Battery electrolyte and preparation method and application thereof

By using electrolytes of lithium salt, ether and sulfone solvents in lithium-ion batteries, combined with appropriate additives, the problem of stable circulation and fast charging of lithium manganese iron phosphate batteries at high voltages is solved, and efficient battery performance is achieved promote.

CN118943483APending Publication Date: 2024-11-12SHANGHAI XUANYI NEW ENERGY DEV CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411213612.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing lithium-ion battery electrolyte is difficult to achieve fast charging and long-term stable circulation of lithium manganese iron phosphate batteries under high voltage platforms, and the manganese precipitation problems caused by the Jahn-Teller effect affect the rate performance and cycle stability of the battery.

Method used

Using battery electrolyte containing lithium salt, ether solvent and sulfone solvent, through reasonable proportions and additives, a protective barrier is formed and ionic conductivity is improved, the viscosity of the electrolyte is reduced, the electrochemical window is enhanced, and the battery circulation is improved. Stability and charging performance.

Benefits of technology

It realizes stable operation and fast charging of lithium-ion batteries under high voltage, improves the cycle stability and charging rate of the battery, with a capacity retention rate greater than 80%, and a charging rate of ≥3C.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005020885970000021
    Figure BDA0005020885970000021
  • Figure BDA0005020885970000041
    Figure BDA0005020885970000041
  • Figure BDA0005020885970000101
    Figure BDA0005020885970000101
Patent Text Reader

Abstract

The invention provides a battery electrolyte and a preparation method and application thereof. The battery electrolyte comprises a lithium salt, an ether solvent, a sulfone solvent and an additive. The type of a solvent in the battery electrolyte is one of important factors influencing the charging performance and the cycle performance of the battery, and a sulfone solvent is used in the battery electrolyte, so that a protective barrier can be formed on an electrolyte interface, and the cycle stability of a battery cell is improved; the ether solvent and the sulfone solvent are cooperatively used in the battery electrolyte, so that on one hand, the viscosity of the battery electrolyte can be reduced, and on the other hand, the ether solvent and the sulfone solvent can jointly have a synergistic effect with the lithium salt and the additive in the electrolyte; through the cooperation of the two functions, the purposes of improving the ionic conductivity and the electrochemical window of the battery electrolyte and improving the cycling stability of the battery cell are achieved, so that the obtained battery not only can achieve the effect of rapid charging, but also can stably operate under a high-voltage platform.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a battery electrolyte and a preparation method and application thereof. Background Art

[0002] With the rapid development of power batteries and electrochemical energy storage, lithium-ion batteries are increasingly used in scalable energy storage devices, especially as a power source for new energy electric vehicles. However, with the rapid development of new energy vehicles, the performance requirements for lithium-ion batteries are gradually increasing, especially seeking lithium-ion batteries with higher energy density, high fast charging capability, high stability, and low-cost systems is the mainstream direction of lithium battery development. In order to meet the requirements of lithium battery development, the research on a new generation of positive electrode materials, lithium manganese iron phosphate (LMFP), has made rapid progress. However, the positive electrode material of lithium manganese iron phosphate batteries has a dual voltage platform, and the manganese precipitation problem caused by the Jahn-Teller effect is still very prominent, affecting the rate performance and cycle stability of the battery cell. At present, by adding a small amount of additives to mature commercial electrolytes, the interface in the battery can be regulated, thereby improving the rate performance and cycle stability of the battery. This method is considered to be an effective method that can be applied on a large scale.

[0003] Among the positive electrode materials of batteries, the voltage platform of lithium iron phosphate (LFP) is 3.4V, while the voltage of lithium manganese iron phosphate (LMFP) with a dual voltage platform can reach 4.1V. In theory, the energy density of LMFP can be increased by more than 20% compared with the former, but the existing commercial electrolytes are difficult to ensure the long-term, rapid and stable circulation of the battery cell under the high voltage of 4.1V. On the other hand, during the charging and discharging process of the battery cell, the manganese precipitation problem caused by the Jahn-Teller effect will cause the loss of electrode active materials, thereby affecting the circulation and fast charging performance of the battery cell. This problem cannot be solved in the electrolyte of the traditional ternary or lithium iron phosphate positive electrode system. In short, due to the particularity of the positive electrode material of lithium manganese iron phosphate battery, there is no ideal practical electrolyte that can realize the stable circulation of lithium-ion batteries at higher rates. In order to solve the above problems, it is also necessary to develop electrolytes suitable for lithium manganese iron phosphate from multiple dimensions such as solvents, lithium salts, and additives.

[0004] An easily overlooked but critical problem in high-voltage lithium-ion battery failure is the embedding of anions into the cathode conductive carbon. Patent CN107959050A discloses a sulfone-based electrolyte for lithium-ion batteries, which clearly states that sulfone solvents can improve the cycle stability of the battery cell by forming a protective barrier at the interface. For example, sulfolane (SL) can prevent the embedding of anions through two mechanisms: (1) through its strong anion-Li +Interaction to provide a high insertion activation barrier; (2) by forming a sulfur-containing, anion-enclosed SL-derived intermediate phase. Under the combined action of these two mechanisms, the LMFP / NCM graphite full battery (cut-off voltage = 5.2V) can operate stably. However, in the method disclosed in the invention, the proportion of sulfone solvents is very high, exceeding 30%, which will cause the overall viscosity of the electrolyte to be too high and cannot meet the requirements of high ionic conductivity and fast charging performance.

[0005] In summary, a suitable battery electrolyte has not yet been found that can both meet the requirements of stable operation under a high voltage platform and achieve fast charging, so as to achieve fast charging of lithium batteries with lithium iron manganese phosphate as the main active substance of the positive electrode material and long-term stable circulation at a higher voltage. Summary of the invention

[0006] The main purpose of the present invention is to provide a battery electrolyte and a preparation method and application thereof, so as to solve the problem that the positive electrode material of lithium manganese iron phosphate battery in the prior art cannot achieve the lithium ion battery both to achieve the effect of fast charging and to operate stably under a high voltage platform when applied to the lithium ion battery.

[0007] In order to achieve the above object, the present invention provides a battery electrolyte, which includes: a lithium salt, an ether solvent, a sulfone solvent and an additive.

[0008] Furthermore, the sulfone solvent is selected from one or more compounds having the structure shown in the following formula (I): wherein R1 and R2 are each independently selected from H, C1-C20 alkyl, C3-C20 cycloalkyl, C6-C30 substituted or unsubstituted aryl, C6-C30 aralkyl, or C1-C6 straight-chain alkyl in which at least part of the hydrogen is replaced by halogen; or, R1, R2 and the S atom to which they are bonded together form a four- to eight-membered ring; preferably, R1 and R2 are each independently selected from H, C1-C5 alkyl, C3-C6 cycloalkyl, C6-C12 aryl, C6-C14 aralkyl, or C1-C3 straight-chain alkyl in which at least part of the hydrogen is replaced by halogen; Alternatively, R1, R2 and the S atom to which they are bonded together form a four- to five-membered ring; more preferably, the C1-C5 alkyl group is methyl, ethyl or propyl, the C3-C6 cycloalkyl group is cyclopropyl, cyclobutyl or cyclopentyl, the C6-C30 substituted or unsubstituted aryl group is phenyl, methylphenyl, ethylphenyl or biphenyl, and the C1-C6 straight-chain alkyl group in which at least part of the hydrogen is substituted by halogen is chloromethyl, dichloromethyl, bromomethyl, dibromomethyl, chloroethyl, dichloroethyl, fluoromethyl, difluoromethyl or difluoroethyl; further preferably, the sulfone solvent is sulfolane and / or 3-methylsulfolane.

[0009] Furthermore, the ether solvent is one or more of tetrahydrofuran, 2-methyltetrahydrofuran, dimethoxymethane, 1,2-dimethoxyethane, and diethylene glycol dimethyl ether.

[0010] Further, the lithium salt is one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium trifluoromethylsulfonate, lithium hexafluoroarsenate, perfluoroalkylsulfonylmethyl lithium and lithium bis(trifluoromethylsulfonyl)imide; preferably, the concentration of the lithium salt in the battery electrolyte is 1 to 2 mol / L; further preferably, the concentration of the lithium salt in the battery electrolyte is 1.5 to 2 mol / L.

[0011] Furthermore, the weight ratio of the sulfone solvent to the ether solvent in the battery electrolyte is (5-30):(70-95); preferably, the weight ratio of the sulfone solvent to the ether solvent is (10-20):(85-90).

[0012] Further, the additive is one or more of fluoroethylene carbonate, vinylene carbonate, tripropargyl phosphate, tri(trimethylsilane)phosphite, vinyl sulfate, methylene disulfonate, lithium bis(oxalatoborate), succinonitrile and adiponitrile; preferably, the additive is at least two of fluoroethylene carbonate, vinylene carbonate, tripropargyl phosphate, tri(trimethylsilane)phosphite, vinyl sulfate, methylene disulfonate, lithium bis(oxalatoborate), succinonitrile and adiponitrile; preferably, the additive is added in an amount of 1.5 to 3.5% of the total weight of the battery electrolyte; further preferably, the additive is added in an amount of 1.5 to 2.5% of the total weight of the battery electrolyte.

[0013] Further, the lithium salt is lithium hexafluorophosphate, the ether solvent is tetrahydrofuran, the sulfone solvent is sulfolane, and the additives are lithium bis(oxalatoborate) and vinyl sulfate, wherein the concentration of lithium hexafluorophosphate is 1.5-2 mol / L, the mass ratio of sulfolane to tetrahydrofuran is (10-15):(85-90), the addition amount of lithium bis(oxalatoborate) and vinyl sulfate is 1.5-2.5%, and the mass ratio of lithium bis(oxalatoborate) and vinyl sulfate is 1:(2-4); or, the lithium salt is lithium bis(fluorosulfonyl)imide, the ether solvent is tetrahydrofuran, the sulfone solvent is sulfolane, and the additives are lithium bis(oxalatoborate) and vinyl carbonate, wherein the concentration of lithium hexafluorophosphate is 1.5-2 mol / L, the mass ratio of sulfolane to tetrahydrofuran is (10-15):(85-90), the addition amount of lithium bis(oxalatoborate) and vinyl sulfate is 1.5-2.5%, and the mass ratio of lithium bis(oxalatoborate) and vinyl sulfate is 1:(2-4). The concentration of lithium imide is 2 mol / L, the mass ratio of sulfolane and tetrahydrofuran is (10-15):90, the amount of lithium bisoxalatoborate and vinyl sulfate added is 1.5%, and the mass ratio of lithium bisoxalatoborate and vinyl sulfate is 1:2; or, the lithium salt is lithium hexafluorophosphate, the ether solvent is tetrahydrofuran, the sulfone solvent is sulfolane, and the additives are lithium bisoxalatoborate and vinyl sulfate, wherein the concentration of lithium hexafluorophosphate is 2 mol / L, the mass ratio of sulfolane and tetrahydrofuran is 15:85, the amount of lithium bisoxalatoborate and vinyl sulfate added is 1.5%, and the mass ratio of lithium bisoxalatoborate and vinyl sulfate is 1:2.

[0014] According to another aspect of the present invention, a method for preparing the above-mentioned battery electrolyte is provided, and the method for preparing the battery electrolyte comprises the following steps: S1, mixing a sulfone solvent and an ether solvent, removing impurities and water, and obtaining a mixed solvent; S2, adding a lithium salt to the mixed solvent to obtain a premixed solution; S3, adding an additive to the premixed solution to obtain a battery electrolyte.

[0015] Furthermore, the above impurity removal and water removal process is obtained by filtering the mixed solvent through an impurity removal and water removal agent, wherein the impurity removal and water removal agent is one or more of molecular sieve, activated carbon, calcium hydride, lithium hydride, anhydrous calcium oxide, calcium chloride, phosphorus pentoxide, alkali metal or alkaline earth metal; preferably, the molecular sieve is at least one of type 3A molecular sieve, type 4A molecular sieve and type 5A molecular sieve; preferably, the molecular sieve is type 4A molecular sieve and / or type 5A molecular sieve.

[0016] According to another aspect of the present invention, a lithium-ion battery is also provided, which includes the above-mentioned battery electrolyte and a battery positive electrode with lithium iron manganese phosphate material as an active material. Preferably, the lithium-ion battery has a capacity retention rate of greater than 80% after 1,000 charge and discharge cycles at a lower limit voltage of 2.75 to 2.90 V and an upper limit voltage of 4.30 to 4.80 V, and its charging rate is ≥3C.

[0017] The present invention provides a battery electrolyte, which includes: lithium salt, ether solvent, sulfone solvent and additive. The type of solvent in the battery electrolyte is one of the important factors affecting the charging performance and cycle performance of the battery. The use of sulfone solvents in the battery electrolyte can improve the cycle stability of the battery cell by forming a protective barrier at the electrolyte interface; and the use of ether solvents and sulfone solvents in the battery electrolyte can reduce the viscosity of the battery electrolyte on the one hand, and on the other hand, the two can work together with lithium salt and additives in the electrolyte. The cooperation of the two aspects achieves the purpose of improving the ionic conductivity and electrochemical window of the battery electrolyte and improving the cycle stability of the battery cell, so that the obtained battery can achieve both the effect of fast charging and stable operation under a high voltage platform. DETAILED DESCRIPTION

[0018] It should be noted that, in the absence of conflict, the embodiments and features in the embodiments of the present application can be combined with each other. The present invention will be described in detail below in conjunction with the embodiments.

[0019] As described in the background technology section, the positive electrode material of lithium iron manganese phosphate batteries has a dual voltage platform, and its voltage can be as high as 4.1V. The existing commercial electrolytes are difficult to ensure the long-term, rapid and stable circulation of the battery cells under the high voltage of 4.1V; coupled with the manganese precipitation problem caused by the Jahn-Teller effect in the battery cells during charging and discharging, it will cause the loss of electrode active materials, which will in turn affect the cycle and fast charging performance of the battery cells. In order to effectively solve the problems of lithium iron manganese phosphate battery positive electrode materials when applied to lithium-ion batteries, so that lithium iron manganese phosphate batteries can achieve both fast charging and stable operation under high voltage platforms, it is necessary to develop electrolytes suitable for lithium iron manganese phosphate in a targeted manner from multiple dimensions such as solvents, lithium salts, and additives.

[0020] In order to solve the above problems, the present invention proposes a battery electrolyte, which includes: lithium salt, ether solvent, sulfone solvent and additive. The battery electrolyte uses a mixture of two solvents, ether solvent and sulfone solvent, as the solvent of the battery electrolyte, and then adds lithium salt and additive, and the several types of substances cooperate to make the obtained battery electrolyte show excellent performance when it acts together with the positive electrode material of lithium manganese iron phosphate battery in lithium ion battery.

[0021] In particular, the battery electrolyte of the present invention uses a mixture of ether solvents and sulfone solvents as the solvent of the battery electrolyte. Sulfone solvents as battery electrolyte solvents not only have high conductivity and high electrochemical window, but also have good solubility and low volatility. The present invention uses sulfone solvents as one of the solvents of the battery electrolyte, which can effectively promote the migration and transmission of ions in the electrolyte in the electrolyte solution, and can also enable the electrolyte to withstand a higher potential range without electrolyte decomposition, thereby facilitating the battery electrolyte to achieve long-term, rapid and stable recycling of the battery cell at a higher voltage. Further, the present invention uses ether solvents as another solvent of the battery electrolyte. Ether solvents also have high conductivity and good thermal stability. In addition, ether solvents also have low viscosity characteristics. The present invention uses ether solvents in combination with sulfone solvents. On the one hand, the viscosity of the battery electrolyte can be reduced as a whole; on the other hand, the energy loss of the electrolyte in the battery cell during ion transmission can be further reduced, the battery life can be extended, and the battery has a higher output power and better charging performance. At the same time, the electrochemical window of the battery electrolyte can also be improved.

[0022] In summary, when the present invention uses a mixture of ether solvents and sulfone solvents as the solvent of the battery electrolyte and applies it to the battery, the two solvents work synergistically in multiple aspects, improving the conductivity of the electrolyte and the electrochemical window of the electrolyte while also improving the cycle stability of the battery, thereby improving the comprehensive performance of the electrolyte when applied to the battery. Applying the above-mentioned battery electrolyte to the battery can not only realize the stable operation of the battery under the high voltage platform, but also enable the battery to achieve the effect of fast charging.

[0023] In a preferred embodiment, the sulfone solvent is selected from one or more compounds having the structure shown in the following formula (I): Wherein, R1 and R2 are independently selected from H, C1-C20 alkyl, C3-C20 cycloalkyl, C6-C30 substituted or unsubstituted aryl, C6-C30 aralkyl or C1-C6 straight chain alkyl with at least part of hydrogen substituted by halogen; or, R1, R2 and the S atom to which they are bonded together form a four- to eight-membered ring. Sulfone solvents have the advantages of good electrical conductivity, high electrochemical window, good solubility and low volatility. Selecting the above sulfone solvents as the solvent of the battery electrolyte can better play the above advantages.

[0024] Preferably, R1 and R2 are each independently selected from H, C1-C5 alkyl, C3-C6 cycloalkyl, C6-C12 aryl, C6-C14 aralkyl or C1-C3 straight-chain alkyl in which at least part of the hydrogen is replaced by halogen; or, R1, R2 and the S atom to which the two are bonded together form a four- to five-membered ring. Sulfone solvents under the above range conditions have better use effects. More preferably, the C1-C5 alkyl is methyl, ethyl or propyl, the C3-C6 cycloalkyl is cyclopropyl, cyclobutyl or cyclopentyl, the C6-C30 substituted or unsubstituted aryl is phenyl, methylphenyl, ethylphenyl or biphenyl, and the C1-C6 straight-chain alkyl in which at least part of the hydrogen is replaced by halogen is chloromethyl, dichloromethyl, bromomethyl, dibromomethyl, chloroethyl, dichloroethyl, fluoromethyl, difluoromethyl or difluoroethyl. Selecting the above specific sulfone solvent types, the battery exhibits better comprehensive performance in actual application. More preferably, the sulfone solvent is sulfolane and / or 3-methylsulfolane. Selecting sulfolane and / or 3-methylsulfolane for application in the battery electrolyte has better performance in the corresponding battery.

[0025] In a preferred embodiment, the ether solvent is one or more of tetrahydrofuran, 2-methyltetrahydrofuran, dimethoxymethane, 1,2-dimethoxyethane, and diethylene glycol dimethyl ether. Ether solvents have not only high electrical conductivity and good thermal stability, but also low viscosity and other characteristics. When the above specific types of ether solvents are selected for use in battery electrolytes, when the electrolyte is actually used in batteries, the battery exhibits a better fast charging effect and better operation under a high voltage platform.

[0026] In a preferred embodiment, the lithium salt in the battery electrolyte is one or more of lithium hexafluorophosphate (LiPF6), lithium bis(fluorosulfonyl)imide (LiFSI), lithium tetrafluoroborate (LiBF4), lithium difluorooxalatoborate (LiDFOB), lithium trifluoromethylsulfonate (LiSO3CF3), lithium hexafluoroarsenate (LiAsF6), perfluoroalkylsulfonylmethyl lithium (LiC(CF3SO2)3) and lithium bis(trifluoromethylsulfonyl)imide (Li(CF3SO2)2N). The lithium salt in the battery electrolyte plays an important role in the battery. The selection of the above-mentioned types of lithium salts in combination with ether solvents and sulfone solvents for use in the battery electrolyte is more conducive to the transmission of ions in the electrolyte and further improves the transmission efficiency of the battery. Preferably, the concentration of the lithium salt in the battery electrolyte is 1 to 2 mol / L. Controlling the concentration of the lithium salt in the battery electrolyte within the above range can take into account the comprehensive performance of the electrolyte such as power density, energy density, stability and safety, so that its performance in all aspects is in a more beneficial range. Further preferably, the concentration of the lithium salt in the battery electrolyte is 1.5-2 mol / L. The effect is better when the concentration of the lithium salt in the electrolyte is controlled within the above more preferred range. When the two lithium salts are compounded for use, any compounding ratio is acceptable, and preferably the weight ratio of the two is 1:(1-2).

[0027] In a preferred embodiment, the weight ratio of sulfone solvents and ether solvents in the battery electrolyte is (5-30): (70-95). The present invention adds sulfone solvents and ether solvents to the battery electrolyte. The mixed use of the two solvents can make them work together, thereby achieving an improvement in the comprehensive performance of the electrolyte. Controlling the weight ratio of sulfone solvents and ether solvents in the electrolyte within the above range can better exert the synergistic effect of sulfone solvents and ether solvents, improve the rapid charging effect of the battery, and improve the operation of the battery under a high voltage platform. Preferably, the weight ratio of sulfone solvents and ether solvents is controlled to be (10-20): (85-90), and the addition amount of sulfone solvents and ether solvents is controlled within the above range. When the battery electrolyte is used in a battery, the effect shown is better.

[0028] In a preferred embodiment, the additive is one or more of fluoroethylene carbonate (FEC), vinylene carbonate (VC), tripropargyl phosphate (TPP), tris(trimethylsilyl) phosphite (TMSP), vinyl sulfate (DTD), methylene disulfonate (MMDS), lithium bis(oxalate borate) (LiBOB), succinonitrile (SN) and adiponitrile (AND). The addition in the battery electrolyte can affect the electrochemical properties of the electrolyte system, and then affect the discharge conditions of the ions. The application of the above specific types of additives in the battery electrolyte is more conducive to improving the comprehensive performance of the battery electrolyte. When the above additives are used, one or more of them can be used in combination. Preferably, the additive is at least two of fluoroethylene carbonate, vinylene carbonate, tripropargyl phosphate, tris(trimethylsilyl) phosphite, vinyl sulfate, methylene disulfonate, lithium bis(oxalate borate), succinonitrile and adiponitrile. The above additives are used in combination, and the battery electrolyte has a better use effect. Preferably, the amount of the additive added is 1.5-3.5% of the total weight of the battery electrolyte. By controlling the amount of the additive added within the above range, the obtained battery electrolyte can show good performance when applied to the battery. Further preferably, the amount of the additive added is 1.5-2.5% of the total weight of the battery electrolyte. By controlling the amount of the additive added within the above more preferred range, the overall effect of the obtained electrolyte is better. When the two additives are compounded for use, any compounding ratio is acceptable, and preferably the weight ratio of the two additives is 1:(2-4).

[0029] In a preferred embodiment, the lithium salt is lithium hexafluorophosphate, the ether solvent is tetrahydrofuran, the sulfone solvent is sulfolane, and the additives are lithium bis(oxalatoborate) and vinyl sulfate, wherein the concentration of lithium hexafluorophosphate is 1.5-2 mol / L, the mass ratio of sulfolane to tetrahydrofuran is (10-15):(85-90), the addition amount of lithium bis(oxalatoborate) and vinyl sulfate is 1.5-2.5%, and the mass ratio of lithium bis(oxalatoborate) and vinyl sulfate is 1:(2-4); or, the lithium salt is lithium bis(fluorosulfonyl)imide, the ether solvent is tetrahydrofuran, the sulfone solvent is sulfolane, and the additives are lithium bis(oxalatoborate) and vinyl carbonate, wherein, The concentration of lithium bis(fluorosulfonyl)imide is 2 mol / L, the mass ratio of sulfolane and tetrahydrofuran is (10-15):90, the amount of lithium bis(oxalate borate) and vinyl sulfate added is 1.5%, and the mass ratio of lithium bis(oxalate borate) and vinyl sulfate is 1:2; or, the lithium salt is lithium hexafluorophosphate, the ether solvent is tetrahydrofuran, the sulfone solvent is sulfolane, and the additives are lithium bis(oxalate borate) and vinyl sulfate, wherein the concentration of lithium hexafluorophosphate is 2 mol / L, the mass ratio of sulfolane and tetrahydrofuran is 15:85, the amount of lithium bis(oxalate borate) and vinyl sulfate added is 1.5%, and the mass ratio of lithium bis(oxalate borate) and vinyl sulfate is 1:2. The above range of conditions is a more preferred condition range obtained by the inventor of the present invention after a large number of experiments, and the battery electrolyte obtained under the above range of conditions has a better effect when applied to batteries.

[0030] According to another aspect of the present invention, a method for preparing a battery electrolyte is also provided, and the preparation method comprises the following steps: S1, mixing a sulfone solvent and an ether solvent, removing impurities and water, and obtaining a mixed solvent; S2, adding a lithium salt to the mixed solvent to obtain a premixed solution; S3, adding an additive to the premixed solution to obtain a battery electrolyte.

[0031] Specifically, the preparation method first mixes a sulfone solvent and an ether solvent to remove impurities and water, then adds lithium salt to the mixed solvent to obtain a premixed solution, and finally adds an additive to the premixed solution to obtain a battery electrolyte. The preparation method can remove water and some trace amounts of anions such as S-containing anions, OH - Impurities such as these are processed to reduce their impact on the performance of the electrolyte. Step-by-step mixing will also make the electrolyte mix more evenly, further improving the stability of the battery electrolyte.

[0032] In a preferred embodiment, the impurity removal and water removal process is obtained by filtering the mixed solvent through an impurity removal and water removal agent, wherein the impurity removal and water removal agent is one or more of molecular sieve, activated carbon, calcium hydride, lithium hydride, anhydrous calcium oxide, calcium chloride, phosphorus pentoxide, alkali metal or alkaline earth metal; preferably, the molecular sieve is at least one of a 3A type molecular sieve, a 4A type molecular sieve and a 5A type molecular sieve; preferably, the molecular sieve is a 4A type molecular sieve and / or a 5A type molecular sieve. The above impurity removal and water removal operation can remove a small amount of water and trace impurities contained in the solvent, reducing the influence of water and impurities on the electrolyte. Using the above substances, the purpose of water removal and impurity removal can be achieved.

[0033] According to another aspect of the present invention, a lithium ion battery is provided, the lithium ion battery comprising the above-mentioned battery electrolyte and a battery positive electrode with lithium manganese iron phosphate material as an active material, preferably the lithium ion battery can be charged and discharged 1000 times at a lower limit voltage of 2.75 to 2.90V and an upper limit voltage of 4.30 to 4.80V with a capacity retention rate greater than 80%, and its charging rate is ≥3C. The battery electrolyte provided by the present invention is used together with the battery positive electrode with lithium manganese iron phosphate material as an active material, so that the obtained lithium ion battery can operate at a higher voltage with an upper limit voltage of 4.3 to 4.8V, and the charging rate can also be improved to more than 3C, with good charge and discharge performance.

[0034] The present application is further described in detail below in conjunction with specific embodiments. These embodiments should not be construed as limiting the scope of protection claimed in the present application.

[0035] Example 1

[0036] Battery electrolyte includes the following components:

[0037] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6]]> DTD, LiBOB

[0038] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 10:90, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 1.0 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0039] Example 2

[0040] Battery electrolyte includes the following components:

[0041] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6]]> DTD, LiBOB

[0042] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 10:90, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 1.5 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0043] Example 3

[0044] Battery electrolyte includes the following components:

[0045] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6]]> DTD, LiBOB

[0046] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 10:90, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0047] Example 4

[0048] Battery electrolyte includes the following components:

[0049] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6]]> DTD, LiBOB

[0050] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0051] Example 5

[0052] The difference from Example 2 is that the added amount of lithium bis(oxalatoborate) and the vinyl sulfate is 2.5%.

[0053] Battery electrolyte includes the following components:

[0054] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6]]> DTD, LiBOB

[0055] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 1.5 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 0.5% of the total weight of the battery electrolyte, and the amount of LiBOB added is 2.0% of the total weight of the battery electrolyte.

[0056] Example 6

[0057] The difference from Example 4 is that the lithium salt is lithium bis(fluorosulfonyl)imide (LiFSI), and the ether solvent and the sulfone are mixed in a weight ratio of 10:90.

[0058] Battery electrolyte includes the following components:

[0059] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran LiFSI DTD, LiBOB

[0060] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 10:90, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 5A molecular sieve, anhydrous calcium oxide and calcium chloride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0061] Example 7

[0062] The difference from Example 7 is that the ether solvent and the sulfone are mixed in a weight ratio of 15:90.

[0063] Battery electrolyte includes the following components:

[0064] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran LiFSI DTD, LiBOB

[0065] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:90, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 5A molecular sieve, anhydrous calcium oxide and calcium chloride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0066] Example 8

[0067] The difference from Example 4 is that the weight ratio of the sulfone solvent to the ether solvent is 20:85.

[0068] Battery electrolyte includes the following components:

[0069] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6]]> DTD, LiBOB

[0070] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 20:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0071] Example 9

[0072] The difference from Example 4 is that the weight ratio of the sulfone solvent to the ether solvent is 5:95.

[0073] Battery electrolyte includes the following components:

[0074] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6]]> DTD, LiBOB

[0075] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 5:95, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0076] Example 10

[0077] The difference from Example 4 is that the weight ratio of the sulfone solvent to the ether solvent is 30:70.

[0078] Battery electrolyte includes the following components:

[0079] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6]]> DTD, LiBOB

[0080] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 30:70, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0081] Embodiment 11

[0082] The difference from Example 4 is that the lithium salt is a composite of lithium hexafluorophosphate and lithium tetrafluoroborate in a mass ratio of 1:1.

[0083] Battery electrolyte includes the following components:

[0084] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6 and LiBF4]]> DTD, LiBOB

[0085] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt (the weight ratio of LiPF6 and LiBF4 is 1:1) is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0086] Example 12

[0087] The difference from Example 4 is that the additive is only DTD.

[0088] Battery electrolyte includes the following components:

[0089]

[0090]

[0091] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additive is added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1.5% of the total weight of the battery electrolyte.

[0092] Embodiment 13

[0093] Battery electrolyte includes the following components:

[0094] Sulfone solvents Ether solvents Lithium salts additive 3-Methylsulfolane 2-Methyltetrahydrofuran LiDFOB FEC, VC

[0095] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, activated carbon and phosphorus pentoxide in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of FEC added in the additive is 1% of the total weight of the battery electrolyte, and the amount of VC added is 0.5% of the total weight of the battery electrolyte.

[0096] Embodiment 14

[0097] Battery electrolyte includes the following components:

[0098] Sulfone solvents Ether solvents Lithium salts additive 3-Methylsulfolane 2-Methyltetrahydrofuran LiDFOB FEC, VC

[0099] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 3A molecular sieve, activated carbon and phosphorus pentoxide in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of FEC added in the additive is 1% of the total weight of the battery electrolyte, and the amount of VC added is 0.5% of the total weight of the battery electrolyte.

[0100] Embodiment 15

[0101] Battery electrolyte includes the following components:

[0102] Sulfone solvents Ether solvents Lithium salts additive p-Tolylpropyl sulfone Dimethoxymethane <![CDATA[LiSO3CF3]]> TPP, TMSP

[0103] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, metal potassium and metal calcium in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of TPP added in the additive is 1% of the total weight of the battery electrolyte, and the amount of TMSP added is 0.5% of the total weight of the battery electrolyte.

[0104] Example 16

[0105] Battery electrolyte includes the following components:

[0106] Sulfone solvents Ether solvents Lithium salts additive Dichloromethyl cyclobutyl sulfone 1,2-Dimethoxyethane <![CDATA[LiAsF6]]> MMDS, SN

[0107] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of MMDS added in the additive is 1% of the total weight of the battery electrolyte, and the amount of SN added is 0.5% of the total weight of the battery electrolyte.

[0108] Embodiment 17

[0109] Battery electrolyte includes the following components:

[0110] Sulfone solvents Ether solvents Lithium salts additive Phenyl ethyl sulfone Diethylene glycol dimethyl ether <![CDATA[LiC(CF3SO2)3]]> DTD, AND

[0111] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of AND added is 0.5% of the total weight of the battery electrolyte.

[0112] Embodiment 18

[0113] Battery electrolyte includes the following components:

[0114] Sulfone solvents Ether solvents Lithium salts additive Dimethyl sulfone Tetrahydrofuran <![CDATA[Li(CF3SO2)2N]]> DTD, LiBOB

[0115] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 2.5% of the total weight of the battery electrolyte.

[0116] Embodiment 19

[0117] The difference from Example 4 is that the ratio of the sulfone solvent to the ether solvent is 40:60.

[0118] Battery electrolyte includes the following components:

[0119] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6]]> DTD, LiBOB

[0120] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 40:60, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0121] Embodiment 20

[0122] The difference from Example 4 is that the concentration of the lithium salt is 0.8 mol / L.

[0123] Battery electrolyte includes the following components:

[0124] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6]]> DTD, LiBOB

[0125] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 0.8 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0126] Embodiment 21

[0127] The difference from Example 4 is that the amount of the additive added is 5% of the total weight of the battery electrolyte.

[0128] Battery electrolyte includes the following components:

[0129] Sulfone solvents Ether solvents Lithium salts additive Sulfolane Tetrahydrofuran <![CDATA[LiPF6]]> DTD, LiBOB

[0130] The above-mentioned sulfone solvent and the above-mentioned ether solvent are mixed in a weight ratio of 15:85, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above-mentioned lithium salt is dissolved in the mixed solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above-mentioned additives are added thereto and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 2% of the total weight of the battery electrolyte, and the amount of LiBOB added is 1% of the total weight of the battery electrolyte.

[0131] Comparative Example 1

[0132] The difference from Example 4 is that only a sulfone solvent is added.

[0133] Battery electrolyte includes the following components:

[0134] Sulfone solvents Ether solvents Lithium salts additive Sulfolane / LiPF6 DTD, LiBOB

[0135] The above sulfone solvent is filtered through an impurity removal and water removal agent to obtain a pure solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above lithium salt is dissolved in the solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above additive is added and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0136] Comparative Example 2

[0137] The difference from Example 4 is that only an ether solvent is added.

[0138] Battery electrolyte includes the following components:

[0139] Sulfone solvents Ether solvents Lithium salts additive / Tetrahydrofuran LiPF6 DTD, LiBOB

[0140] The above ether solvent is filtered through an impurity removal and water removal agent to obtain a pure solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; the above lithium salt is dissolved in the solvent, and the concentration of the lithium salt in the electrolyte is 2 mol / L; finally, the above additive is added and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0141] Comparative Example 3

[0142] Ethylene carbonate (EC) and diethyl carbonate (DMC) are mixed in a weight ratio of 1:1, and then filtered through an impurity removal and water removal agent to obtain a mixed solvent, wherein the impurity removal and water removal agent is a mixture of 4A molecular sieve, calcium hydride and lithium hydride in a mass ratio of 1:1:1; lithium salt LiPF6 is dissolved in the mixed solvent, and the concentration of lithium salt in the electrolyte is 1 mol / L; finally, additives DTD and LiBOB are added and mixed evenly to obtain a battery electrolyte. Among them, the amount of DTD added in the additive is 1% of the total weight of the battery electrolyte, and the amount of LiBOB added is 0.5% of the total weight of the battery electrolyte.

[0143] The electrolytes prepared in Examples 1 to 21 and Comparative Examples 1 and 3 were applied to lithium manganese iron phosphate batteries, and their relevant performance was tested, and the specific test data was recorded in Table 1. The data shown in Table 1 are the test results of the capacity retention rate (%) at each rate obtained by charging and discharging the battery cells prepared by the electrolytes prepared in the Examples and Comparative Examples at 1C, 2C, 3C, 4C, and 5C between 2.75V and 4.80V; and under the test conditions of 25°C, 3C charging, and 1C discharging, each battery sample was charged and discharged between 2.75V and 4.8V, and the first cycle test result was used as the capacity 100% benchmark, each sample was cycled 1000 times, and the capacity retention rate (%) after 1000 cycles was obtained.

[0144] The preparation method and specific testing method of the battery are described as follows:

[0145] Regarding the preparation of the battery: the positive electrode of the soft-pack battery cell contains, by weight percentage, 29% of ternary materials containing 7 series (Ni content 70%-80%), 67% of lithium manganese iron phosphate material, the content ratio of Mn and Fe in the lithium manganese iron phosphate material is 6:4, and 4% of conductive binder, wherein the conductive binder includes conductive carbon black (SP), carbon nanotubes, and polyvinylidene fluoride (PVDF); the negative electrode contains, by weight percentage, 96% of graphite and 4% of conductive binder, wherein the conductive binder includes SP, polyacrylic acid (PAA), styrene-butadiene rubber emulsion (SBR), and carbon nanotubes. After the top and side of the above-mentioned battery cell are sealed, 40g of the electrolyte prepared in the above-mentioned embodiment and comparative example are added respectively, and the battery cell is obtained after liquid injection and packaging.

[0146] Battery performance test

[0147] Rate capacity retention test: At 25°C, each battery sample was charged and discharged at 1C, 2C, 3C, 4C, and 5C between 2.75V and 4.8V, respectively. The 0.33C test result was taken as the capacity 100% benchmark, and the capacity retention rate (%) at each rate was obtained.

[0148] Fast charge cycle stability test: At 25°C, 3C charging and 1C discharging test conditions, each battery sample was charged and discharged between 2.75V and 4.8V. The first cycle test result was used as the capacity 100% benchmark. Each sample was cycled 1000 times, and the capacity retention rate (%) after 1000 cycles was obtained.

[0149] Table 1

[0150]

[0151]

[0152] From the above description, it can be seen that the above embodiments of the present invention achieve the following technical effects:

[0153] The electrolytes prepared in Examples 1 to 21 and Comparative Examples 1 and 3 were applied to lithium manganese iron phosphate batteries, and their related performance was tested. According to the results in Table 1, the electrolytes prepared in Examples 1 to 21 were applied to lithium manganese iron phosphate batteries, and the capacity retention rates of 1C, 2C, 3C, 4C, and 5C charging and discharging between 2.75V and 4.8V, respectively, showed better results than those of the comparative examples. Under the test conditions of 25°C, 3C charging and 1C discharging, each battery sample was charged and discharged between 2.75V and 4.8V. After 1000 cycles, its capacity retention rate was still significantly improved compared with the comparative example.

[0154] In particular, in Examples 1 to 18, the preparation conditions are controlled within the preferred range when preparing the battery electrolyte. When the prepared electrolyte is applied to the lithium manganese iron phosphate battery, the battery samples are charged and discharged between 2.75V and 4.80V under the test conditions of 25°C, 3C charging, and 1C discharging. When the cycle is 1000 cycles, the capacity retention rate is above 80%, and the charging rate is ≥3C. The capacity retention rate after 1000 cycles can even reach 91.87%, which has obvious progressive significance. In the comparative examples, when only sulfone solvents or only ether solvents are used as the solvent of the battery electrolyte when preparing the electrolyte, or when the conventional solvent formula is used to prepare the battery electrolyte, the charging rate and the capacity retention rate after 1000 cycles are far different from the effects obtained by the scheme described in the present invention.

[0155] In summary, the battery electrolyte prepared by the technical scheme of the present invention and the preparation method described in the present application, when applied to a lithium-ion battery with a battery positive electrode using lithium iron manganese phosphate material as an active material, the lithium-ion battery can be charged and discharged 1000 times within a preferred range at a lower limit voltage of 2.75 to 2.90V and an upper limit voltage of 4.30 to 4.80V with a capacity retention rate greater than 80%, and its charging rate is ≥3C, with good fast charging performance and cycle stability.

[0156] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A battery electrolyte, characterized in that: The battery electrolyte comprises: lithium salt, ether solvent, sulfone solvent and additives.

2. The battery electrolyte according to claim 1, characterized in that The sulfone solvent is selected from one or more compounds having a structure shown in the following formula (I): wherein said R1 and said R2 are each independently selected from H, C1-C20 alkyl, C3-C20 cycloalkyl, C6-C30 substituted or unsubstituted aryl, C6-C30 aralkyl or C1-C6 straight-chain alkyl in which at least part of hydrogen is replaced by halogen; or, said R1, said R2 and the S atom to which they are bonded together form a four- to eight-membered ring; Preferably, R1 and R2 are each independently selected from H, C1-C5 alkyl, C3-C6 cycloalkyl, C6-C12 aryl, C6-C14 aralkyl or C1-C3 straight-chain alkyl in which at least part of hydrogen is replaced by halogen; or, R1, R2 and the S atom to which they are bonded together form a four- to five-membered ring; More preferably, the C1-C5 alkyl group is methyl, ethyl or propyl, the C3-C6 cycloalkyl group is cyclopropyl, cyclobutyl or cyclopentyl, the C6-C30 substituted or unsubstituted aryl group is phenyl, methylphenyl, ethylphenyl or biphenyl, and the C1-C6 straight-chain alkyl group in which at least part of the hydrogen is substituted by halogen is chloromethyl, dichloromethyl, bromomethyl, dibromomethyl, chloroethyl, dichloroethyl, fluoromethyl, difluoromethyl or difluoroethyl; More preferably, the sulfone solvent is sulfolane and / or 3-methylsulfolane.

3. The battery electrolyte according to claim 1, characterized in that The ether solvent is one or more of tetrahydrofuran, 2-methyltetrahydrofuran, dimethoxymethane, 1,2-dimethoxyethane, and diethylene glycol dimethyl ether.

4. The battery electrolyte according to any one of claims 1 to 3, characterized in that The lithium salt is one or more of lithium hexafluorophosphate, lithium bis(fluorosulfonyl)imide, lithium tetrafluoroborate, lithium difluorooxalatoborate, lithium trifluoromethylsulfonate, lithium hexafluoroarsenate, perfluoroalkylsulfonylmethyl lithium and lithium bis(trifluoromethylsulfonyl)imide; Preferably, the concentration of the lithium salt in the battery electrolyte is 1 to 2 mol / L; Further preferably, the concentration of the lithium salt in the battery electrolyte is 1.5 to 2 mol / L.

5. The battery electrolyte according to any one of claims 1 to 4, characterized in that The weight ratio of the sulfone solvent to the ether solvent in the battery electrolyte is (5-30):(70-95); Preferably, the weight ratio of the sulfone solvent to the ether solvent is (10-20):(85-90).

6. The battery electrolyte according to any one of claims 1 to 4, characterized in that: The additive is one or more of fluoroethylene carbonate, vinylene carbonate, tripropargyl phosphate, tris(trimethylsilyl)phosphite, vinyl sulfate, methylene methanedisulfonate, lithium bis(oxalatoborate), succinonitrile and adiponitrile; Preferably, the additive is at least two of the fluoroethylene carbonate, the vinylene carbonate, the tripropargyl phosphate, the tris(trimethylsilyl)phosphite, the vinyl sulfate, the methylene methanedisulfonate, the lithium bis(oxalatoborate), the succinonitrile and the adiponitrile; Preferably, the additive is added in an amount of 1.5 to 3.5% of the total weight of the battery electrolyte; Further preferably, the additive is added in an amount of 1.5-2.5% of the total weight of the battery electrolyte.

7. The battery electrolyte according to any one of claims 1 to 4, characterized in that The lithium salt is lithium hexafluorophosphate, the ether solvent is tetrahydrofuran, the sulfone solvent is sulfolane, and the additives are lithium bis(oxalatoborate) and vinyl sulfate, wherein the concentration of the lithium hexafluorophosphate is 1.5-2 mol / L, the mass ratio of the sulfolane to the tetrahydrofuran is (10-15):(85-90), the addition amounts of the lithium bis(oxalatoborate) and the vinyl sulfate are 1.5-2.5%, and the mass ratio of the lithium bis(oxalatoborate) and the vinyl sulfate is 1:(2-4); or, The lithium salt is lithium bis(fluorosulfonyl)imide, the ether solvent is tetrahydrofuran, the sulfone solvent is sulfolane, and the additives are lithium bis(oxalatoborate) and vinylene carbonate, wherein the concentration of the lithium bis(fluorosulfonyl)imide is 2 mol / L, the mass ratio of the sulfolane to the tetrahydrofuran is (10-15):90, the addition amount of the lithium bis(oxalatoborate) and the vinyl sulfate is 1.5%, and the mass ratio of the lithium bis(oxalatoborate) and the vinyl sulfate is 1:2; or, The lithium salt is lithium hexafluorophosphate, the ether solvent is tetrahydrofuran, the sulfone solvent is cyclopentane, and the additives are lithium bis(oxalatoborate) and vinyl sulfate, wherein the concentration of the lithium hexafluorophosphate is 2 mol / L, the mass ratio of the cyclopentane to the tetrahydrofuran is 15:85, the addition amounts of the lithium bis(oxalatoborate) and the vinyl sulfate are 1.5%, and the mass ratio of the lithium bis(oxalatoborate) and the vinyl sulfate is 1:

2.

8. A method for preparing a battery electrolyte according to any one of claims 1 to 7, characterized in that: The method for preparing the battery electrolyte comprises the following steps: S1, mixing a sulfone solvent and an ether solvent, removing impurities and water, and obtaining a mixed solvent; S2, adding a lithium salt to the mixed solvent to obtain a premixed solution; S3, adding additives to the premixed solution to obtain the battery electrolyte.

9. The method for preparing a battery electrolyte according to claim 8, characterized in that: The impurity removal and water removal process is obtained by filtering the mixed solvent through the impurity removal and water removal reagent, wherein the impurity removal and water removal reagent is one or more of molecular sieve, activated carbon, calcium hydride, lithium hydride, anhydrous calcium oxide, calcium chloride, phosphorus pentoxide, alkali metal or alkaline earth metal; Preferably, the molecular sieve is at least one of type 3A molecular sieve, type 4A molecular sieve and type 5A molecular sieve; Preferably, the molecular sieve is type 4A molecular sieve and / or type 5A molecular sieve.

10. A lithium ion battery, characterized in that: The invention comprises a battery electrolyte as claimed in any one of claims 1 to 7 and a battery positive electrode with lithium iron manganese phosphate material as an active material, wherein the capacity retention rate of the lithium ion battery after 1000 charge and discharge cycles at a lower limit voltage of 2.75 to 2.90 V and an upper limit voltage of 4.30 to 4.80 V is preferably greater than 80%, and its charging rate is ≥3C.