°C, and the reaction temperature in step H2 is 70°C.

[0081] The adsorption temperature of the reactor in step 2 is 85°C.

[0082] Comparative Example 1

[0083] In this comparative example, no dispersant was added, and the remaining steps were the same as those in Example 1.

[0084] Comparative Example 2

[0085] In this comparative example, 10,13-epoxy-10,12-octadecadienoic acid was not added during the preparation of the dispersant, and the remaining steps were consistent with those in Example 1.

[0086] Comparative Example 3

[0087] In this comparative example, 3-mercaptothiophene was not added during the preparation of the dispersant, and the remaining steps were consistent with those of Example 1.

[0088] Electrochemical performance test of iodine-loaded porous cathode materials

[0089] The positive electrode material, binder PVDF, and acetylene black prepared in the above embodiment and comparative example were mixed evenly in a ratio of 80:10:10, and then evenly coated on zinc foil after being prepared into a paste with water, and dried in a vacuum oven at 80°C for 12 hours to obtain a positive electrode. A 2016-type button-type zinc ion battery was assembled with zinc foil as the negative electrode, zinc sulfate aqueous solution as the electrolyte, and glass fiber diaphragm as the diaphragm. The first discharge specific capacity and the discharge specific capacity after 200 cycles were tested in the voltage range of 1.0-1.8V and the current density of 260mA / g. The electrochemical properties of the composite positive electrode materials in each embodiment and comparative example are shown in Table 1.

[0090] Table 1 Electrochemical properties of positive electrode materials corresponding to the examples and comparative examples

[0091]

[0092] From the electrochemical performance test results of the positive electrode materials prepared in the above examples and comparative examples, it can be seen that the positive electrode material prepared by this method has excellent specific capacity, cycle and rate performance.

[0093] It should be understood that the above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with the technology to understand the content of the present invention and implement it accordingly, and they cannot be used to limit the protection scope of the present invention. Any equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing an iodine-loaded porous positive electrode material for a zinc battery, the operating steps of which are: Step 1: Weigh 45-60 parts of precursor manganese carbonate, 30-50 parts of carbon source and 0.007-0.07 parts of dispersant by mass, use a planetary ball mill for ball milling, transfer the mixed powder after ball milling to a tube furnace for sintering for 1-3 hours, cool to room temperature, and wash repeatedly with dilute hydrochloric acid and deionized water, and then dry; Step 2: Weigh 50-75 parts of the mixture prepared in step 1 and 90-180 parts of iodine, use a planetary ball mill to mix them, transfer the mixed powder after ball milling to a reactor, heat the reactor for adsorption for 8-12 hours, evacuate the reactor, continue to keep warm for 2-5 hours, and slowly cool down to obtain an iodine-loaded porous positive electrode material for zinc batteries.

2. The method for preparing an iodine-loaded porous positive electrode material for a zinc battery according to claim 1, characterized in that: In the step 1, the carbon source is selected from at least one of sucrose, maltose, glucose and citric acid.

3. The method for preparing an iodine-loaded porous positive electrode material for a zinc battery according to claim 1, characterized in that: In the steps 1 and 2, the ball milling jar is made of agate, the ball milling beads are made of zirconium beads, the ball milling speed is 200-400 rpm, and the ball milling time is 0.5-2 hours.

4. The method for preparing an iodine-loaded porous positive electrode material for a zinc battery according to claim 1, characterized in that: Inert gas is used for protection during the sintering in step 1 and the adsorption in step 2. The inert gas is selected from one of argon, helium or nitrogen.

5. The method for preparing an iodine-loaded porous positive electrode material for a zinc battery according to claim 1, characterized in that: In the step 1, the sintering temperature is 650-850° C., and the heating rate of the tubular furnace is 2-5° C. / min.

6. The method for preparing an iodine-loaded porous positive electrode material for a zinc battery according to claim 1, characterized in that: The preparation method of the dispersant in step 1 is: H1: 0.18-0.36 parts of manganese nitrate and 0.3-0.6 parts of 10,13-epoxy-10,12-octadecadienoic acid were weighed and placed in 100-150 parts of water, reacted at 20-30°C for 100-150 minutes, and the water was distilled off; H2: Continue to add 11-22 parts of 3-mercaptothiophene, 100-150 parts of N-methylpyrrolidone, and 3-6 parts of sodium ethoxide, react at 60-70°C for 100-150 minutes, then add 10-20 parts of isosorbide divinyl ether, react at 60-70°C for 30-50 minutes to obtain a dispersant.

7. The method for preparing an iodine-loaded porous positive electrode material for a zinc battery according to claim 6, characterized in that: The reaction temperature in step H1 is 20-30°C, and the reaction temperature in step H2 is 60-70°C.

8. The method for preparing an iodine-loaded porous positive electrode material for a zinc battery according to claim 1, characterized in that: The adsorption temperature of the reactor in step 2 is 65-85°C.

Citation Information

Cited By

  • High-capacity stable manganese-iodine composite material, preparation method and application thereof, preparation method of positive electrode material, positive electrode plate and zinc ion battery

    CN120824341A