Positive pole piece as well as preparation method and application thereof
By using a stacked waterproof conductive breathable layer and catalytic layer in the positive electrode sheet of the air battery, the conductive particles are used to reduce the resistance and improve the oxygen adsorption capacity, the problem of large existing positive electrode resistance is solved, and the current density of the air battery is significantly improved. Energy density.
Patent Information
- Application Number
- CN202410934796.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-12
- Publication Date
- 2024-11-12
AI Technical Summary
The positive electrode of the existing air battery has a large resistance, resulting in poor performance, affecting the performance of the overall battery.
A positive electrode sheet is designed, using a laminated waterproof conductive breathable layer, current collector layer and catalytic layer. The conductive particles include platinum, carbon platinum platinum, carbon silver plating, carbon nickel plating or carbon gold plating, and the excellent conductivity of the conductive particles is carried out. The properties and catalytic effects reduce resistance, improve oxygen adsorption capacity, and enhance current density and energy density.
It significantly reduces the resistance of the positive electrode plate, improves the current density and energy density of the air battery, enhances the oxygen entry speed, improves the overall performance, and obtains the positive electrode plate with low resistance, high breathability and excellent waterproof performance through a simple process. .
Smart Images

Figure CN118943385A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of batteries, and in particular relates to a positive electrode sheet and a preparation method and application thereof. Background Art
[0002] Air battery is a kind of chemical battery, which has the characteristics of low cost, long life, high energy density, and environmental friendliness. Air battery usually includes a positive electrode, an electrolyte and a metal negative electrode, among which the performance of the positive electrode greatly affects the performance of the air battery. At present, the resistance of the positive electrode in the related technology is large, which makes the performance of the air battery poor. Summary of the invention
[0003] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides a positive electrode sheet having the characteristic of low resistance.
[0004] The invention also provides an air battery.
[0005] The present invention also proposes the application of the positive electrode plate.
[0006] In the first aspect of the present invention, a positive electrode plate is proposed, comprising a stacked waterproof, conductive, and breathable layer, a current collector layer, and a catalytic layer, wherein the waterproof, conductive, and breathable layer comprises a mixed material I, wherein the mixed material I comprises conductive particles I and a carbon material I, wherein the conductive particles I comprise at least one of platinum, carbon-plated platinum, carbon-supported platinum, carbon-plated silver, carbon-plated nickel, or carbon-plated gold.
[0007] The positive electrode sheet according to the embodiment of the present invention has at least the following beneficial effects:
[0008] The waterproof conductive breathable layer of the present invention adds a specific type of conductive particles I, which have excellent conductivity, can significantly reduce the resistance of the positive electrode sheet, improve the performance of the positive electrode sheet, and apply the positive electrode sheet to the air battery, which can significantly improve the current density of the air battery. In addition, the conductive particles I in the present invention have the catalytic effect, and are also porous and have a large specific surface area, so they have an excellent effect of absorbing oxygen, accelerate the entry of oxygen, thereby accelerating the formation of current, and improving the energy density of the positive electrode sheet.
[0009] In some embodiments of the present invention, the conductive particles I include one or two of carbon-supported platinum, carbon-plated platinum, carbon-plated silver, carbon-plated nickel, carbon-plated gold or platinum.
[0010] In some embodiments of the present invention, the conductive particles I include one or two of carbon-plated platinum, carbon-plated silver, carbon-plated nickel or carbon-plated gold.
[0011] In some embodiments of the present invention, the average particle size of the conductive particles I is 10 nm-100 μm, and can be 40 nm-20 μm.
[0012] In some embodiments of the present invention, the average particle size of the carbon-plated silver in the conductive particles I is 5-50 μm, and can be 10-30 μm.
[0013] In some embodiments of the present invention, the average particle size of the carbon-plated platinum in the conductive particles I is 10-200nm, and can be 30-60nm. In some embodiments of the present invention, the average particle size of the carbon-plated gold in the conductive particles I is 10-200nm, and can be 30-60nm. In some embodiments of the present invention, the average particle size of the carbon-plated nickel in the conductive particles I is 10-200nm, and can be 30-60nm.
[0014] In some embodiments of the present invention, the specific surface area of the conductive particles I is in the range of 10-100 m 2 / g, optional 40-60m 2 / g.
[0015] In some embodiments of the present invention, in the waterproof, conductive, breathable layer, the mass fraction of the conductive particles I is 0.1-60%, such as 15-60% by mass.
[0016] In some embodiments of the present invention, the carbon material I includes at least one of conductive carbon black, acetylene black or activated carbon.
[0017] In some embodiments of the present invention, the waterproof, conductive and breathable layer further includes an adhesive I.
[0018] In some embodiments of the present invention, the binder I includes at least one of PVDF, PTFE or PVA.
[0019] In some embodiments of the present invention, the raw material of the binder I includes at least one of PVDF emulsion, PTFE emulsion or PVA emulsion.
[0020] In some embodiments of the present invention, in the waterproof, conductive and breathable layer, the mass fraction of the binder I is 20-80%.
[0021] In some embodiments of the present invention, the raw materials for preparing the waterproof, conductive and breathable layer include raw materials for binder I, mixed material I and pore-forming agent I.
[0022] In some embodiments of the present invention, the pore-forming agent I comprises at least one of ammonium bicarbonate, polyethylene glycol, sodium chloride or polyvinyl alcohol.
[0023] In some embodiments of the present invention, the mass ratio of the mixed material I to the pore-forming agent I is (5-10):(1-6).
[0024] In some embodiments of the present invention, the thickness of the waterproof, conductive, breathable layer is 0.02-0.5 mm, and can be optionally 0.02-0.2 mm.
[0025] In some embodiments of the present invention, the air permeability of the waterproof conductive breathable layer is 50-500 mL / m 2 *min@7kpa.
[0026] In some embodiments of the present invention, the sheet resistance of the waterproof, conductive and breathable layer is 10-200Ω / sq.
[0027] In some embodiments of the present invention, the current collector layer is a metal current collector layer.
[0028] In some embodiments of the present invention, the metal current collector layer includes a metal mesh. Optionally, the metal mesh includes but is not limited to one or more of a nickel mesh, a stainless steel mesh, or a copper mesh.
[0029] In some embodiments of the present invention, the mesh size of the metal mesh is 20-100 meshes, and can be optionally 20-60 meshes.
[0030] In some embodiments of the present invention, the thickness of the current collector layer is 0.01-0.15 mm.
[0031] In some embodiments of the present invention, the sheet resistance of the current collector layer is 2-20Ω / sq.
[0032] In some embodiments of the present invention, the catalytic layer includes a mixed material II, a catalyst and a binder II, and the mixed material II includes conductive particles II and carbon material II.
[0033] In some embodiments of the present invention, the conductive particles II include at least one of platinum, carbon-plated platinum, carbon-supported platinum, carbon-plated silver, carbon-plated nickel, or carbon-plated gold.
[0034] In some embodiments of the present invention, the conductive particles II include one or two of carbon-plated platinum, carbon-supported platinum, carbon-plated silver, carbon-plated nickel, carbon-plated gold or platinum.
[0035] In some embodiments of the present invention, the conductive particles II include one or two of carbon-plated platinum, carbon-plated silver, carbon-plated nickel, or carbon-plated gold-plated platinum.
[0036] In some embodiments of the present invention, the catalyst includes at least one of manganese dioxide, a perovskite-type oxide catalyst, Pt, or a metal macrocyclic compound catalyst.
[0037] In some embodiments of the invention, the catalyst comprises manganese dioxide.
[0038] Through the above implementation, the conductive particles II have catalytic properties and conductive properties, and can cooperate with the catalyst (such as manganese dioxide) to improve the catalytic efficiency. In some embodiments of the present invention, the addition of conductive particles II can increase the energy density of the catalytic layer by 10-15%.
[0039] In some embodiments of the present invention, the average particle size of the conductive particles II is 10 nm-100 μm, and can be 30 nm-50 μm.
[0040] In some embodiments of the present invention, the average particle size of the carbon-plated silver in the conductive particles II is 10-70 μm, and can be 40-60 μm.
[0041] In some embodiments of the present invention, the average particle size of the carbon-plated platinum in the conductive particles II is 10-200nm, and can be 30-60nm. In some embodiments of the present invention, the average particle size of the carbon-plated gold in the conductive particles II is 10-200nm, and can be 30-60nm. In some embodiments of the present invention, the average particle size of the carbon-plated nickel in the conductive particles II is 10-200nm, and can be 30-60nm.
[0042] In some embodiments of the present invention, the specific surface area of the conductive particles II is 180-350 m 2 / g, such as 205-282m 2 / g.
[0043] In some embodiments of the present invention, in the catalytic layer, the mass fraction of the conductive particles II is 10-60%, such as optionally 15-60%.
[0044] In some embodiments of the present invention, the carbon material II includes at least one of conductive carbon black, acetylene black or activated carbon.
[0045] In some embodiments of the present invention, the binder II includes at least one of PVDF, PTFE or PVA.
[0046] In some embodiments of the present invention, the raw material of the binder II includes at least one of PVDF emulsion, PTFE emulsion or PVA emulsion.
[0047] In some embodiments of the present invention, in the catalytic layer, the mass fraction of the binder II is 30-70%.
[0048] In some embodiments of the present invention, in the catalytic layer, the mass ratio of the mixed material II to the catalyst is (5-20):(5-10).
[0049] In some embodiments of the present invention, the thickness of the catalytic layer is 0.02-0.3 mm.
[0050] In some embodiments of the present invention, the air permeability of the catalyst layer is 50-500 mL / m 2 *min@7kpa.
[0051] In some embodiments of the present invention, the sheet resistance of the catalytic layer is 10-50Ω / sq.
[0052] In some embodiments of the present invention, a gas diffusion layer is provided between the waterproof conductive breathable layer and the current collector layer.
[0053] In some embodiments of the present invention, the gas diffusion layer comprises a carbon material layer.
[0054] In some embodiments of the present invention, the carbon material layer includes at least one of carbon paper, carbon cloth or carbon felt.
[0055] Through the above implementation, the carbon material diffusion layer is used as a gas diffusion layer, which is conducive to the air that passes through the waterproof conductive breathable layer to be evenly distributed in the metal current collecting layer, allowing the air to fully contact the catalyst electrolyte to increase the current density and energy density. The provision of the gas diffusion layer can increase the mechanical strength and soft toughness of the positive electrode sheet and increase the energy density of the battery.
[0056] In some embodiments of the present invention, the thickness of the gas diffusion layer is 0.01-0.4 mm.
[0057] In some embodiments of the present invention, the gas diffusion layer has an air permeability of 20-50 L / m 2 *min@7kpa.
[0058] In some embodiments of the present invention, the sheet resistance of the gas diffusion layer is 5-50Ω / sq.
[0059] The second aspect of the present invention proposes a method for preparing a positive electrode plate, comprising the following steps: stacking a waterproof, conductive, and breathable prefabricated layer, a gas diffusion prefabricated layer, a current collector prefabricated layer, and a catalytic prefabricated layer, and pressing them together to form a stacked waterproof, conductive, and breathable layer, a gas diffusion layer, a current collector layer, and a catalytic layer to obtain the positive electrode plate.
[0060] The method for preparing the positive electrode sheet according to the embodiment of the present invention has at least the following beneficial effects:
[0061] The preparation method of the positive electrode plate of the present invention has the advantages of simple process, easy operation, short production cycle, controllable film thickness, etc. The prepared positive electrode plate has the characteristics of low resistance, good air permeability and excellent waterproof performance.
[0062] In some embodiments of the present invention, the waterproof, conductive and breathable prefabricated layer has a thickness of 0.01-0.7 mm.
[0063] In some embodiments of the present invention, the thickness of the gas diffusion prefabricated layer is 0.01-0.5 mm.
[0064] In some embodiments of the present invention, the thickness of the current collector prefabricated layer is 0.05-0.3 mm.
[0065] In some embodiments of the present invention, the thickness of the catalytic prefabricated layer is 0.01-0.5 mm.
[0066] In some embodiments of the present invention, during the pressing step, 10-100 kg / cm 2 The pressure is 5-20 minutes.
[0067] In some embodiments of the present invention, after the pressing, sintering is performed to obtain the positive electrode sheet.
[0068] In some embodiments of the present invention, in the sintering step, the sintering is performed at 300-400° C. for 1-3 hours.
[0069] In some embodiments of the present invention, the positive electrode sheet is obtained by pressing, sintering and cutting.
[0070] In some embodiments of the present invention, the waterproof, conductive and breathable prefabricated layer, the gas diffusion prefabricated layer, the current collector prefabricated layer and the catalytic prefabricated layer are stacked and then pressed.
[0071] In some embodiments of the present invention, the preparation method comprises the following steps: stacking the waterproof conductive breathable prefabricated layer, the gas diffusion prefabricated layer, the current collector prefabricated layer and the catalytic prefabricated layer in sequence, pressing and sintering them to obtain the positive electrode sheet.
[0072] In some embodiments of the present invention, the preparation method comprises the following steps: stacking the waterproof conductive breathable prefabricated layer, the gas diffusion prefabricated layer, the current collector prefabricated layer and the catalytic prefabricated layer in sequence, and placing them on a mold coated with polytetrafluoroethylene for pressing.
[0073] In some embodiments of the present invention, the preparation method includes preparing a waterproof, conductive and breathable prefabricated layer, which specifically includes the following operations:
[0074] Sa-1, mixing an alcohol solvent with mixed material I, adding pore former I, adding raw materials of binder I, stirring, separating, and obtaining coagulation material I;
[0075] Sa-2, the condensate I is pressed for a second time and dried to obtain a waterproof, conductive and breathable prefabricated layer.
[0076] In some embodiments of the present invention, the alcohol solvent includes at least one of ethanol or propanol. Alternatively, the alcohol solvent includes at least one of anhydrous ethanol or anhydrous propanol. Specifically, the propanol can be selected from at least one of n-propanol or isopropanol.
[0077] Through the above implementation, when the alcohol solvent in the present invention volatilizes at high temperature, air gaps will appear due to the expansion of the gas. However, the alcohol solvent is a liquid, so the air gap will be very small. It can be combined with the gasification of the pore-forming agent I during the subsequent sintering step to increase the air permeability, increase the number of pores, and thus increase the air permeability of the waterproof conductive air permeable layer. In some embodiments of the present invention, the air permeability of the positive electrode plate can reach 100mL / cm 2 *min(@7kpa) or above.
[0078] In some embodiments of the present invention, in step Sa-1, the mass ratio of the raw materials of the mixed material I and the binder I is (3-10):(0.5-5).
[0079] In some embodiments of the present invention, in step Sa-1, anhydrous ethanol is mixed with mixed material I. Preferably, the ratio of anhydrous ethanol to mixed material I is (20-50) mL: (3-10) g.
[0080] In some embodiments of the present invention, in step Sa-1, anhydrous ethanol is mixed with conductive particles I and carbon material I.
[0081] In some embodiments of the present invention, in step Sa-1, after adding the mixed material I to the anhydrous ethanol, the material is dispersed by stirring with a stirrer for 10-90 minutes, or dispersed by ultrasound for 10-50 minutes, and then the pore-forming agent I is added.
[0082] In some embodiments of the present invention, in step Sa-1, after adding the pore-forming agent I, the mixture is stirred or ultrasonically dispersed for 10-50 minutes, and then the binder I is added.
[0083] In some embodiments of the present invention, in step Sa-1, the raw materials of binder I are added, stirred until agglomerates are formed, and then agglomerates I are separated.
[0084] In some embodiments of the present invention, in step Sa-2, the secondary pressing step comprises: rolling the coagulation I for 10-20 minutes, placing it in a mold, and then using a hydraulic press to press the coagulation I in the mold. Optionally, the pressing method is cold pressing.
[0085] In some embodiments of the present invention, in step Sa-2, after secondary pressing, drying is performed to obtain a waterproof, conductive, breathable layer. Optionally, the pressing parameters of the hydraulic press include: a pressure of 10-100 kg / cm 2 Optionally, the condensate I is pressed down to a preset thickness I by a hydraulic press, and the pressure is maintained for 3-10 minutes. Optionally, the preset thickness I is 0.01-0.7 mm.
[0086] Through the above-mentioned implementation mode, the present invention adopts a secondary pressing film-forming process, which first uses an open mill and other devices to roll the film once, and then uses a flat hydraulic press to cold-press the film for the second time. Since the secondary cold-pressing film-forming uses a mold, the thickness of the film can be controlled and the thickness is more uniform, which well solves the problem that the waterproof film in the related technology is difficult to make thin or the thickness is uneven.
[0087] In some embodiments of the present invention, in step Sa-2, after the coagulant I is rolled in a rubber mill for 10-20 minutes, the coagulant I is placed on a mold of target thickness, and the mold is placed on a hydraulic press at a pressure of 10-100 kg / cm 2 , press down to a preset thickness and keep the pressure for 3-10 minutes, then dry to obtain a waterproof, conductive and breathable prefabricated layer.
[0088] In some embodiments of the present invention, in step Sa-2, the drying temperature is 50-100° C., and the drying time is 30-100 min.
[0089] In some embodiments of the present invention, the raw materials for preparing the catalytic layer include raw materials for binder II, ethanol, mixed material II and a catalyst.
[0090] In some embodiments of the present invention, the raw materials for preparing the catalytic layer further include pore former II.
[0091] In some embodiments of the present invention, the pore former II comprises at least one of ammonium bicarbonate, polyethylene glycol, sodium chloride or polyvinyl alcohol.
[0092] In some embodiments of the present invention, the preparation method includes preparing a catalytic prefabricated layer, specifically comprising the following operations:
[0093] Sb-1, mixing ethanol with mixed material II and a catalyst, adding the raw material of binder II, stirring, separating, and obtaining a coagulant II;
[0094] Sb-2, pressing and drying the condensate II to obtain a catalytic prefabricated layer.
[0095] In some embodiments of the present invention, in step Sb-1, ethanol is mixed with mixed material II and a catalyst, pore-forming agent II is added, raw materials of binder II are added, stirred, and separated to obtain coagulant II.
[0096] In some embodiments of the present invention, in step Sb-1, the mass ratio of the mixed material II to the pore-forming agent II is (0.5-10):1.
[0097] In some embodiments of the present invention, in step Sb-1, the mass ratio of the raw materials of the mixed material II and the binder II is (1-8):(1-5).
[0098] In some embodiments of the present invention, in step Sb-1, anhydrous ethanol is mixed with mixed material II and a catalyst. Preferably, the ratio of anhydrous ethanol to mixed material II and a catalyst is (20-50) mL: (1-8) g: (0.5-5) g.
[0099] In some embodiments of the present invention, in step Sb-1, anhydrous ethanol is mixed with conductive particles II and carbon material II.
[0100] In some embodiments of the present invention, in step Sb-1, after adding the mixed material II and the catalyst to the anhydrous ethanol, the mixture is stirred and dispersed for 10-30 minutes using a stirrer, or ultrasonically dispersed for 10-30 minutes, and then the raw materials of the binder II are added.
[0101] In some embodiments of the present invention, in step Sb-1, the raw material of binder II is added, stirred until agglomerates are formed, and then agglomerates II are separated.
[0102] In some embodiments of the present invention, in step Sb-2, the condensate II is rolled for 10-20 minutes, placed in a mold, and then the condensate II in the mold is pressed by a hydraulic press and dried to obtain a catalytic prefabricated layer. Preferably, the pressing parameters of the hydraulic press include: a pressure of 10-100 kg / cm 2 Optionally, a hydraulic press is used to press the condensate II down to a preset thickness II and then the pressure is maintained for 3-10 minutes. Optionally, the preset thickness II is 0.01-0.5 mm.
[0103] In some embodiments of the present invention, in step Sb-2, after the coagulant II is rolled in a rubber mill for 10-20 minutes, the coagulant II is placed on a mold of target thickness, and the mold is placed on a hydraulic press at a pressure of 10-100 kg / cm 2 , press down for 3-10 minutes, and then dry to obtain a catalytic prefabricated layer.
[0104] In some embodiments of the present invention, in step Sb-2, the drying temperature is 50-100° C., and the drying time is 30-100 min.
[0105] According to a third aspect of the present invention, an air battery is provided, wherein the air battery comprises the above-mentioned positive electrode plate.
[0106] In some embodiments of the present invention, the air battery further includes an electrolyte and a negative electrode plate. BRIEF DESCRIPTION OF THE DRAWINGS
[0107] The present invention will be further described below with reference to the accompanying drawings and embodiments, wherein:
[0108] Figure 1 Schematic diagram of the structure of the positive electrode plate in Example 4 of the present invention. DETAILED DESCRIPTION
[0109] The following will be combined with the embodiments to clearly and completely describe the concept of the present invention and the technical effects produced, so as to fully understand the purpose, characteristics and effects of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, other embodiments obtained by those skilled in the art without creative work are all within the scope of protection of the present invention.
[0110] The parameters not specifically described in the following examples are conventional settings in the art and are technical information disclosed in the industry. Therefore, even if they are not described, they will not affect the understanding of the specific implementation methods of the technical solution of the present invention and the scope of protection actually claimed by the present invention by those skilled in the art. The experimental methods in the following examples without specifying specific conditions are usually carried out according to conventional conditions in the art or according to the conditions recommended by the manufacturer; the raw materials, reagents, etc. used, unless otherwise specified, are all raw materials and reagents that can be obtained from commercial channels such as conventional markets.
[0111] In the mixed carbon powder I: carbon-plated silver: the average particle size is 20 μm (Japan CAG-45, carbon-plated silver can also be purchased from other manufacturers); carbon-plated platinum: the average particle size is 50 nm, and the mass fraction of platinum in the carbon-plated platinum is 5%; carbon-plated gold: the average particle size is 40 nm, and the mass fraction of gold in the carbon-plated gold is 5%; the specific surface area of each carbon-plated metal ranges from 40 to 60 m 2 / g;
[0112] In mixed carbon powder II: Carbon silver plating: average particle size is 50μm (the mass fraction of silver in carbon silver plating is 50%), Nantong Yijie YJ15S40. Carbon silver plating produced by other manufacturers can also be purchased; Carbon platinum plating: average particle size is 30-50nm, the mass fraction of platinum in carbon platinum plating is 5%; Carbon gold plating: average particle size is 40nm, the mass fraction of gold in carbon gold plating is 5%; the specific surface area of each carbon-plated metal ranges from 205-282m 2 / g;
[0113] Nickel mesh: thickness 0.02mm, mesh size 80;
[0114] PTFE: Chemours, DISP 30. PTFE products from other manufacturers can also be purchased.
[0115] PVDF: Solvay 5130S, PVDF products produced by other manufacturers can also be purchased;
[0116] Hydraulic press: purchased from Foshan Hexing Hydraulic Machinery Co., Ltd.; model YG73-50T.
[0117] Example 1
[0118] This embodiment discloses a positive electrode sheet, which includes a waterproof conductive air-permeable layer, a current collector layer, and a catalyst layer stacked in sequence, with thicknesses of approximately 0.2 mm, 0.05 mm, and 0.15 mm, respectively. The preparation process of the positive electrode sheet includes:
[0119] (I) Preparation of a waterproof, conductive and breathable prefabricated layer, specifically comprising:
[0120] 1) Pour 200 mL of anhydrous ethanol into a container, then pour 40 g of mixed carbon powder I (including 10 g of carbon-plated silver, 20 g of acetylene black, and 10 g of activated carbon) into the anhydrous ethanol, and use a stirrer to disperse for 20 min (ultrasonic dispersion for 10 min may also be used); then add 10 g of ammonium bicarbonate, stir or ultrasonically disperse for 10 min to obtain a mixed solution I; add 50 g of a binder (PVDF emulsion with a solid content of 60%) to the mixed solution I, use a stirrer to stir until agglomerates are formed, and then separate the agglomerates from the solvent;
[0121] 2) Place the coagulant in a rubber mixing mill (speed ratio: 1:1.2) and roll it for 10 minutes (first pressing). Then place the coagulant on a mold of target thickness. Place the mold on a hydraulic press and cold press (room temperature) at a pressure of 20 kg / cm 2 , press down to the target thickness and keep the pressure for 3 minutes (second pressing) and then take out to obtain a film layer I with a thickness of 0.2 mm;
[0122] 3) Dry the membrane layer I in a drying oven at 60° C. for 100 min, and take it out to obtain a waterproof, conductive, and breathable prefabricated layer;
[0123] (II) Preparation of the catalytic prefabricated layer, specifically comprising:
[0124] 1) Pour 200 mL of anhydrous ethanol (200-500 mL) into a container, then pour 15 g of mixed carbon powder II (including 10 g of carbon-plated silver and 5 g of conductive carbon black) into the anhydrous ethanol, and also pour 10 g of manganese dioxide into the anhydrous ethanol, and use a stirrer to disperse for 10 min (ultrasonic dispersion for 10 min can also be used) to obtain a mixed solution II; pour 50 g of a binder (PVDF emulsion with a solid content of 60%) into the mixed solution II, use a stirrer to stir until agglomerates are formed, and then separate the agglomerates from the solvent;
[0125] 2) Place the coagulant in a rubber mixing mill (speed ratio: 1:1.2) and roll it for 10 minutes. Then place the coagulant on a mold of target thickness. Place the mold on a hydraulic press and press it (at room temperature) at a pressure of 10 kg / cm 2 , press down to the target thickness and keep the pressure for 3 minutes before taking out to obtain the film layer II with a thickness of 0.15mm;
[0126] 3) Place the membrane layer II in a drying oven at 100°C and dry it for 50 minutes (30-100 minutes is acceptable), then take it out to obtain a catalytic prefabricated layer.
[0127] (III) Pressing into film:
[0128] The waterproof conductive breathable prefabricated layer, the nickel mesh and the catalytic prefabricated layer are stacked together in order, and the three are placed on a mold coated with Teflon (polytetrafluoroethylene) and a 20kg / cm 2 The pressure was applied and pressed for 5 minutes. After being taken out, it was placed in a high-temperature oven and sintered at 340°C for 1 hour to obtain a laminated waterproof, conductive, and breathable layer, a current collector layer, and a catalyst layer. The laminated layers were cut to obtain a positive electrode sheet.
[0129] This embodiment also discloses an air battery, including the positive electrode plate in this embodiment.
[0130] Example 2
[0131] This embodiment discloses a positive electrode sheet, which includes a waterproof conductive air-permeable layer, a current collector layer, and a catalyst layer stacked in sequence, with thicknesses of approximately 0.2 mm, 0.05 mm, and 0.15 mm, respectively. The preparation process of the positive electrode sheet includes:
[0132] (I) Preparation of a waterproof, conductive and breathable prefabricated layer, specifically comprising:
[0133] 1) Pour 200 mL of anhydrous ethanol into a container, then pour 50 g of mixed carbon powder I (including 20 g of carbon-plated platinum, 20 g of acetylene black, and 10 g of activated carbon) into the anhydrous ethanol, and use a stirrer to disperse for 30 minutes (ultrasonic dispersion for 20 minutes may also be used); then add 15 g of sodium chloride, stir or ultrasonically disperse for 10 minutes to obtain a mixed solution I; add 40 g of a binder (PTFE emulsion with a solid content of 60%) to the mixed solution I, use a stirrer to stir until agglomerates are formed, and then separate the agglomerates from the solvent;
[0134] 2) Place the coagulant in a rubber mixing mill (speed ratio: 1:1.2) and roll it for 12 minutes. Then place the coagulant on a mold of target thickness. Place the mold on a hydraulic press and press it (at room temperature) at a pressure of 25 kg / cm 2 , press down to the target thickness and hold the pressure for 3 minutes before taking out to obtain a film layer I with a thickness of 0.2 mm;
[0135] 3) Dry the membrane layer I in a drying oven at 65°C for 90 minutes, and take it out to obtain a waterproof, conductive and breathable prefabricated layer;
[0136] (II) Preparation of the catalytic prefabricated layer, specifically comprising:
[0137] 1) Pour 300 mL of anhydrous ethanol into a container, then pour 30 g of mixed carbon powder II (including 10 g of carbon-plated silver and 20 g of conductive carbon black) into the anhydrous ethanol, and also pour 10 g of manganese dioxide into the container, and stir and disperse them for 10 min using a stirrer (ultrasonic dispersion for 10 min may also be used) to obtain a mixed solution II; pour 50 g of a binder (PTFE emulsion with a solid content of 60%) into the mixed solution II, stir with a stirrer until agglomerates are formed, and then separate the agglomerates from the solvent;
[0138] 2) Place the coagulant in a rubber mixing mill (speed ratio: 1:1.2) and roll it for 10 minutes. Then place the coagulant on a mold of target thickness. Place the mold on a hydraulic press and press it (at room temperature) at a pressure of 10 kg / cm 2 , press down to the target thickness and keep the pressure for 3 minutes before taking out to obtain the film layer II with a thickness of 0.15mm;
[0139] 3) Place the membrane layer II in a drying oven at 100°C and dry it for 50 minutes (30-100 minutes is acceptable), then take it out to obtain a catalytic prefabricated layer.
[0140] (III) Pressing into film:
[0141] The waterproof conductive breathable prefabricated layer, the nickel mesh and the catalytic prefabricated layer are stacked together in order, and the three are placed on a mold coated with Teflon (polytetrafluoroethylene) and a 20kg / cm 2The pressure was applied for 5 minutes, and then the mixture was taken out and placed in a high temperature oven for sintering at 340°C for 1 hour to obtain a stacked waterproof conductive breathable layer, a current collector layer and a catalyst layer, which were cut to obtain a positive electrode sheet. The mass fraction of carbon-plated platinum in the waterproof conductive breathable layer was about 20%.
[0142] This embodiment also discloses an air battery, including the positive electrode plate in this embodiment.
[0143] Example 3
[0144] This embodiment discloses a positive electrode sheet, which includes a waterproof conductive air-permeable layer, a current collector layer, and a catalyst layer stacked in sequence, with thicknesses of approximately 0.2 mm, 0.05 mm, and 0.15 mm, respectively. The preparation process of the positive electrode sheet includes:
[0145] (I) Preparation of a waterproof, conductive and breathable prefabricated layer, specifically comprising:
[0146] 1) Pour 300 mL of anhydrous ethanol into a container, then pour 55 g of mixed carbon powder I (including 25 g of carbon gold plating, 20 g of acetylene black, and 10 g of activated carbon) into the anhydrous ethanol, and use a stirrer to disperse for 50 min (ultrasonic dispersion for 20 min may also be used); then add 15 g of sodium chloride, stir or ultrasonically disperse for 10 min to obtain a mixed solution I; add 30 g of a binder (PTFE emulsion with a solid content of 60%) to the mixed solution I, use a stirrer to stir until agglomerates are formed, and then separate the agglomerates from the solvent;
[0147] 2) Place the coagulant in a rubber mixing mill (speed ratio: 1:1.2) and roll it for 15 minutes. Then place the coagulant on a mold of target thickness. Place the mold on a hydraulic press and press it (at room temperature) at a pressure of 40 kg / cm 2 , press down to the target thickness and hold the pressure for 5 minutes before taking out to obtain a film layer I with a thickness of 0.2 mm;
[0148] 3) Dry the membrane layer I in a drying oven at 90° C. for 90 minutes, and take it out to obtain a waterproof, conductive, and breathable prefabricated layer;
[0149] (II) Preparation of the catalytic prefabricated layer, specifically comprising:
[0150] 1) Pour 500 mL of anhydrous ethanol into a container, then pour 30 g of mixed carbon powder II (including 10 g of carbon-plated gold and 20 g of conductive carbon black) into the anhydrous ethanol, and also pour 10 g of manganese dioxide, and then add 10 g of polyvinyl alcohol, and use a stirrer to stir and disperse for 30 min (ultrasonic dispersion can also be used for 20 min) to obtain a mixed solution II; pour 40 g of a binder (PTFE emulsion with a solid content of 60%) into the mixed solution II, use a stirrer to stir until agglomerates are formed, and then separate the agglomerates from the solvent;
[0151] 2) Place the coagulant in a rubber mixing mill (speed ratio: 1:1.2) and roll it for 20 minutes. Then place the coagulant on a mold of target thickness. Place the mold on a hydraulic press and press it (at room temperature) at a pressure of 50 kg / cm 2 , press down for 3 minutes to the target thickness and take out after maintaining the pressure, to obtain a film layer II with a thickness of 0.15 mm;
[0152] 3) Place the membrane layer II in a drying oven at 100°C and dry it for 100 minutes, then take it out to obtain a catalytic prefabricated layer.
[0153] (III) Pressing into film:
[0154] The waterproof conductive breathable prefabricated layer, nickel mesh and catalytic prefabricated layer are stacked together in order, and the three are placed on a mold coated with Teflon (polytetrafluoroethylene) and applied with 100kg / cm 2 The pressure was applied for 5 minutes, and the mixture was taken out and placed in a high temperature oven for sintering at 380°C for 1 hour, and cut to obtain a stacked waterproof conductive breathable layer, a current collector layer and a catalyst layer, and a positive electrode sheet. The mass fraction of carbon-plated gold in the waterproof conductive breathable layer is about 25%.
[0155] This embodiment also discloses an air battery, including the positive electrode plate in this embodiment.
[0156] Example 4
[0157] This embodiment discloses a positive electrode sheet, which includes a waterproof conductive breathable layer, a gas diffusion layer, a current collector layer, and a catalyst layer stacked in sequence, with thicknesses of approximately 0.2 mm, 0.2 mm, 0.05 mm, and 0.15 mm, respectively. The structural schematic diagram of the positive electrode sheet is shown in FIG. Figure 1 As shown, the preparation process of the positive electrode sheet includes:
[0158] (I) Preparation of waterproof, conductive and breathable prefabricated layer: same as in Example 1;
[0159] (II) Preparation of the catalytic prefabricated layer, same as in Example 1;
[0160] (III) Pressing into film:
[0161] The waterproof conductive breathable prefabricated layer, the gas diffusion prefabricated layer (carbon cloth with a thickness of 0.12 mm), the nickel mesh and the catalytic prefabricated layer are stacked together in order, and the four are placed on a mold coated with Teflon (polytetrafluoroethylene) and a 100 kg / cm 2 The pressure was applied and pressed for 5 minutes. After being taken out, it was placed in a high-temperature oven and sintered at 380°C for 1 hour to obtain a laminated waterproof, conductive, breathable layer, a gas diffusion layer, a current collector layer, and a catalyst layer, which were then cut to obtain a positive electrode sheet.
[0162] This embodiment also discloses an air battery, including the positive electrode plate in this embodiment.
[0163] Example 5
[0164] This embodiment discloses a positive electrode plate, which is different from Embodiment 4 in that the positive electrode plate in this embodiment does not contain a gas diffusion layer.
[0165] This embodiment also discloses an air battery, including the positive electrode plate in this embodiment.
[0166] Example 6
[0167] This embodiment discloses a positive electrode sheet, which includes a waterproof conductive air-permeable layer, a current collector layer, and a catalyst layer stacked in sequence, with thicknesses of approximately 0.2 mm, 0.05 mm, and 0.15 mm, respectively. The preparation process of the positive electrode sheet includes:
[0168] (I) Preparation of a waterproof, conductive and breathable prefabricated layer, specifically comprising:
[0169] 1) Pour 200 mL of anhydrous ethanol into a container, then pour 50 g of mixed carbon powder I (including 10 g of activated carbon, 10 g of conductive carbon black, 0.05 g of carbon-supported platinum, and the rest is acetylene black) into the anhydrous ethanol, and use a stirrer to disperse for 30 minutes (ultrasonic dispersion for 20 minutes may also be used); then add 10 g of ammonium bicarbonate, stir or ultrasonically disperse for 20 minutes to obtain a mixed solution I; add 50 g of a binder (PVA emulsion with a solid content of 60%) to the mixed solution I, use a stirrer to stir until agglomerates are formed, and then separate the agglomerates from the solvent;
[0170] 2) Place the coagulant in a rubber mixing mill (speed ratio: 1:1.2) and roll it for 12 minutes. Then place the coagulant on a mold of target thickness. Place the mold on a hydraulic press and press it (at room temperature) at a pressure of 25 kg / cm 2 , press down to the target thickness and hold the pressure for 3 minutes before taking out to obtain a film layer I with a thickness of 0.2 mm;
[0171] 3) Dry the membrane layer I in a drying oven at 65°C for 90 minutes, and take it out to obtain a waterproof, conductive and breathable prefabricated layer;
[0172] (II) Preparation of the catalytic prefabricated layer, specifically comprising:
[0173] 1) Pour 300 mL of anhydrous ethanol into a container, then pour 40 g of mixed carbon powder II (0.1 g of platinum, 20 g of activated carbon, and the rest is acetylene black) into the anhydrous ethanol, then add 10 g of manganese dioxide, and use a stirrer to disperse for 10 min (ultrasonic dispersion for 10 min may also be used) to obtain a mixed solution II; pour 30 g of a binder (PVA emulsion with a solid content of 60%) into the mixed solution II, use a stirrer to stir until agglomerates are formed, and then separate the agglomerates from the solvent;
[0174] 2) Place the coagulant in a rubber mixing mill (speed ratio: 1:1.2) and roll it for 15 minutes. Then place the coagulant on a mold of target thickness. Place the mold on a hydraulic press and press it (at room temperature) at a pressure of 60 kg / cm 2 , press down to the target thickness and keep the pressure for 3 minutes before taking out to obtain the film layer II with a thickness of 0.15mm;
[0175] 3) Place the membrane layer II in a drying oven at 100°C and dry it for 50 minutes (30-100 minutes is acceptable), then take it out to obtain a catalytic prefabricated layer.
[0176] (III) Pressing into film:
[0177] The waterproof conductive breathable prefabricated layer, the nickel mesh and the catalytic prefabricated layer are stacked together in order, and the three are placed on a mold coated with Teflon (polytetrafluoroethylene) and a 20kg / cm 2 The pressure was applied and pressed for 5 minutes. After being taken out, the layer was placed in a high-temperature oven and sintered at 340°C for 1 hour to obtain a laminated waterproof, conductive, and breathable layer, a current collector layer, and a catalyst layer, which were then cut to obtain a positive electrode sheet.
[0178] This embodiment also discloses an air battery, including the positive electrode plate in this embodiment.
[0179] Example 7
[0180] This embodiment discloses a positive electrode sheet, which is different from the embodiment 3 in that a gas diffusion layer (carbon cloth with a thickness of 0.12 mm) is added between the waterproof conductive gas permeable layer and the current collector layer in the positive electrode sheet of this embodiment. Specifically, the steps of preparing the positive electrode sheet in this embodiment include:
[0181] (I) to (II): Same as Example 3;
[0182] (III) Pressing into film:
[0183] The waterproof conductive breathable prefabricated layer, carbon cloth, nickel mesh and catalytic prefabricated layer are stacked together in order, and the three are placed on a mold coated with Teflon (polytetrafluoroethylene) and applied with 100kg / cm 2The pressure was applied and pressed for 5 minutes. After being taken out, the mixture was placed in a high-temperature oven and sintered at 380°C for 1 hour. The mixture was cut to obtain a laminated waterproof, conductive, and breathable layer, a gas diffusion layer, a current collector layer, and a catalyst layer to obtain a positive electrode sheet.
[0184] This embodiment also discloses an air battery, including the positive electrode plate in this embodiment.
[0185] In some other embodiments of the present invention, the thickness of the waterproof conductive breathable layer in the positive electrode plate is 0.02-0.2 mm, and the air permeability is 50-500 mL / cm 2 *min@7kpa, square resistance is 10-200Ω / sq; and / or, the thickness of the current collector layer is 0.01-0.15mm, square resistance is 2-20Ω / sq; and / or, the thickness of the catalyst layer is 0.02-0.3mm, square resistance is 10-50Ω / sq; and / or, the thickness of the gas diffusion layer is 0.01-0.4mm, and the air permeability is 20-50L / cm 2 *min@7kpa, square resistance is 5-50Ω / sq.
[0186] Comparative Example 1
[0187] This comparative example discloses a positive electrode plate, which is different from Example 4 in that: in the preparation of the waterproof, conductive and breathable prefabricated layer in step (Ⅰ) of this comparative example: the mixed carbon powder Ⅰ used does not contain carbon silver plating, and the mixed carbon powder Ⅰ in this comparative example is a mixture of 50g of acetylene black and activated carbon (the mass ratio of acetylene black to activated carbon is 2:1), that is, the waterproof, conductive and breathable layer in this comparative example does not contain carbon silver plating; and the thickness of the gas diffusion layer in the positive electrode plate in this comparative example is 0.25mm.
[0188] This comparative example also discloses an air battery, including the positive electrode plate in this comparative example.
[0189] Comparative Example 2
[0190] This comparative example discloses a positive electrode plate, which differs from Example 4 in that: in the preparation of the catalytic prefabricated layer in step (II) of this comparative example: the mixed carbon powder II used does not contain carbon silver plating: the total added amount of the mixed carbon powder II in this comparative example is the same as that in Example 4, and an equal amount of conductive carbon black is used in this comparative example to replace the carbon silver plating in Example 4, that is, the catalytic layer in this comparative example does not contain carbon silver plating.
[0191] This comparative example also discloses an air battery, including the positive electrode plate in this comparative example.
[0192] Test example
[0193] This test example tests the performance of the positive electrode sheets in the embodiments and comparative examples, specifically including:
[0194] The surface resistance tester was used to test the surface resistance of the positive electrode sheets in Examples 1-7 and Comparative Examples 1-2; the air permeability tester was used to test the air permeability of the positive electrode sheets in Examples 1-7 and Comparative Examples 1-2; the test results are detailed in Table 1:
[0195] Table 1
[0196] Experimental example Surface resistance at 1cm distance (Ω) <![CDATA[Air permeability (mL / cm 2 *min@7 kPa)]]> Example 1 70 20 Example 2 50 50 Example 3 20 100 Example 4 45 60 Example 5 58 69 Example 6 80 140 Example 7 20 130 Comparative Example 1 60 50 Comparative Example 2 85 48
[0197] In summary, in the waterproof conductive breathable layer of the positive electrode sheet of the present invention, by adding a specific type of conductive particles I, the conductive particles I have excellent conductivity, which significantly improves the resistance of the positive electrode sheet and significantly improves the current density of the air battery. Moreover, the conductive particles I in the present invention have the catalytic effect, and are also porous and have a large specific surface area. Therefore, they have an excellent effect of adsorbing oxygen, accelerate the entry of oxygen, thereby accelerating the formation of current and improving the energy density of the positive electrode sheet. In some embodiments of the present invention, by adding conductive particles I, the energy density of the waterproof conductive breathable layer in the present invention is increased by 10-15% compared to not adding conductive particles I, and the surface resistance is reduced by 10-50%.
[0198] In the catalytic layer of the positive electrode plate of the present invention, the conductive particles II have catalytic and conductive properties, and can cooperate with the catalyst (such as manganese dioxide) to improve the catalytic efficiency. In some embodiments of the present invention, the addition of conductive particles II can increase the energy density of the catalytic layer by 10-15%.
[0199] The waterproof, conductive, breathable layer and the catalytic layer have good chemical or electrochemical corrosion resistance because they contain fluorine materials, and the carbon material has excellent chemical resistance. In some embodiments of the present invention, the metal current collecting layer is added with electroplated precious metal materials to enhance its chemical resistance.
[0200] The preparation method of the positive electrode plate of the present invention has the advantages of simple process, easy operation, short production cycle, controllable film thickness, relatively conventional equipment, low preparation cost, etc. The prepared positive electrode plate has the characteristics of low resistance (volume resistance can be reduced by 30-40%), good air permeability and excellent waterproof performance. Among them, the pore-forming agent I is gasified and combined with pore-forming during high-temperature volatilization and dry sintering of ethanol to increase the air permeability: when anhydrous ethanol evaporates at high temperature, air gaps will appear due to the expansion of gas, and anhydrous ethanol is a liquid (metal compounds are difficult to dissolve in anhydrous ethanol), so the air gap will be very small. Similarly, the liquid pore-forming agent I in the present invention is the same, which has the advantages of easy dispersion, simplified steps (only sintering temperature is needed to gasify the liquid pore-forming agent), number of pores (double pores, larger air permeability, more oxygen entering), etc., which effectively improves the air permeability of the waterproof conductive air-permeable layer. The air permeability of the positive electrode plate in the present invention can reach 100mL / cm 2*min (@7kpa) or more. In addition, in the process of preparing the waterproof, conductive and breathable prefabricated layer, the initial film is first formed by rolling with an open mill, and then the semi-finished product is formed by applying pressure with a hydraulic press. The thickness control is precise and the process is simple. First, the waterproof, conductive and breathable prefabricated layer and the catalytic prefabricated layer are prepared, and then the current collector prefabricated layer (metal mesh) and the gas diffusion prefabricated layer (such as carbon paper) are stacked. After each layer is stacked, it is hydraulically sintered again, which shortens the process time and makes each layer more compact.
[0201] It should be noted that the “room temperature” in this article, unless otherwise specified, is 20-35° C.; the meaning of “about” for numerical values in this article is an error of ±12%.
[0202] The embodiments of the present invention are described in detail above in conjunction with the accompanying drawings, but the present invention is not limited to the above embodiments. Various changes can be made within the knowledge of ordinary technicians in the relevant technical field without departing from the purpose of the present invention. In addition, the embodiments of the present invention and the features in the embodiments can be combined with each other without conflict.
Claims
1. A positive electrode sheet, It is characterized in that It includes a waterproof, conductive and breathable layer, a current collector layer and a catalytic layer which are stacked. The waterproof, conductive and breathable layer includes a mixed material I. The mixed material I includes conductive particles I and a carbon material I. The conductive particles I include at least one of platinum, carbon-plated platinum, carbon-supported platinum, carbon-plated silver, carbon-plated nickel or carbon-plated gold.
2. The positive electrode sheet according to claim 1, It is characterized in that In the waterproof, conductive, breathable layer, the mass fraction of conductive particles I is 15-60%; and / or, the carbon material I includes at least one of conductive carbon black, acetylene black or activated carbon; and / or, the raw materials for preparing the waterproof, conductive, breathable layer include the raw materials of the binder I, the mixed material I and the pore-forming agent I; and / or, the thickness of the waterproof, conductive, breathable layer is 0.02-0.5 mm.
3. The positive electrode sheet according to claim 1, It is characterized in that The pore-forming agent I includes at least one of ammonium bicarbonate, polyethylene glycol, sodium chloride or polyvinyl alcohol.
4. The positive electrode sheet according to claim 1, It is characterized in that The catalytic layer includes a mixed material II, a catalyst and a binder II, and the mixed material II includes conductive particles II and a carbon material II.
5. The positive electrode sheet according to claim 4, It is characterized in that The conductive particles II include at least one of platinum, carbon-supported platinum, carbon-plated platinum, carbon-plated silver, carbon-plated nickel or carbon-plated gold; and / or the catalyst includes at least one of manganese dioxide, perovskite-type oxide catalyst, Pt or metal macrocyclic compound catalyst.
6. The positive electrode sheet according to claim 1, It is characterized in that A gas diffusion layer is provided between the waterproof conductive breathable layer and the current collector layer.
7. A method for preparing a positive electrode sheet, It is characterized in that The method comprises the following steps: stacking a waterproof conductive breathable prefabricated layer, a current collector prefabricated layer and a catalytic prefabricated layer, and pressing them together to form a stacked waterproof conductive breathable layer, a current collector layer and a catalytic layer to obtain the positive electrode sheet.
8. The method for preparing the positive electrode sheet according to claim 7, It is characterized in that The waterproof, conductive and breathable prefabricated layer, the gas diffusion prefabricated layer, the current collector prefabricated layer and the catalytic prefabricated layer are stacked and then pressed.
9. The method for preparing the positive electrode sheet according to claim 7, It is characterized in that The preparation method comprises preparing a waterproof, conductive and breathable prefabricated layer, and specifically comprises the following operations: Sa-1, mixing an alcohol solvent with mixed material I, adding pore former I, adding raw materials of binder I, stirring, separating, and obtaining coagulation material I; Sa-2, the condensate I is pressed for a second time and dried to obtain a waterproof, conductive and breathable prefabricated layer.
10. An air battery, It is characterized in that It includes the positive electrode sheet as described in any one of claims 1 to 6 or the positive electrode sheet made by the method as described in any one of claims 7 to 9.