High-stability CuMox Pt / C core-shell catalyst as well as synthesis method and application thereof
Patent Information
- Application Number
- CN202310529744.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-05-11
- Publication Date
- 2024-11-12
AI Technical Summary
但是此类元素常见于合金类催化剂的掺杂,在核壳结构中引入此类元素以增强自身稳定性的研究仍然较少
[0016] According to the carbon carrier platinum-based core-shell structure catalyst, preparation method and application provided by the present invention, cheap molybdenum-doped copper as the core highly stable CuMo is prepared by the above method. x @Pt/C core-shell catalyst. The catalyst obtained by this method includes a Mo-doped Cu core and an outer Pt shell. Therefore, the carbon-supported platinum-based core-shell structure catalyst is a three-way core-shell catalyst. The invention also provides a highly stable copper-molybdenum@platinum ternary core-shell (CuMo x @Pt/C) synthesis strategy.
Smart Images

Figure CN118943393A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of nanomaterials, and in particular to a core-shell structure, a preparation method thereof and an application thereof in fuel cell electrocatalytic oxygen reduction. Background Art
[0002] Proton exchange membrane fuel cells (PEMFCs) have attracted attention as an efficient and clean energy conversion device. However, the oxygen reduction reaction at the cathode requires the use of expensive platinum-carbon catalysts (Pt / C). The high cost and scarcity of Pt are key obstacles to the wider application of PEMFC. At the same time, existing commercial Pt / C catalysts still have problems such as insufficient activity and poor stability under high potential and long cycles. In view of the current status of Pt / C catalysts, it is an effective strategy to coat Pt on transition metals to form a core-shell. Thanks to the compressive strain caused by the difference in the lattices between the inner and outer layers, the utilization efficiency of the Pt outer layer is improved, and the intrinsic activity is also improved due to lattice compression. At the same time, the Pt outer shell can also provide certain protection for the relatively active metal in the inner layer.
[0003] At present, core-shell catalysts mostly use metals such as Pd and Ir as the core. Although these metal elements have good stability, they still belong to the category of precious metals. Their scarcity and high prices still make it difficult to solve the difficulties currently faced by platinum-based catalysts.
[0004] Although using cheap but active metals (such as Co, Cu, etc.) as kernels has more advantages in terms of cost, the active kernels are more easily dissolved in the long-term cycle process, resulting in the rapid decay of performance. CN109378484A invented a uniformly distributed Cu-Fe@Cu@Pt / C catalyst, which uses a cheap metal kernel and enhances the stability of the CuFe kernel catalyst based on the Cu subsurface protection strategy. However, the Fe element can induce the Fenton reaction to damage the fuel cell proton membrane, so its application in the long-term electrochemical cycle process is still limited. Using corrosion-resistant elements such as Mo and Au for doping can enhance catalyst stability, and it is also more friendly to the proton membrane. However, such elements are common in the doping of alloy catalysts, and the research on introducing such elements in the core-shell structure to enhance its own stability is still less. Summary of the invention
[0005] In view of this, the technical problem solved by the present invention is to provide a CuMo x@Pt / C core-shell catalyst and preparation method thereof, the method is simple to synthesize, the Pt shell has typical core-shell compression strain characteristics, and can effectively improve the intrinsic activity of Pt. More importantly, due to the effective Mo doping strategy, the Cu-Mo-Pt bridging effect produced significantly enhances the interaction between the core and shell, so that the stability of the catalyst is significantly improved. The catalyst provided by the present invention has good mass specific activity and stability, and shows good application potential in the field of fuel cells.
[0006] To achieve the above object, the technical solution adopted by the present invention is:
[0007] The present application provides a highly stable CuMo x @Pt / C core-shell catalyst, the catalyst CuMo x The core is a core, wherein x represents the doping ratio of Mo in the Cu core; the outer shell is Pt, which has obvious core-shell compression strain characteristics. The ratio of Mo:Cu in the core of the catalyst is 1:9-1:1; the grain size of the core-shell structure is 3-4nm; the thickness of the Pt shell is 0.5-2nm, and the total mass of Pt in the catalyst accounts for 15wt%.
[0008] The present application also provides a method for preparing the core-shell material, which has the following characteristics and comprises the following steps:
[0009] (1) Cu and Mo precursors are dissolved in ethylene glycol to obtain solution A, a capping agent and a reducing agent are dissolved in a solvent to obtain solution B, solutions A and B are mixed, and a carbon carrier is added for ultrasonic dispersion to obtain a precursor mixture. The capping agent is hexadecyltrimethylammonium bromide (CTAB), the reducing agent is ascorbic acid (AA), and the carbon carrier is XC-72.
[0010] (2) The mixed solution in (1) is heated in a reaction kettle to obtain a suspension after reaction; the heating temperature is 150-200°C and the reaction time is 6-12 hours. The reaction solution is centrifuged to obtain a solid product, which is washed to obtain CuMo x / C.
[0011] (3) The solid product is dispersed in ethylene glycol, and a Pt metal salt solution is gradually added dropwise at 80-110°C. After the addition is completed, the temperature is raised to 200°C and kept warm for 6 hours. The resulting reaction solution is centrifuged, washed and dried to obtain the highly stable CuMo x @Pt / C core-shell catalyst.
[0012] Furthermore, in step (1), the Mo precursor is (NH4)2MoO4·4H2O, and the Cu precursor is CuCl2·2H2O. The molar ratio of Cu to Mo precursor is 1:9-1:1.
[0013] Furthermore, the Pt salt in step (3) is H2PtCl6·6H2O, and the concentration of the prepared solution is 0.5-5 mg / mL.
[0014] The present invention also provides an application of the catalyst in an oxygen reduction reaction, characterized in that a unique Mo doping strategy significantly improves its long-term cycle stability.
[0015] Function and effect of the invention:
[0016] According to the carbon-supported platinum-based core-shell structure catalyst, preparation method and application provided by the present invention, a highly stable CuMo catalyst with inexpensive molybdenum-doped copper as the core is prepared by the above method. x The catalyst obtained by the method comprises a Mo-doped Cu core and an outer Pt shell, so the carbon-supported platinum-based core-shell catalyst is a ternary core-shell catalyst. The present invention also provides a highly stable copper-molybdenum-platinum ternary core-shell (CuMo) catalyst. x @Pt / C) synthesis strategy.
[0017] On the other hand, the catalyst has excellent durability and activity in acidic oxygen reduction reactions. Due to the effective Mo doping strategy, the resulting Cu-Mo-Pt bridging effect significantly enhances the interaction between the core and the shell, making it difficult for the core to dissolve during long cycles, thereby achieving maximum retention of activity. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] Figure 1 The CuMo provided in Example 1 and Comparative Example 1 of the present invention 0.2 X-ray diffraction (XRD) patterns of Cu@Pt / C, Cu@Pt / C and commercial Pt / C.
[0019] Figure 2 The CuMo provided in Example 1 of the present invention 0.2 High-resolution transmission electron microscopy (HRTEM) image of @Pt / C.
[0020] Figure 3 The CuMo provided in Example 1 of the present invention 0.2 @Pt / C particle size distribution diagram.
[0021] Figure 4 The CuMo provided in Example 1 of the present invention 0.2 @Pt / C element distribution line scan.
[0022] Figure 5 The CuMo provided in Example 1 and Comparative Example 1 of the present invention 0.2X-ray photoelectron spectroscopy (XPS) graphs of Pt4f@Pt / C, Cu@Pt / C and commercial Pt / C.
[0023] Figure 6 The CuMo prepared in Example 1 of the present invention 0.2 Linear polarization curves (LSV) of @Pt / C initially and after 50,000 cycles of stability testing.
[0024] Figure 7 LSV of the Cu@Pt / C prepared in comparative example 1 of the present invention at the initial stage and after 20,000 cycles of stability test.
[0025] Figure 8 The CuMo provided in Example 1 and Comparative Example 1 of the present invention 0.2 Mass activity histograms of initial and after stability testing for @Pt / C, Cu@Pt / C, and commercial Pt / C. DETAILED DESCRIPTION
[0026] In order to further understand the present invention, the preferred embodiments of the present invention are described below in conjunction with examples. Obviously, the described examples are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0027] The raw materials and reagents used in the embodiments of the present invention can be purchased from conventional biochemical reagent stores.
[0028] Example 1
[0029] A CuMo with high oxygen reduction activity and high durability 0.2 @Pt / C ternary core-shell catalyst. Take 26.8mgCuCl2·2H2O and 6.0mg(NH4)2MoO4·4H2O and dissolve them in 20mL ethylene glycol to obtain solution A. Take 120mg CTAB and 240mg AA and dissolve them in 20mL ethylene glycol to obtain solution B. Then mix solutions A and B, and add 74mg XC-72 carrier. After the mixture is treated with ultrasonic dispersion for 1 hour, it is transferred to a Teflon-lined reactor, heated at 170°C for 10 hours, and then cooled to room temperature. The resulting mixture is then magnetically stirred for 6h, then centrifuged and the solid is washed twice with ethanol, and finally dried under vacuum conditions to obtain CuMo 0.2 / C.
[0030] The CuMo synthesized in the above steps 0.2 / C was dispersed in 30 mL of ethylene glycol and heated to 105 °C in an oil bath under magnetic stirring. -119.5 mL of H2PtCl6·6H2O / ethylene glycol solution (2 mg mL -1 ), and then the temperature was raised to 200°C and maintained for 6 hours. After the reaction was completed, the obtained mixed solution was naturally cooled to room temperature, centrifuged to obtain a solid product, and then the obtained product was washed twice with ethanol and dried to obtain CuMo with high oxygen reduction activity and high durability. 0.2 @Pt / C ternary core-shell catalyst.
[0031] from Figure 1 It can be seen from the XRD patterns of each catalyst that CuMo 0.2 @Pt / C and Cu@Pt / C both have characteristic peaks corresponding to the (111), (200), (220) and (311) crystal planes of Pt, and both have a certain degree of positive shift compared to commercial Pt / C. 0.2 In @Pt / C, the diffraction peak corresponding to the Pt(111) crystal plane shifts from 39.8° to 40.9°, which means that the interplanar spacing is compressed from 0.227nm to 0.219nm. Figure 2 This is consistent with the HRTEM measurement in the figure. This lattice compression is helpful to improve the intrinsic activity of Pt. Figure 3 The particle size distribution of CuMo is calculated based on the HRTEM image. 0.2 The average particle size of @Pt / C is 3.2±0.2nm. Figure 4 The element line scan image proves that the Mo element is effectively incorporated into the core rather than appearing on the Pt surface. Figure 5 The difference in Pt binding energy between the presented catalyst and commercial Pt / C was compared, and the negative shift (about 0.5 eV) in the binding energy of the synthesized catalyst was attributed to the d-orbital electron enrichment caused by lattice compression.
[0032] Example 2
[0033] A CuMo with high oxygen reduction activity and high durability 0.1 @Pt / C ternary core-shell catalyst. Take 26.8mgCuCl2·2H2O and 3.0mg(NH4)2MoO4·4H2O and dissolve them in 20mL ethylene glycol to obtain solution A. Take 120mg CTAB and 240mg AA and dissolve them in 20mL ethylene glycol to obtain solution B. Then mix solutions A and B, and add 74mg XC-72 carrier. After the mixture is treated with ultrasonic dispersion for 1 hour, it is transferred to a Teflon-lined reactor, heated at 150°C for 6 hours, and then cooled to room temperature. The resulting mixture is then magnetically stirred for 6 hours, then centrifuged and the solid is washed twice with ethanol, and finally dried under vacuum conditions to obtain CuMo 0.1 / C.
[0034] The CuMo synthesized in the above steps 0.1 / C was dispersed in 30 mL of ethylene glycol and heated to 80 °C in an oil bath under magnetic stirring. -1 19.5 mL of H2PtCl6·6H2O / ethylene glycol solution (0.5 mg mL -1 ), and then the temperature was raised to 200°C and maintained for 6 hours. After the reaction was completed, the obtained mixed solution was naturally cooled to room temperature, centrifuged to obtain a solid product, and then the obtained product was washed twice with ethanol and dried to obtain CuMo with high oxygen reduction activity and high durability. 0.1 @Pt / C ternary core-shell catalyst.
[0035] Example 3
[0036] A CuMo with high oxygen reduction activity and high durability 0.5 @Pt / C ternary core-shell catalyst. Take 26.8mgCuCl2·2H2O and 15.0mg(NH4)2MoO4·4H2O and dissolve them in 20mL ethylene glycol to obtain solution A. Take 120mg CTAB and 240mg AA and dissolve them in 20mL ethylene glycol to obtain solution B. Then mix solutions A and B, and add 74mg XC-72 carrier. After the mixture is treated with ultrasonic dispersion for 1 hour, it is transferred to a Teflon-lined reactor, heated at 200°C for 12 hours, and then cooled to room temperature. The resulting mixture is then magnetically stirred for 6h, then centrifuged and the solid is washed twice with ethanol, and finally dried under vacuum conditions to obtain CuMo 0.5 / C.
[0037] The CuMo synthesized in the above steps 0.5 / C was dispersed in 30 mL of ethylene glycol and heated to 110 °C in an oil bath under magnetic stirring. -1 19.5 mL of H2PtCl6·6H2O / ethylene glycol solution (5 mg mL -1 ), and then the temperature was raised to 200°C and maintained for 6 hours. After the reaction was completed, the obtained mixed solution was naturally cooled to room temperature, centrifuged to obtain a solid product, and then the obtained product was washed twice with ethanol and dried to obtain CuMo with high oxygen reduction activity and high durability. 0.5 @Pt / C ternary core-shell catalyst.
[0038] Comparative Example 1:
[0039] A Cu@Pt / C ternary core-shell catalyst with high oxygen reduction activity. 26.8 mg CuCl2·2H2O was dissolved in 20 mL ethylene glycol to obtain solution A. 120 mg CTAB and 240 mg AA were dissolved in 20 mL ethylene glycol to obtain solution B. Solutions A and B were then mixed and 74 mg XC-72 carrier was added. The mixture was ultrasonically dispersed for 1 hour and then transferred to a Teflon-lined reactor, heated at 170°C for 10 hours, and then cooled to room temperature. The resulting mixture was magnetically stirred for 6 hours, then centrifuged and the solid was washed twice with ethanol, and finally dried under vacuum conditions to obtain Cu / C.
[0040] The Cu / C synthesized in the above steps was dispersed in 30 mL of ethylene glycol and heated to 105 °C in an oil bath under magnetic stirring. -1 19.5 mL of H2PtCl6·6H2O / ethylene glycol solution (2 mg mL -1 ), after the addition is completed, the temperature is raised to 200°C and maintained for 6 hours. After the reaction is completed, the obtained mixed solution is naturally cooled to room temperature, centrifuged to obtain a solid product, and then the obtained product is washed twice with ethanol and dried to obtain a Cu@Pt / C catalyst without Mo.
[0041] Test Example 1
[0042] The CuMo in Example 1 0.2 @Pt / C and Cu@Pt / C prepared in Comparative Example 1 were used as catalysts for electrochemical testing. Specifically, the electrochemical testing process of the catalyst ORR was as follows:
[0043] 1. Disperse 2 mg of catalyst in 700 μL of deionized water, 280 μL of ethanol and 20 μL of 5%
[0044] The Nafion solution was ultrasonicated for 1 h to obtain catalyst ink.
[0045] 2. Take 10 μL of ink and drop it on a rotating disk electrode with a diameter of 5 mm and spin dry it at a speed of 500 rpm.
[0046] 3. CV test was carried out in N2-saturated 0.1M HClO4, with a CV range of 0V to 1.2V (vs RHE) and a scan rate of 50mVs -1 .
[0047] 4.LSV test is carried out in 0.1M HClO4 saturated with O2, and the LSV range is 0.1V~1.1V
[0048] (vs RHE), scan rate 10 mV s -1 .
[0049] 5. The stability test was carried out in N2-saturated 0.1 M HClO4, with a CV range of 0.6 V to 0.95 V (vs RHE) and a scan rate of 200 mV s -1 .
[0050] Figure 6 The CuMo prepared in Example 1 of the present invention 0.2 LSV of initial and after 50,000 cycles of stability of @Pt / C. The results show that CuMo 0.2 @The half-wave potential of Pt / C only dropped by 7mV.
[0051] Figure 7 The initial and 20,000 cycles of stability LSV of Cu@Pt / C prepared in Comparative Example 1 of the present invention show that the half-wave potential of Cu@Pt / C decreases by 12 mV before and after the stability test. Figure 8 The mass activity loss bar graph of each catalyst and commercial Pt / C after the stability test. After 50,000 cycles, CuMo 0.2 The performance of Cu@Pt / C is only 8.7% attenuated, while after 20,000 cycles, the performance of Cu@Pt / C is 23.3% attenuated. The above figure shows that due to the effective Mo doping strategy, the Cu-Mo-Pt bridging effect significantly enhances the interaction between the core and shell, thus making CuMo 0.2 The inner core of the @Pt / C catalyst is difficult to dissolve during long cycles, achieving maximum retention of activity.
[0052] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.
Claims
1. A CuMo x @Pt / C core-shell catalyst, characterized in that CuMo x is the core, where x represents the doping ratio of Mo in the Cu core; the outer shell is Pt, which has obvious core-shell compressive strain characteristics.
2. The core-shell catalyst according to claim 1, characterized in that The doping ratio of Mo:Cu in the core is 1:9-1:1; the grain size of the core-shell structure is 3-4nm; and the thickness of the Pt shell is 0.5-2nm.
3. The method for preparing the core-shell composite material according to claim 1, characterized in that: The following steps are involved: (1) dissolving Cu and Mo precursors in ethylene glycol to obtain solution A, dissolving a capping agent and a reducing agent in a solvent to obtain solution B, mixing solutions A and B, and adding a carbon carrier for ultrasonic dispersion to obtain a precursor mixture. The capping agent is hexadecyltrimethylammonium bromide (CTAB), the reducing agent is ascorbic acid (AA), and the carbon carrier is XC-72; (2) heating the mixed solution in (1) in a reaction kettle to obtain a suspension after reaction; the heating temperature is 150-200° C., and the reaction time is 6-12 h; centrifuging the reaction solution to obtain a solid product, and washing to obtain CuMo x / C; (3) dispersing the solid product in ethylene glycol, gradually adding a Pt metal salt solution at 80-110° C., heating to 200° C. and keeping the temperature for 6 h after the addition is completed; centrifuging the resulting reaction solution, washing and drying to obtain the highly stable CuMo x @Pt / C core-shell catalyst.
4. CuMo according to claim 3 x / C preparation method, characterized in that, The commercial carbon black described in step (1) is XC-72; the Cu precursor is cupric chloride dihydrate; the Mo precursor is ammonium molybdate; the molar ratio of Cu and Mo precursors is 1:9-1:1; the heating temperature is 150-200°C, and the reaction time is 6-12h; the capping agent is hexadecyltrimethylammonium bromide (CTAB), the reducing agent is ascorbic acid (AA), and the carbon carrier is XC-72.
5. CuMo according to claim 3 x @Pt / C preparation method, characterized in that, In step (3), the Pt metal salt is chloroplatinic acid; the mass concentration of the Pt salt solution is 0.5-5 mg / mL; and the reduction temperature is 80-110°C.
6. The method according to claim 3, characterized in that: The centrifugation, washing and drying methods described in claim 3 are all conventional laboratory methods, and the washing liquid is water or ethanol.
7. The highly stable CuMo x @Pt / C core-shell catalyst, characterized in that The CuMo x @Pt / C core-shell catalyst is prepared based on any one of the routes described in claims 4-7.
8. The highly stable CuMo according to any one of claims 1 to 2 x @Pt / C core-shell catalysts are used in oxygen reduction reaction (ORR).
Citation Information
Patent Citations
Method for preparing carbon-supported core-shell compact copper iron-copper-platinum catalyst for fuel cell
CN109378484A