Recycling method of positive electrode material and regenerated positive electrode material

By preparing an organic nickel source shell on the surface of waste cathode material and sintering it, the problems of carbon dioxide emissions and poor electrochemical performance during cathode material recycling were solved, realizing the preparation of highly efficient regenerated cathode material and improving electrochemical performance and specific capacity.

CN118943547AActive Publication Date: 2024-11-12四川新能源汽车创新中心有限公司
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410988669.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-23
Publication Date
2024-11-12
Estimated Expiration
2044-07-23

AI Technical Summary

Technical Problem

Existing cathode material recycling processes suffer from carbon dioxide emissions and poor electrochemical performance, especially the low specific capacity of low- and medium-nickel recycled materials.

Method used

An organic nickel source shell was prepared on the surface of waste cathode material using a liquid phase method. Ni-MOF material was formed through hydrothermal reaction and then mixed with lithium source and sintered to form a recycled cathode material.

Benefits of technology

This process improves the uniformity of nickel source dispersion and the tightness of contact on the surface of waste cathode materials, thereby enhancing the electrochemical performance of recycled cathode materials. The process is simple, low-cost, and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943547A_ABST
    Figure CN118943547A_ABST
Patent Text Reader

Abstract

The invention discloses a recycling method of a positive electrode material and a regenerated positive electrode material, and belongs to the technical field of battery material recycling. The recycling method comprises the following steps: preparing an organic nickel source shell layer on the surface of the positive electrode material, mixing with a lithium source, and sintering to obtain the regenerated positive electrode material. The method is simple in process, low in cost and environment-friendly, and the recycled positive electrode material which can be recycled can be obtained after the waste positive electrode material is regenerated. According to the method, an organic nickel source shell layer is firstly prepared on the surface of the waste positive electrode material, and then lithium supplement sintering is carried out, so that compared with the mode that nickel oxide or hydroxide is directly added in the recycling, upgrading and reconstructing process, a nickel source can be dispersed on the surface of the waste positive electrode material more uniformly, a larger contact area is obtained, and the lithium supplement sintering efficiency is improved. And moreover, the contact between the nickel source and the waste positive electrode material is closer, and the obtained regenerated positive electrode material has better electrochemical performance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of battery material recycling, and in particular to a positive electrode material recycling method and a regenerated positive electrode material. Background Art

[0002] Lithium-ion batteries are widely used in portable electronic products, electric vehicles, and energy storage systems. How to effectively recycle power batteries will become a critical issue in recent years.

[0003] Positive electrode materials (NCM and NCA) are the main positive electrode materials used in lithium-ion batteries. Their main recycling processes include pyrometallurgical recycling and hydrometallurgical recycling. However, the above recycling process involves high-temperature smelting, acid leaching and chemical precipitation, which inevitably lead to carbon dioxide emissions and other waste generation. Direct repair technology is a repair method that does not destroy the original material structure and restores its phase-changed harmful structure to its initial state.

[0004] In recent years, most power battery materials are based on medium and low nickel. Even after they are recycled using direct repair technology, the corresponding recycled materials still have poor electrochemical performance (such as low specific capacity).

[0005] In view of this, the present invention is proposed. Summary of the invention

[0006] The object of the present invention is to provide a method for recovering positive electrode materials and regenerating positive electrode materials to solve or improve the above technical problems.

[0007] The present invention can be implemented like this:

[0008] In a first aspect, the present invention provides a method for recovering positive electrode materials, which comprises the following steps: preparing an organic nickel source shell on the surface of waste positive electrode materials to obtain a positive electrode material precursor; mixing the positive electrode material precursor with a lithium source and sintering them to obtain a regenerated positive electrode material.

[0009] In an optional embodiment, the waste positive electrode material is a layered structure.

[0010] In an optional embodiment, the waste positive electrode material includes at least one of waste nickel cobalt manganese oxide positive electrode material, waste nickel cobalt aluminum oxide positive electrode material and waste lithium cobalt oxide positive electrode material;

[0011] And / or, the organic nickel source shell layer is a Ni-MOF material having a metal organic framework structure.

[0012] In an optional embodiment, the preparation of the organic nickel source shell layer comprises: mixing the waste positive electrode material and the raw material for preparing the organic nickel source shell layer and then performing a hydrothermal reaction;

[0013] The preparation raw materials include nickel salt, organic ligand and organic solvent.

[0014] In an optional embodiment, the nickel salt includes at least one of Ni(NO3)2, NiCl2, Ni(CH3COO)2, and Ni(SO4)2;

[0015] and / or, the organic ligand comprises at least one of terephthalic acid, phthalic acid, 2,5-dihydroxyterephthalic acid and trimesic acid;

[0016] And / or, the organic solvent includes N,N-dimethylformamide.

[0017] In an optional embodiment, the hydrothermal reaction is carried out at 120° C. to 180° C. for 8 h to 16 h.

[0018] In an alternative embodiment, the lithium source comprises at least one of LiOH, Li2CO3, LiNO3, and CH3COOLi.

[0019] In an optional embodiment, the sintering includes a first sintering stage and a second sintering stage; wherein, the first sintering stage is to keep the temperature at 450℃~550℃ for 4h~5h, and the second sintering stage is to keep the temperature at 750℃~900℃ for 8h~15h, and then cool down to 200℃~220℃.

[0020] In an optional embodiment, the heating rate and cooling rate of the sintering process are both 1°C / min to 12°C / min;

[0021] And / or, sintering is performed in an oxygen atmosphere.

[0022] In an optional embodiment, the heating rate and cooling rate of the sintering process are both 5° C. / min to 10° C. / min.

[0023] In an optional embodiment, the sintering is performed under the condition of an oxygen partial pressure of 0.01 to 1 standard atmosphere.

[0024] In a second aspect, the present invention provides a regenerated positive electrode material, which is obtained by treating waste positive electrode material with the recycling method of any one of the aforementioned embodiments.

[0025] The beneficial effects of the present invention include:

[0026] The present invention adopts a method of first preparing an organic nickel source shell layer on the surface of the waste positive electrode material and then performing lithium supplementation sintering. Compared with directly adding nickel oxide or hydroxide in the recycling and upgrading process, the nickel source can be dispersed more evenly on the surface of the waste positive electrode material, obtaining a larger contact area, and also facilitating a closer contact between the nickel source and the waste positive electrode material. The obtained regenerated positive electrode material has better electrochemical performance. The method is simple in process, low in cost, and environmentally friendly, and can regenerate the waste positive electrode material to obtain a reusable regenerated positive electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0028] Figure 1 This is a SEM image of the waste positive electrode material powder in Example 1;

[0029] Figure 2 This is a SEM image of the regenerated positive electrode material in Example 1;

[0030] Figure 3 This is the SEM image of the regenerated positive electrode material in Comparative Example 1. DETAILED DESCRIPTION

[0031] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0032] The following is a detailed description of the positive electrode material recovery method and the regenerated positive electrode material provided in the present application.

[0033] At present, some technologies increase the specific capacity of medium- and low-nickel recycled positive electrode materials by increasing the nickel content, but the inventor proposes: if nickel oxide or hydroxide is directly used as the nickel source for high-temperature nickel supplementation through solid-phase sintering, during the solid-phase sintering process, due to the high melting point of nickel oxide, it is difficult to reach a molten state at a suitable sintering temperature, resulting in a small contact area between the waste positive electrode material and the nickel source, which is not conducive to nickel diffusion. As a result, during the sintering process, the contact between the waste positive electrode material and the nickel oxide or hydroxide is poor, and the nickel element is difficult to diffuse evenly, making it difficult to effectively improve the electrochemical properties of the sintered material.

[0034] Based on this, the present invention creatively proposes to use a liquid phase method to prepare an organic nickel source on the surface of the waste positive electrode material to form an organic nickel source shell. This method can make the nickel source disperse more evenly on the surface of the waste positive electrode material to obtain a larger contact area, and can also make the contact between the nickel source and the waste positive electrode material closer, which is beneficial to improving the electrochemical performance of the regenerated positive electrode material.

[0035] It should be emphasized that the "medium-low nickel" in the present invention can be understood as: before adding nickel, the relative content of nickel in the positive electrode material is low. After adding nickel, the relative content of nickel in the positive electrode material is high, which can be correspondingly referred to as "high nickel". Therefore, the present invention does not specifically limit the nickel content of the regenerated positive electrode material before adding nickel. Positive electrode materials with any nickel content can use the method of the present invention to increase the nickel content to improve the electrochemical properties such as the specific capacity of the regenerated positive electrode material. In some of the enumerated embodiments, "medium-low nickel" can mean that the nickel content in the positive electrode material does not exceed 50%, and "high nickel" can mean that the nickel content in the positive electrode material is not less than 80%.

[0036] For reference, the method for recycling positive electrode materials in waste lithium-ion batteries proposed in the present application may include the following steps: preparing an organic nickel source shell on the surface of the waste positive electrode material to obtain a positive electrode material precursor; mixing the positive electrode material precursor with a lithium source and sintering them to obtain a regenerated positive electrode material.

[0037] Waste positive electrode materials can be obtained, for example, by disassembling and separating waste battery bags to obtain positive electrode sheets, then calcining the positive electrode sheets to allow powder to fall off the current collector, collecting the powder, grinding it and sieving it to obtain waste positive electrode material powder.

[0038] For example, the calcination temperature may be 550° C., and the calcination time may be 1 h to 4 h.

[0039] In some embodiments, the spent positive electrode material may illustratively but not limitatively include at least one of spent nickel cobalt manganese oxide positive electrode material, spent nickel cobalt aluminum oxide positive electrode material, and spent lithium cobalt oxide positive electrode material.

[0040] In some embodiments, the waste positive electrode material may be a layered structure.

[0041] In some embodiments, the above-mentioned waste positive electrode material may be a single crystal structure, and its average particle size may be 4 μm to 6 μm, such as 4 μm, 4.5 μm, 5 μm, 5.5 μm or 6 μm. In some other embodiments, the waste positive electrode material may be a polycrystalline structure. However, after the waste positive electrode material with a single crystal structure adopts the method provided by the present invention, the improvement in specific capacity and other aspects is more obvious. The reason may be that when the single crystal structure is coated in the liquid phase, the coating can be in close contact with all positions of the particles, so it is more possible to coat all positions of the particles evenly; while the contact positions between particles of the polycrystalline structure are more difficult to achieve effective contact with the coating, which makes the coating effect of these positions worse.

[0042] In the present invention, the organic nickel source shell layer is a Ni-MOF material having a metal organic framework structure.

[0043] Ni-MOF material is used as the Ni source. Compared with inorganic nickel source, Ni-MOF is easier to deposit on the surface of the particles, achieving uniform Ni-MOF coating.

[0044] In some embodiments, the preparation of the organic nickel source shell layer may include: mixing the waste positive electrode material and the raw material for preparing the organic nickel source shell layer and then performing a hydrothermal reaction;

[0045] The preparation raw materials include nickel salt, organic ligand and organic solvent.

[0046] Specifically, nickel salt and organic ligand can be dissolved in an organic solvent to form a mixed solution, and then the waste positive electrode material is dispersed in the mixed solution, stirred for 20 minutes to 60 minutes, and then transferred to a hydrothermal reactor for hydrothermal reaction.

[0047] The nickel salt may illustratively but not limitatively include at least one of Ni(NO3)2, NiCl2, Ni(CH3COO)2 and Ni(SO4)2.

[0048] The organic ligand may illustratively but not limitatively include at least one of terephthalic acid, phthalic acid, 2,5-dihydroxyterephthalic acid, and trimesic acid.

[0049] The organic solvent may illustratively but not limitedly include N,N-dimethylformamide (DMF).

[0050] The relationship between the amount of the above ligand and nickel can be referred to as follows: based on the carboxyl groups contained in the ligand, two carboxyl groups match one Ni 2+ .

[0051] In some embodiments, the hydrothermal reaction can be carried out at 120°C to 180°C (such as 120°C, 130°C, 140°C, 150°C, 160°C, 170°C or 180°C, etc.) for 8h to 16h (such as 8h, 10h, 12h, 14h or 16h, etc.).

[0052] Through the above hydrothermal reaction, a Ni-MOF shell can be formed on the surface of the waste positive electrode material.

[0053] In some embodiments, the lithium source may illustratively but not limitingly include at least one of LiOH, Li2CO3, LiNO3, and CH3COOLi.

[0054] The total amount of lithium contained in the waste positive electrode material and the lithium contained in the newly added lithium source is 1.03 to 1.08 times (in molar amount) the total amount of transition metals in the positive electrode material precursor.

[0055] The sintering includes a first sintering stage and a second sintering stage. The first sintering stage can be kept at 450°C to 550°C (such as 450°C, 480°C, 500°C, 520°C or 550°C) for 4h to 5h (such as 4h, 4.5h or 5h), and the second sintering stage can be kept at 750°C to 900°C (such as 750°C, 780°C, 800°C, 820°C, 850°C, 880°C or 900°C) for 8h to 15h (such as 8h, 10h, 12h or 15h), and then cooled to 200°C to 220°C (such as 200°C, 205°C, 210°C, 215°C or 220°C).

[0056] The heating rate and cooling rate of the sintering process can be 1°C / min to 12°C / min (such as 1°C / min, 2°C / min, 3°C / min, 4°C / min, 5°C / min, 6°C / min, 7°C / min, 8°C / min, 9°C / min, 10°C / min, 11°C / min or 12°C / min, etc.). In some preferred embodiments, the heating rate and cooling rate of the sintering process can be 5°C / min to 10°C / min.

[0057] The sintering may be performed in an oxygen atmosphere. For example, the sintering may be performed under a condition where the oxygen partial pressure is 0.01 to 1 standard atmosphere, for example, the oxygen partial pressure during sintering may be 0.02, 0.06, 0.08, 0.1, 0.2, 0.4 or 0.8 standard atmospheres.

[0058] After cooling to 200-220°C, cool to room temperature, then grind and sieve.

[0059] As above, the present invention adopts a liquid phase method to prepare a precursor of a nickel source coated on waste positive electrode particles. Compared with the high-temperature solid phase nickel supplementation process of directly adding nickel oxide or hydroxide, the nickel source is more likely to be in close contact with the waste positive electrode particles, and the nickel element is more likely to diffuse into the waste positive electrode material, and the nickel dispersion is more uniform, and the electrochemical performance is better. In the traditional solid phase sintering nickel supplementation process, the waste positive electrode material has a smaller contact area with the nickel source, the reactant contact is poor, and it is difficult to diffuse uniformly between high nickel and low nickel particles, which is not conducive to nickel diffusion, resulting in poor electrochemical performance. In addition, the present invention uses Ni-MOF as a Ni source. During the hydrothermal reaction process, Ni-MOF is more likely to be complexed on the surface of the particles to form a uniform nickel source shell layer relative to an inorganic nickel source. In the subsequent high temperature treatment process, there are more nickel diffusion channels, which is more conducive to uniform dispersion. In addition, relative to traditional pyrometallurgical and wet recovery, the method provided by the present invention has the advantages of simple process, low cost, environmental friendliness, and reusability after regeneration.

[0060] Accordingly, the present invention provides a regenerated positive electrode material, which is obtained by treating waste positive electrode material with the recycling method of any one of the aforementioned embodiments.

[0061] The regenerated positive electrode material has a higher nickel content than the waste positive electrode material and has electrochemical properties such as higher specific capacity.

[0062] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0063] Example 1

[0064] This embodiment provides a method for recovering positive electrode materials from waste lithium-ion batteries, comprising the following steps:

[0065] S1: will contain NCM111(LiNi 0.33 Co 0.33 Mn 0.33 The waste battery bags of O2) positive electrode materials are disassembled under an inert atmosphere and the positive electrode sheets are obtained by separation.

[0066] S2: The positive electrode sheet was calcined at 550°C for 2h to make the powder fall off the current collector. The powder was collected, ground and sieved (400 mesh) to obtain the waste positive electrode material powder (waste NCM111 powder, the SEM image of which is shown in FIG. Figure 1 shown).

[0067] S3: Disperse 0.027 mol Ni(NO3)2 and 0.027 mol BDC in 30 ml DMF solution and stir evenly to obtain a mixed solution. Add 0.1 mol waste NCM111 powder to the mixed solution and stir for 20 min, then transfer to a polytetrafluoroethylene hydrothermal reactor, keep warm at 120 ° C for 16 h, and then filter, wash and dry to obtain Ni-MOF-coated waste NCM111 precursor.

[0068] S4: The above cathode material precursor was mixed with Li2CO3 (3% excess) and then transferred into an oxygen atmosphere furnace. Under the condition of oxygen partial pressure of 0.01 standard atmosphere, the temperature was raised to 450°C at 10°C / min and kept for 4h, then raised to 900°C at 10°C / min and kept for 8h, then cooled to 300°C at 10°C / min, cooled to room temperature, ground and sieved to obtain R-NCM622 (LiNi 0.6 Co 0.2 Mn 0.2 O2) regenerated positive electrode material (the SEM image of the regenerated positive electrode material is as shown in Figure 2 As shown, the "R" in "R-NCM622" stands for "regeneration", the same below).

[0069] Example 2

[0070] This embodiment provides a method for recovering positive electrode materials from waste lithium-ion batteries, comprising the following steps:

[0071] S1: will contain NCM111(LiNi 0.33 Co 0.33 Mn 0.33 The waste battery bags of O2) positive electrode materials are disassembled under an inert atmosphere and the positive electrode sheets are obtained by separation.

[0072] S2: The positive electrode sheet was calcined at 550° C. for 2 h to allow the powder to fall off the current collector. The powder was collected, ground and sieved (400 mesh) to obtain waste positive electrode material powder (waste NCM111 powder).

[0073] S3: Disperse 0.047 mol NiCl2 and 0.047 mol BDC in 50 ml DMF solution and stir evenly to obtain a mixed solution. Then add 0.1 mol waste NCM111 powder to the mixed solution and stir for 60 min, then transfer to a polytetrafluoroethylene hydrothermal reactor, keep warm at 180 ° C for 8 h, and then filter, wash and dry to obtain Ni-MOF coated waste NCM111 precursor.

[0074] S4: The above cathode material precursor was mixed with LiOH (8% excess) and then transferred into an oxygen atmosphere furnace. Under the condition of oxygen partial pressure of 1 standard atmosphere, the temperature was raised to 550°C at 5°C / min and kept for 4 hours, then raised to 850°C at 5°C / min and kept for 15 hours, then cooled to 300°C at 5°C / min, cooled to room temperature, ground and sieved to obtain R-NCM811 (LiNi 0.8 Co 0.1 Mn 0.1 O2) regenerates the positive electrode material.

[0075] Example 3

[0076] This embodiment provides a method for recovering positive electrode materials from waste lithium-ion batteries, comprising the following steps:

[0077] S1: will contain NCM523(LiNi 0.5 Co 0.2 Mn 0.3 The waste battery bags of O2) positive electrode materials are disassembled under an inert atmosphere and the positive electrode sheets are obtained by separation.

[0078] S2: The positive electrode sheet was calcined at 550° C. for 2 h to allow the powder to fall off the current collector. The powder was collected, ground and sieved (400 mesh) to obtain waste positive electrode material powder (waste NCM523 powder).

[0079] S3: Disperse 0.04 mol Ni(SO4)2 and 0.04 mol BDC in 40 ml DMF solution and stir evenly to obtain a mixed solution. Then add 0.1 mol waste NCM523 powder to the mixed solution and stir for 40 min, then transfer to a polytetrafluoroethylene hydrothermal reactor, keep warm at 150°C for 12 h, and then filter, wash and dry to obtain Ni-MOF coated waste NCM523 precursor.

[0080] S4: The above cathode material precursor was mixed with LiOH (5% excess) and then transferred into an oxygen atmosphere furnace. Under the condition of oxygen partial pressure of 1 standard atmosphere, the temperature was raised to 500°C at 5°C / min and kept for 5h, then raised to 750°C at 5°C / min and kept for 12h, then cooled to 300°C at 5°C / min, cooled to room temperature, ground and sieved to obtain R-NCM90 (LiNi 0.9 Co 0.4 Mn 0.6 O2) regenerates the positive electrode material.

[0081] Comparative Example 1

[0082] This comparative example provides a method for recovering positive electrode materials from waste lithium-ion batteries, comprising the following steps:

[0083] S1: will contain NCM111(LiNi 0.33 Co 0.33 Mn 0.33 The waste battery bags of O2) positive electrode materials are disassembled under an inert atmosphere and the positive electrode sheets are obtained by separation.

[0084] S2: The positive electrode sheet was calcined at 550° C. for 2 h to allow the powder to fall off the current collector. The powder was collected, ground and sieved (400 mesh) to obtain waste positive electrode material powder (waste NCM111 powder).

[0085] S3: 0.1 mol of waste NCM111 powder was mixed with 0.27 mol of NiO and Li2CO3 (3% excess) and then transferred into an oxygen atmosphere furnace. Under the condition of oxygen partial pressure of 1 standard atmosphere, the temperature was raised to 450°C at 10°C / min and kept at this temperature for 6 h, then raised to 900°C at 10°C / min and kept at this temperature for 8 h, then cooled to 300°C at 10°C / min, cooled to room temperature, ground and sieved to obtain R-NCM622 (LiNi 0.6 Co 0.2 Mn 0.2 O2) regenerated positive electrode material (its SEM image is as follows Figure 3 shown).

[0086] Comparative Example 2

[0087] This comparative example provides a method for recovering positive electrode materials from waste lithium-ion batteries, comprising the following steps:

[0088] S1: will contain NCM111(LiNi 0.33 Co 0.33 Mn 0.33 The waste battery bags of O2) positive electrode materials are disassembled under an inert atmosphere and the positive electrode sheets are obtained by separation.

[0089] S2: The positive electrode sheet was calcined at 550° C. for 2 h to allow the powder to fall off the current collector. The powder was collected, ground and sieved (400 mesh) to obtain waste positive electrode material powder (waste NCM111 powder).

[0090] S3: 0.1 mol of waste NCM111 powder was mixed with 0.027 mol of Ni(OH)2 and LiOH (8% excess) and then transferred into an oxygen atmosphere furnace. Under the condition of oxygen partial pressure of 1 standard atmosphere, the temperature was raised to 550°C at 5°C / min and kept for 4 hours, then raised to 850°C at 5°C / min and kept for 15 hours, then cooled to 300°C at 5°C / min, cooled to room temperature, ground and sieved to obtain R-NCM811 (LiNi 0.8 Co 0.1 Mn0.1 O2) regenerates the positive electrode material.

[0091] Test example

[0092] The regenerated positive electrode materials obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were weighed with a conductive agent (Super P) and a binder (5% PVDF dissolved in NMP) at a mass ratio of 90:5:5 and placed in a stirring box; the stirring box was placed in a homogenizer with a set program to mix the materials, and then evenly coated on a 16μm aluminum foil by a coating machine, the coating thickness was controlled at 0.25mm, and a positive electrode sheet with a diameter of 14mm was obtained after drying, cutting, weighing and extrusion. Metal lithium was used as the negative electrode, and a CR2032 button cell was assembled using LiPF6 / EC / EMC electrolyte and PE diaphragm.

[0093] After the button cell was placed for 10 hours, it was placed on a blue battery tester (CT2001C) for charge and discharge cycle performance test. The test conditions were set as: 25°C, 2.8V~4.3V, and the button half-cell was activated by cycling at 0.1C / 0.1C for 3 weeks, and then cycled at 1C / 1C for 200 weeks to examine the specific capacity and cycle performance of the positive electrode material. The results are shown in Table 1.

[0094] Table 1 Performance test results

[0095]

[0096]

[0097] It can be seen from Table 1 that the regenerated positive electrode material obtained by the method provided by the present invention has better 0.1C first discharge capacity, 0.1C first charge and discharge efficiency and cycle performance, which indicates that the method provided by the present invention can effectively realize the recycling of waste positive electrode materials.

[0098] In summary, the recycling method provided by the present invention has simple process, low cost, and is environmentally friendly, and can regenerate waste positive electrode materials to obtain reusable regenerated positive electrode materials. The method adopts a method of first preparing an organic nickel source shell layer on the surface of the waste positive electrode material, and then performing lithium supplementation sintering. Compared with directly adding nickel oxide or hydroxide during the nickel supplementation process, the nickel source can be dispersed more evenly on the surface of the waste positive electrode material, obtain a larger contact area, and is also conducive to making the contact between the nickel source and the waste positive electrode material closer, and the resulting regenerated positive electrode material has better electrochemical properties.

[0099] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A method for recovering positive electrode materials, characterized in that: The method comprises the following steps: preparing an organic nickel source shell layer on the surface of waste positive electrode material to obtain a positive electrode material precursor; mixing the positive electrode material precursor with a lithium source and then sintering to obtain a regenerated positive electrode material.

2. The recycling method according to claim 1, characterized in that: The waste positive electrode material is a layered structure.

3. The recycling method according to claim 1, characterized in that: The waste positive electrode material comprises at least one of waste nickel cobalt manganese oxide positive electrode material, waste nickel cobalt aluminum oxide positive electrode material and waste lithium cobalt oxide positive electrode material; And / or, the organic nickel source shell layer is a Ni-MOF material having a metal organic framework structure.

4. The recycling method according to any one of claims 1 to 3, characterized in that: The preparation of the organic nickel source shell layer comprises: mixing the waste positive electrode material and the raw material for preparing the organic nickel source shell layer and then performing a hydrothermal reaction; The preparation raw materials include nickel salt, organic ligand and organic solvent.

5. The recycling method according to claim 4, characterized in that: The nickel salt includes at least one of Ni(NO3)2, NiCl2, Ni(CH3COO)2 and Ni(SO4)2; and / or, the organic ligand comprises at least one of terephthalic acid, phthalic acid, 2,5-dihydroxyterephthalic acid and trimesic acid; And / or, the organic solvent comprises N,N-dimethylformamide.

6. The recycling method according to claim 4, characterized in that: The hydrothermal reaction is carried out at 120°C to 180°C for 8h to 16h.

7. The recycling method according to claim 1, characterized in that: The lithium source includes at least one of LiOH, Li2CO3, LiNO3 and CH3COOLi.

8. The recycling method according to claim 1, characterized in that: The sintering includes a first sintering stage and a second sintering stage; wherein, the first sintering stage is to keep the temperature at 450℃~550℃ for 4h~5h, and the second sintering stage is to keep the temperature at 750℃~900℃ for 8h~15h, and then cool down to 200℃~220℃.

9. The recycling method according to claim 8, characterized in that: The heating rate and cooling rate of the sintering process are both 1℃ / min~12℃ / min; and / or, sintering is performed in an oxygen atmosphere; Preferably, the heating rate and cooling rate during the sintering process are both 5°C / min to 10°C / min; Preferably, the sintering is performed under the condition that the oxygen partial pressure is 0.01 to 1 standard atmosphere.

10. A regenerated positive electrode material, characterized in that: The regenerated positive electrode material is obtained by treating waste positive electrode material with the recovery method described in any one of claims 1 to 9.

Citation Information

Patent Citations

  • A ternary cathode material with high conductivity and a preparation method thereof

    CN109244449A

  • Preparation method of trimetallic MOF-derived ternary cathode material

    CN109585835A

  • Metal organic framework material and preparation method and application thereof

    CN113444253A

  • Lithium ion battery positive electrode material uniformly coated with MOF (Metal Organic Framework) and preparation method of lithium ion battery positive electrode material

    CN114188536A

  • Li (Ni1 / 2Mn3 / 2) 1-xMxO4-yNy and preparation and application thereof

    CN116102079A