Preparation method of high-dispersity LATP powder
Through nano-grinding, airflow depolymerization and deep water removal, the dispersion of LATP powders is improved by using grinding solvents of different polarities and lithium salts, the problem of easy agglomeration of 100-nanometer powders is solved, and high dispersion is achieved The preparation of LATP powder and the improvement of battery performance are simple and low-cost, suitable for large-scale production.
Patent Information
- Application Number
- CN202411303910.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-19
- Publication Date
- 2024-11-12
AI Technical Summary
It is difficult to prepare high-dispersible 100-nanometer LATP powders, which are prone to agglomeration, resulting in poor battery performance. Common methods such as high energy consumption for secondary sintering or the introduction of coupling agents affect battery performance.
Using nano-grinding, airflow depolymerization, deep water removal and low dew point packaging methods, the steric steric hindrance and zeta potential of the powder are increased by grinding solvents of different polarities and lithium salts, reducing surface effects and agglomeration phenomena, and achieving high Preparation of dispersible LATP powder.
The preparation of high-dispersible nano-scale LATP powder is realized, which reduces the surface effect of the powder, improves dispersion and battery performance, and is simple and cheap, suitable for large-scale production.
Smart Images

Figure CN118943503A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of lithium battery raw materials, and in particular to a method for preparing highly dispersible LATP powder. Background Art
[0002] Lithium-ion batteries have the advantages of high energy density, high operating voltage, long service life and no memory effect. They have been widely used in consumer electronic products such as mobile phones, digital cameras and laptops, and have broad application prospects in electric vehicles, large-scale energy storage and other fields. However, conventional liquid lithium-ion batteries still have problems such as insufficient energy density and potential safety hazards. The emergence of solid-state batteries can perfectly solve the above problems. While improving energy density, organic electrolytes and diaphragms are replaced with inorganic solid electrolytes to achieve the intrinsic safety of lithium-ion batteries. Currently, common solid electrolytes are mainly oxides, polymers, sulfides and halides.
[0003] As an oxide solid electrolyte, LATP has been widely used and used due to its high chemical and electrochemical stability, high ionic conductivity, easy processing, low cost, and good mechanical properties. Its application scenarios mainly include positive and negative electrode coating, diaphragm coating, pole piece blending, organic-inorganic composite diaphragms, etc. In order to better exert its performance, diaphragm coating often uses LATP powder with a particle size of 500-800nm to make coating slurry, and positive and negative electrode coating or pole piece blending often uses LATP powder with a particle size of 100nm-300nm. Whether LATP powder is doped into the slurry or LATP powder is coated with positive and negative electrode materials and then sintered, this puts forward high requirements on the particle size uniformity and dispersibility of nano LATP powder. The 300nm-800nm LATP powder currently circulating on the market has good dispersibility and basically no agglomeration when well preserved. However, as the "main force" of positive and negative electrode blending, 100nm LATP powder is difficult to maintain high dispersibility and will have particle agglomeration.
[0004] The particle size of 100 nanometers is small, the volume fraction of atoms located on the surface is large, and the atomic density is reduced, which makes the nanoparticles have surface effect, volume effect and quantum size effect. Due to the surface effect and volume effect, the nanopowder itself is easy to agglomerate, and the larger specific surface area will also make the powder absorb water more quickly. During the positive electrode coating or blending process, the agglomerated LATP powder cannot be evenly dispersed in the slurry, the particle size is different, and it cannot be fully and evenly mixed with the positive electrode material. The water absorption of the powder will also cause the battery moisture content to be too high, and ultimately lead to poor battery performance.
[0005] Patent CN117352828A adopts secondary sintering technology to reduce a large amount of crystal water adsorbed on the surface of the solid electrolyte. The method is simple, the moisture content of the prepared powder is low, and it can be prepared on a large scale. However, the secondary sintering method has high energy consumption, and powder agglomeration will occur after sintering, and the powder needs to be depolymerized for a second time, which is a long process. Patent CN108676197A adopts the method of adding a coupling agent to the solution system, and then ultrasonically dispersing the material powder, evaporating the solvent, and blowing drying the material powder in steps to obtain a nano powder with high dispersibility. However, the coupling agent added thereto will have a negative impact on the battery performance when introduced into the battery system, and the chemical bonding between the silane coupling agent listed therein and the nano material is not suitable for LATP powder. Summary of the invention
[0006] In view of the above problems, the present invention aims to provide a method for preparing highly dispersible LATP powder with low cost and easy scalability.
[0007] To achieve the technical purpose, the scheme of the present invention is: a method for preparing highly dispersible LATP powder, the specific steps are as follows:
[0008] S1. Nano-grinding: Add LATP coarse powder, lithium-containing salt and grinding solvent into a nano-sand mill according to a specified ratio, and grind to form a nano-slurry with uniform particle size distribution;
[0009] S2, drying: transferring the nano-sized slurry to an oven for drying to obtain a dried material;
[0010] S3, airflow depolymerization: airflow depolymerization of the dried material is performed using airflow pulverization equipment to obtain depolymerized LATP powder of a specified particle size;
[0011] S4, deep dehydration: the depolymerized LATP powder after airflow depolymerization is transferred into a vacuum oven for deep dehydration. After the dehydration is completed, high-purity inert gas is filled into the oven to normal pressure, and then the inert gas is continuously passed to cool down to obtain dry LATP powder;
[0012] S5. Packaging: Dry LATP powder should be packaged in a low dew point environment and stored in a sealed container.
[0013] Preferably, in step S1, LATP is Li 1+x Al x Ti 2-x (PO4)3, wherein 0≤x≤0.5, the particle size D of the LATP in the LATP coarse powder max ≤100μm; the particle size of LATP in the nano-slurry is D50=100±10nm;
[0014] The grinding rotor of the nano sand mill is a pin-type sand mill or a turbine-type sand mill, and the ball-material separation structure of the nano sand mill is a centrifugal separation structure or a screen separation structure; the size range of the grinding zirconium beads in the nano sand mill is 0.05-0.3 mm, and the mass percentage of LATP in the nano-sized slurry is 10%-70%.
[0015] Preferably, the lithium-containing salt is one or more of lithium bis(trifluoromethylsulfonyl imide), lithium acetate, and lithium borate; and the mass percentage of the lithium-containing salt is 0.5-3%.
[0016] Preferably, the grinding solvent is one or more of isopropanol, n-butanol or dimethyl carbonate; the mass percentage of the grinding solvent is 27-89.5%.
[0017] Preferably, in step S2, the oven is a vacuum oven, the vacuum degree is controlled below 300 Pa, the drying temperature is 70-120° C., the drying time is 6-10 h, and the residual amount of grinding solvent in the dried material is 0.5%-4%.
[0018] Preferably, in step S3, the air flow pulverizing equipment is an open-loop air flow pulverizer or a closed-loop air flow pulverizer, the air source used by the air flow pulverizing equipment is high-purity nitrogen or compressed air after moisture removal, and the depolymerization process should be carried out in a low dew point environment, with a dew point range of 0 to -50°C.
[0019] Preferably, in step S4, the vacuum degree of the vacuum oven is controlled below 300 Pa, the dehydration temperature is 80-150° C., and the dehydration time is 1-8 hours. The nitrogen flow time is 10-120 minutes, and the internal pressure of the oven is slightly positive during the nitrogen flow process; the particle size D50 of the dried LATP powder is 100±8nm.
[0020] Preferably, in step S5, the temperature of the oven is lowered to ≤50° C. before the powder is packaged, and the dew point of the packaging environment is 0 to -50° C. The sealed storage is stored in an aluminum-plastic bag with a slight negative pressure seal.
[0021] The beneficial effects of the present invention are as follows: the present application is a method for preparing highly dispersed nano-scale LATP powder; in view of the technical problem that 100-nanometer LATP powder is extremely prone to agglomeration due to its surface effect, volume effect and quantum size effect, and highly dispersed LATP powder cannot be prepared, and the application is limited, the present application uses grinding solvents of different polarities to grind the powder, establishes a powder solvation film on the surface of the powder particles, thereby increasing steric hindrance and reducing the surface effect of the nanopowder; by adding corresponding lithium-containing salts to enhance the Zeta potential of the powder, the charge repulsion between the powders is made greater than the van der Waals force, and the powder dispersibility is improved. The method of the present application is simple, low-cost, and easy to mass produce. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 It is a processing flow chart of the present invention;
[0023] Figure 2 This is the SEM picture of the present invention. DETAILED DESCRIPTION
[0024] The present invention is further described in detail below with reference to the accompanying drawings and specific embodiments.
[0025] like Figure 1-2 As shown, the specific embodiment of the present invention is an embodiment: a method for preparing highly dispersible LATP powder, the specific steps are as follows:
[0026] S1. Nano-grinding: Add LATP coarse powder, lithium-containing salt and grinding solvent into a nano-sand mill according to a specified ratio. The grinding rotor of the nano-sand mill is a pin-type sand mill or a turbine-type sand mill. The ball-material separation structure of the nano-sand mill is a centrifugal separation structure or a screen separation structure. The size range of the grinding zirconium beads in the nano-sand mill is 0.05-0.3 mm, and the mass percentage of LATP in the nano-slurry is 10%-70%.
[0027] The nano-sized slurry with uniform particle size distribution is prepared by grinding; LATP is Li 1+x Al x Ti 2-x (PO4)3, wherein 0≤x≤0.5, the particle size D of the LATP in the LATP coarse powder max ≤100μm; the particle size of LATP in the nano-slurry is D50=100±10nm;
[0028] The lithium-containing salt is one or more of lithium hexafluorophosphate, lithium hexafluoroarsenate, lithium tetrafluoroborate, lithium difluorophosphate, lithium bisoxalate borate, lithium difluorooxalate borate, lithium bis(trifluoromethylsulfonyl imide), lithium bis(fluorosulfonyl imide), lithium difluorobisoxalate phosphate, lithium trifluoromethylsulfonate, lithium (fluorosulfonyl)(perfluorobutylsulfonyl)imide, lithium bis(pentafluoroethylsulfonyl)imide, lithium bis(fluoromalonate)borate, lithium bis(2-methyl-2-fluoromalonate)borate, 4,5-dicyano-2-trifluoromethyl-imidazole lithium, lithium citrate, lithium acetate, lithium oxalate, lithium acetate, lithium borate, lithium perchlorate, lithium chlorate, lithium nitrate, lithium iodate, lithium bromate, lithium hexafluorosilicate, lithium silicate, lithium sulfate or lithium phosphate; the mass percentage of the lithium-containing salt is 0.5-3%.
[0029] The grinding solvent is one or more of N-methylpyrrolidone, methanol, ethanol, n-propanol, isopropanol, n-butanol, isobutanol, acetone, acetonitrile, butyronitrile, dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, ethylene carbonate, propylene carbonate, petroleum ether, cyclohexane, pentane oxide, carbon tetrachloride, trichloroethylene, carbon disulfide, toluene, xylene, benzene, dichloromethane, chloroform, ether, ethyl acetate, and acetone; the mass percentage of the grinding solvent is 27-89.5%.
[0030] S2, drying: the nano-sized slurry is transferred to an oven for drying to obtain a dried material; the oven is a vacuum oven, the vacuum degree is controlled below 300Pa, the drying temperature is 70-120°C, the drying time is 6-10h, and the residual amount of the grinding solvent in the dried material is 0.5%-4%.
[0031] S3. Airflow depolymerization: Use airflow pulverizing equipment to perform airflow depolymerization on the dried material to obtain depolymerized LATP powder of a specified particle size; the airflow pulverizing equipment is an open-loop airflow pulverizer or a closed-loop airflow pulverizer, and the air source used by the airflow pulverizing equipment is high-purity nitrogen or compressed air after moisture removal. The depolymerization process should be carried out in a low dew point environment, and the dew point range is 0 to -50°C.
[0032] S4, deep dehydration: the depolymerized LATP powder after airflow depolymerization is transferred into a vacuum oven for deep dehydration. After the dehydration is completed, high-purity inert gas is filled into the oven to normal pressure, and then the inert gas is continuously passed to cool down to obtain dry LATP powder; the vacuum degree of the vacuum oven is controlled below 300Pa, the dehydration temperature is 80-150℃, and the dehydration time is 1-8h. The nitrogen passing time is 10-120min, and the internal pressure of the oven is slightly positive during the nitrogen passing process; the particle size D50 in the dry LATP powder is 100±8nm.
[0033] S5. Packaging: Dry LATP powder is packaged in a low dew point environment and sealed for storage. The temperature of the oven is reduced to ≤50°C before packaging the powder, and the dew point environment of the packaging is 0 to -50°C. The sealed storage is stored in an aluminum-plastic bag with a slight negative pressure seal.
[0034] Embodiment 1
[0035] S101, nano-grinding: 10 kg of LATP coarse powder (D50 = 1.2 μm) max ≤100μm), 203g of LiTFSI (lithium bis(trifluoromethylsulfonyl)imide) and 56kg of n-butanol were added into a pin-type nano sand mill (centrifugal dual-power type) at a solid content of 15%, and after grinding for 6.5 hours, the LATP particle size of the nano-sized slurry was obtained to be D50=102nm; wherein the size range of the grinding zirconium beads was 0.05-0.15mm;
[0036] S102, drying: the nano-sized slurry is transferred to a vacuum oven for drying at a temperature of 110° C. for a drying time of 8 hours, and the residual amount of n-butanol in the dried material is 2%, to obtain a dried material with a LATP particle size of D50=106 nm;
[0037] S103, airflow depolymerization: airflow depolymerization of the dried material is performed using airflow grinding equipment in a room with a dew point of -40°C, and high-purity nitrogen is used as grinding gas to obtain depolymerized LATP powder with a LATP particle size of D50 = 103 nm;
[0038] S104, deep dehydration: the depolymerized LATP powder after airflow depolymerization is transferred into a vacuum oven for deep dehydration, the vacuum degree is 60Pa, the dehydration temperature is 130°C, the dehydration time is 16H, after the dehydration is completed, high-purity nitrogen is filled into the oven to normal pressure, and then the nitrogen is continuously passed to cool down, to obtain dry LATP powder with a LATP particle size D50=104nm;
[0039] S105. Packaging: Dry LATP powder should be packaged in a low dew point environment and stored in a sealed container.
[0040] The particle size measured in each step of this embodiment and the moisture content of the final powder are shown in the table below.
[0041] D10 / nm D50 / nm D90 / nm D99 / nm Moisture content / ppm S101 60 102 226 345 / S102 65 106 230 345 8575 S103 62 103 226 348 9364 S104 63 104 236 350 894 S105 65 105 240 354 900
[0042] Embodiment 2
[0043] S101, nano-grinding: 10 kg of LATP coarse powder (D50 = 1.2 μm) max≤100μm), 46.7g of lithium acetate and 56kg of isopropanol were added into a pin-type nano sand mill (centrifugal dual-power type) at a solid content of 15%, and after grinding for 7 hours, the LATP particle size of the nano-slurry was obtained, D50 = 97nm; wherein the size range of the grinding zirconium beads was 0.05-0.15mm;
[0044] S102, drying: transferring the nano-sized slurry to a vacuum oven for drying at a temperature of 75° C. for 8 hours, and the residual amount of n-butanol in the dried material being 3%, to obtain a dried material having a LATP particle size of D50=96 nm;
[0045] S103, airflow depolymerization: airflow depolymerization of the dried material is performed using airflow pulverization equipment in a room with a dew point of -40°C, and high-purity nitrogen is used as grinding gas to obtain depolymerized LATP powder with a LATP particle size of D50 = 100 nm;
[0046] S104, deep dehydration: the depolymerized LATP powder after airflow depolymerization is transferred into a vacuum oven for deep dehydration, the vacuum degree is 60Pa, the dehydration temperature is 130°C, the dehydration time is 16H, after the dehydration is completed, high-purity nitrogen is filled into the oven to normal pressure, and then the nitrogen is continuously passed to cool down, to obtain dry LATP powder with a LATP particle size D50=105nm;
[0047] S105. Packaging: Dry LATP powder should be packaged in a low dew point environment and stored in a sealed container.
[0048] The particle size measured in each step of this embodiment and the moisture content of the final powder are shown in the table below.
[0049] D10 / nm D50 / nm D90 / nm D99 / nm Moisture content / ppm S101 57 97 226 345 / S102 60 96 224 345 11260 S103 60 100 230 345 10638 S104 63 104 236 350 780 S105 60 105 225 345 780
[0050] Comparative Example 1
[0051] Compared with Example 1, LiTFSI (lithium bis(trifluoromethylsulfonyl)imide) was not added to S101, and other parameters remained the same. The particle size measured in each step of this comparative example and the water content of the final powder are shown in the table below.
[0052] D10 / nm D50 / nm D90 / nm D99 / nm Moisture content / ppm S101 60 108 220 345 / S102 63 104 291 1215 9648 S103 64 138 1074 1688 105651 S104 79 221 1633 2360 638 S105 81 223 1782 2518 689
[0053] Comparative Example 2
[0054] Compared with Example 1, S102 uses xylene as the sanding solvent for sanding, and other parameters remain the same. The particle size measured in each step of this comparative example and the water content of the final powder are shown in the table below.
[0055] D10 / nm D50 / nm D90 / nm D99 / nm Moisture content / ppm S101 60 105 218 345 / S102 64 138 1074 1688 6545 S103 75 189 1135 1904 5165 S104 79 232 1752 2531 663 S105 77 226 1649 2519 642
[0056] Comparative Example 3
[0057] Compared with Example 1, in step S103, the depolymerization was not carried out in a room with a dew point of -40°C, and other parameters remained the same. The particle size measured in each step of this comparative example and the water content of the final powder are shown in the table below.
[0058] D10 / nm D50 / nm D90 / nm D99 / nm Moisture content / ppm S101 63 103 226 345 / S102 63 105 250 345 8139 S103 90 258 2816 5228 13844 S104 81 250 2955 5397 4395 S105 93 276 3018 5573 4826
[0059] Due to its surface effect, volume effect and quantum size effect, 100 nanometer LATP powder is very easy to agglomerate, and its application is limited. The preparation method of a highly dispersible LATP powder described in the present invention is reasonably designed. By selecting grinding solvents with different polarities, a powder solvation film is established, thereby increasing steric hindrance and reducing the surface effect of the nanopowder; by adding corresponding lithium-containing salts to enhance the Zeta potential of the powder, the charge repulsion between the powders is made greater than the van der Waals attraction, thereby improving the powder dispersibility.
[0060] This method selects grinding solvents of different polarities to establish a powder solvation film, thereby increasing steric hindrance and reducing the surface effect of nanopowders; secondly, the Zeta potential of the powder is enhanced by adding corresponding lithium-containing salts, so that the charge repulsion between the powders is greater than the van der Waals force, thereby improving the powder dispersibility. The method is simple, low-cost, can be prepared on a large scale, and has broad application prospects.
[0061] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any slight modification, equivalent substitution and improvement made to the above embodiment based on the technical essence of the present invention should be included in the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing highly dispersible LATP powder, characterized in that: The specific steps are as follows: S1. Nano-grinding: Add LATP coarse powder, lithium-containing salt and grinding solvent into a nano-sand mill according to a specified ratio, and grind to form a nano-slurry with uniform particle size distribution; S2, drying: transferring the nano-sized slurry to an oven for drying to obtain a dried material; S3, airflow depolymerization: airflow depolymerization of the dried material is performed using airflow pulverization equipment to obtain depolymerized LATP powder of a specified particle size; S4, deep dehydration: the depolymerized LATP powder after airflow depolymerization is transferred into a vacuum oven for deep dehydration. After the dehydration is completed, high-purity inert gas is filled into the oven to normal pressure, and then the inert gas is continuously passed to cool down to obtain dry LATP powder; S5. Packaging: Dry LATP powder should be packaged in a low dew point environment and stored in a sealed container.
2. The method for preparing highly dispersible LATP powder according to claim 1, characterized in that: In step S1, LATP is Li 1+x Al x Ti 2-x (PO4)3, wherein 0≤x≤0.5, the particle size D of the LATP in the LATP coarse powder max ≤100μm; the particle size of LATP in the nano-slurry is D50=100±10nm; The grinding rotor of the nano sand mill is a pin-type sand mill or a turbine-type sand mill, and the ball-material separation structure of the nano sand mill is a centrifugal separation structure or a screen separation structure; the size range of the grinding zirconium beads in the nano sand mill is 0.05-0.3 mm, and the mass percentage of LATP in the nano-sized slurry is 10%-70%.
3. The method for preparing highly dispersible LATP powder according to claim 1, characterized in that: The lithium-containing salt is one or more of lithium bis(trifluoromethylsulfonyl imide), lithium acetate and lithium borate; the mass percentage of the lithium-containing salt is 0.5-3%.
4. The method for preparing highly dispersible LATP powder according to claim 1, characterized in that: The grinding solvent is one or more of isopropanol, n-butanol or dimethyl carbonate; the mass percentage of the grinding solvent is 27-89.5%.
5. The method for preparing highly dispersible LATP powder according to claim 1, characterized in that: In the step S2, a vacuum oven is used, the vacuum degree is controlled below 300 Pa, the drying temperature is 70-120° C., the drying time is 6-10 hours, and the residual amount of grinding solvent in the dried material is 0.5%-4%.
6. The method for preparing highly dispersible LATP powder according to claim 1, characterized in that: In step S3, the air flow pulverizing equipment is an open-loop air flow pulverizer or a closed-loop air flow pulverizer. The air source used by the air flow pulverizing equipment is high-purity nitrogen or compressed air after moisture removal. The depolymerization process should be carried out in a low dew point environment, and the dew point range is 0 to -50°C.
7. The method for preparing highly dispersible LATP powder according to claim 1, characterized in that: In step S4, the vacuum degree of the vacuum oven is controlled below 300 Pa, the dehydration temperature is 80-150° C., and the dehydration time is 1-8 hours. The nitrogen flow time is 10-120 minutes, and the internal pressure of the oven is slightly positive during the nitrogen flow process; the particle size D50 of the dried LATP powder is 100±8nm.
8. The method for preparing highly dispersible LATP powder according to claim 1, characterized in that: In the step S5, the temperature of the oven is lowered to ≤50° C. before the powder is packaged, and the dew point environment of the packaging is 0 to -50° C. The sealed storage is stored in an aluminum-plastic bag with a slight negative pressure seal.
Citation Information
Patent Citations
Method for improving nano powder dispersity
CN108676197A
Treatment method for solving high moisture problem of nano solid electrolyte
CN117352828A