Surface modified diaphragm and preparation method thereof

Through nano Al2O3 surface modification and pre-radiation treatment, combined with ceramic particle coating, the problem of unstable separator graft reaction is solved, the hydrophilicity and wettability of the lithium-ion battery separator is improved, and the battery ratio is significantly improved. Cyclic performance.

CN118943644AActive Publication Date: 2024-11-12GUIZHOU MEILING POWER SUPPLY CO LTD
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411183864.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-11-12
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The graft modification treatment of existing lithium-ion battery separators is not thorough, resulting in unstable grafting reaction of functional monomers, affecting the hydrophilicity and wettability of the separators, and thus limiting the electrochemical performance and durability of the lithium-ion battery. .

Method used

NanoAl2O3 surface modification and pre-radiation treatment methods are used to treat inorganic ceramic particles through silane coupling agent to form stable graft groups, and ceramic particles are coated on the surface of the membrane to enhance the hydrophilicity and wettability of the membrane. .

Benefits of technology

It significantly improves the hydrophilicity and wettability of the separator, improves the magnification and circulation performance of the lithium-ion battery, and enhances the compatibility between the separator and the electrode material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118943644A_ABST
    Figure CN118943644A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a surface modified diaphragm in the technical field of lithium ion batteries, and the preparation method comprises the following steps: S1, surface modification of nano Al2O3: preparing nano Al2O3 into a suspension, dissolving a silane coupling agent in ethanol, dropwise adding into the suspension at a certain speed, reacting in an inert gas environment, filtering, washing, and drying to obtain the surface modified diaphragm; after the reaction is completed, washing and drying the Al2O3 precipitate to obtain primarily modified nano Al2O3; adding the preliminarily modified nano Al2O3 into a mixed solvent of concentrated sulfuric acid and concentrated nitric acid, and after the reaction is completed, washing and drying the precipitate to obtain modified nano Al2O3 with free radical functional groups; s2, pre-radiating the base material; s3, performing surface grafting treatment on the diaphragm; and S4, coating of ceramic particles: dissolving the modified nano Al2O3, adding a binder to obtain ceramic particle slurry, and coating the graft modified diaphragm with the ceramic particle slurry to obtain the surface modified diaphragm. The hydrophilic property and the wettability of the diaphragm base material are improved, and the rate and the cycle performance of the battery are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to a surface modified diaphragm and a preparation method thereof. Background Art

[0002] Lithium-ion battery separator is one of the key components of lithium-ion batteries. The separator can maintain the relative position of the battery during use, prevent the positive and negative electrodes from directly contacting and short-circuiting, and provide a channel for the smooth migration of lithium ions during the charging and discharging process. The chemical stability, thermal stability, mechanical strength, porosity, etc. of lithium-ion battery separators have an important impact on the performance, safety and life of lithium-ion batteries.

[0003] Diaphragm radiation grafting is a method for preparing battery diaphragms using radiation grafting technology. It refers to the process of generating active points in polymer diaphragm materials through high-energy radiation and grafting functional monomers onto these active points, thereby giving the diaphragm new chemical and physical properties. Diaphragm radiation grafting can significantly improve the hydrophilicity and wettability of the diaphragm, facilitate the transmission of ions, improve the electrochemical performance of lithium-ion batteries, and also help increase the durability of the diaphragm in different environments, improve the compatibility of the diaphragm with other components such as electrode materials, and optimize the overall performance of the battery. However, most of the grafting modification treatments in the prior art are directly grafted on the surface of the diaphragm or on the surface of the inorganic ceramic material. The surface of the diaphragm or the surface of the inorganic ceramic material is not treated in any way, resulting in an incomplete grafting reaction of the functional monomer. The diaphragm pre-radiation treatment method used in this application not only makes the connection structure formed by the sinking group and the grafting group on the surface of the inorganic ceramic particles more stable, but also provides sinking particles and incompletely reacted sinking groups that further improve the hydrophilicity and wettability of the diaphragm substrate. Summary of the invention

[0004] The present invention aims to provide a surface-modified diaphragm and a method for preparing the same, which not only makes the connection structure formed by the trapping group and the grafting group on the surface of the inorganic ceramic particles more stable, but also the provided trapping particles and incompletely reacted trapping groups further enhance the hydrophilicity and wettability of the diaphragm substrate.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing a surface modified diaphragm comprises the following steps:

[0007] S1. Surface modification of nano-Al2O3: Prepare nano-Al2O3 into a suspension, dissolve a silane coupling agent in ethanol, and drop it into the suspension at a certain speed, react under an inert gas environment, and after the reaction is completed, wash and dry the Al2O3 precipitate to obtain preliminary modified nano-Al2O3; add the preliminary modified nano-Al2O3 into a mixed solvent of concentrated sulfuric acid and concentrated nitric acid, and after the reaction is completed, wash and dry the precipitate to obtain modified nano-Al2O3 with free radical functional groups;

[0008] S2, substrate pre-irradiation: the radiation bag is filled with inert gas, the diaphragm is sealed in the radiation bag, and the sealed bag is placed in the radiation field and then taken out;

[0009] S3, membrane surface grafting treatment: adding organic solvent, solvent, concentrated sulfuric acid and reaction inhibitor to the irradiated membrane, passing inert gas at room temperature, and then reacting under water bath heating conditions. After the reaction is completed, washing and drying are performed to obtain a grafted modified membrane;

[0010] S4. Coating of ceramic particles: dissolve the modified nano-Al2O3 and add a binder to obtain a ceramic particle slurry, and apply the ceramic particle slurry on the grafted modified diaphragm to obtain a surface modified diaphragm.

[0011] Working principle and beneficial effects of the present invention:

[0012] After S1 of the present application is treated with a coupling agent, a large number of surface active functional groups exist on the surface of the inorganic ceramic particles, which is conducive to their combination with the pre-irradiation treated substrate. The free radical group is an oxidizing group, which is conducive to improving the hydrophilicity of nano Al2O3; S2 pre-irradiation substrate promotes the coating and hydrophilicity of ceramic diaphragm; S3 irradiated PE diaphragm will produce alkyl radicals, allyl radicals and polyolefin radicals. After adding grafting monomers to methanol, the free radicals generated under the action of the catalyst react with the radiation-generated free radicals to form new products. The new product refers to the combination of the groups on both sides to form water, grafted copolymers and other products. The branched structure formed by the chemical reaction enables the free radical monomer molecules of the irradiated PE diaphragm to be combined with the main chain. Compared with the original diaphragm, the grafted diaphragm is more conducive to surface coating and has better adhesion properties.

[0013] The diaphragm pre-radiation treatment method used in the present application not only makes the connection structure formed by the trapping group and the grafted group on the surface of the inorganic ceramic particles more stable, but the provided trapping particles and incompletely reacted trapping groups also further enhance the hydrophilicity and wettability of the diaphragm substrate, significantly improving the rate and cycle performance of the battery.

[0014] Optimally, S1 dries the nano-Al2O3, adds ethanol, and ultrasonically disperses it into a nano-Al2O3 suspension, heats it to 40-70°C, and connects it to a condensation reflux device.

[0015] Optimally, the silane coupling agent is KH570, which is added dropwise to the nano-Al2O3 suspension at a rate of 2 to 3 ml / min, and reacted for 12 to 24 hours in an inert gas environment. After the reaction is completed, the Al2O3 precipitate is washed 3 to 5 times with anhydrous ethanol and dried to obtain the initially modified nano-Al2O3.

[0016] Optimally, S1 is added with a mixed solvent of concentrated sulfuric acid: concentrated nitric acid in a volume ratio of 3:1, and reacted at 60-80°C for 12-24h. After the reaction is completed, the Al2O3 precipitate is washed 3-5 times with anhydrous ethanol and dried to obtain modified nano-Al2O3 with free radical functional groups.

[0017] Optimally, S2 radiation uses Co60-γ rays, the radiation dose is 50-150kGy, the radiation time is 4-12h, the radiation electron beam is 0.5-2MeV, the radiation electron current is 0.5-5mA, the inert gas is nitrogen or argon, the diaphragm is made of PE or PP material, and the thickness is 6-15um.

[0018] Optimally, the organic solvent is oleic acid or acrylic acid or hydroxymethyl acrylic acid, the solvent is deionized water or methanol, and the reaction inhibitor is one or more of copper sulfate, ammonium ferrous sulfate or metal salts.

[0019] Optimally, S3 is introduced with inert gas at room temperature for 20 to 30 minutes, and then reacted in a water bath for 4 to 6 hours. After the reaction is completed, it is washed 3 to 5 times with a mixed solvent of permanent deionized water + ethanol, and dried for 8 to 10 hours to obtain a grafted modified diaphragm.

[0020] Optimally, deionized water is added to S3 to dissolve the modified nano-Al2O3, and a lithium polyacrylate binder is added, and ultrasonic dispersion is performed to obtain a modified nano-Al2O3 ceramic particle slurry.

[0021] Optimally, S4 uses a scraper to coat the modified nano-Al2O3 ceramic particle slurry on one side of the grafted modified membrane, and after drying, coats the other side of the grafted modified membrane in the same manner. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 is the rate performance diagram of the diaphragm;

[0023] Figure 2 The cycle performance diagram is shown in Figure 2. DETAILED DESCRIPTION

[0024] The following is further described in detail through specific implementation methods:

[0025] Example 1 (membrane substrate + nano-Al2O3 with only pre-irradiation):

[0026] Substrate pre-irradiation: This radiation uses Co60-γ rays, the radiation dose is 50-150kGy, the radiation time is 4-12h, the radiation electron beam is 0.5-2MeV, the radiation electron current is 0.5-5mA, the inert gas is nitrogen or argon, the diaphragm is made of PE or PP material, and the thickness is 6-15um;

[0027] Before starting the equipment, soak the cut diaphragms in acetone for 12 hours, deionized water for 12 hours, and finally wash with deionized water, dry, and put into radiation bags, fill with inert gas and seal in radiation polyethylene bags. Then, place the sealed bags in the radiation field, take them out after 4-12 hours of radiation, and store them in a freeze drying box.

[0028] Coating of ceramic particles: add 13.50g of nano-Al2O3 to 300ml of deionized water, stir for 12h, and then ultrasonically disperse for 1h, add 1.5g of lithium polyacrylate binder, stir for 4h, and then ultrasonically disperse for 30min to obtain Al2O3 ceramic particle slurry; use a scraper to coat the slurry on one side of the diaphragm, dry the prepared diaphragm in a vacuum oven at 70°C for 8h, and then coat the other side in the same way to obtain the diaphragm of Example 1.

[0029] Example 2 (modified nano-Al2O3 coating + diaphragm pre-irradiation):

[0030] Substrate pre-irradiation: This radiation uses Co60-γ rays, the radiation dose is 50-150kGy, the radiation time is 4-12h, the radiation electron beam is 0.5-2MeV, the radiation electron current is 0.5-5mA, the inert gas is nitrogen or argon, the diaphragm is made of PE or PP material, and the thickness is 6-15um;

[0031] Before starting the equipment, soak the cut diaphragms in acetone for 12 hours, deionized water for 12 hours, and finally wash with deionized water, dry, and put into radiation bags, fill with inert gas and seal in radiation polyethylene bags. Then, place the sealed bags in the radiation field, take them out after 4-12 hours of radiation, and store them in a freeze drying box.

[0032] Surface modification of nano-Al2O3: Dry 100g of nano-Al2O3 at 100℃ for 12h, place in a flask, add 350ml of ethanol, and ultrasonically disperse for 30min to form a nano-Al2O3 suspension, heat to 40-70℃, and connect to a condensation reflux device. Dissolve 1.14g of silane coupling agent KH570 in 50ml of ethanol, add it dropwise to the nano-Al2O3 suspension at a rate of 2ml / min, and react for 12-24h under an inert gas environment. After the reaction is completed, wash the Al2O3 precipitate with anhydrous ethanol for 3-5 times, and dry at 60℃ to obtain the initially modified nano-Al2O3;

[0033] Place the preliminarily modified nano-Al2O3 in a flask, add 200 ml of a mixed solvent of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, react at 60-80°C for 12-24 hours, wash the Al2O3 precipitate with anhydrous ethanol for 3-5 times after the reaction is completed, and dry at 60°C to obtain modified nano-Al2O3 with free radical functional groups;

[0034] Coating of ceramic particles: 13.50 g of modified nano-Al2O3 was added to 300 ml of deionized water, stirred for 12 h, and then ultrasonically dispersed for 1 h. 1.5 g of lithium polyacrylate binder was added, stirred for 4 h, and then ultrasonically dispersed for 30 min to obtain a modified nano-Al2O3 ceramic particle slurry.

[0035] Coating of ceramic particles: add 13.50g of modified nano-Al2O3 to 300ml of deionized water, stir for 12h, and then ultrasonically disperse for 1h, add 1.5g of lithium polyacrylate binder, stir for 4h, and then ultrasonically disperse for 30min to obtain modified nano-Al2O3 ceramic particle slurry; use a scraper to coat the slurry on one side of the diaphragm, dry the prepared diaphragm in a vacuum oven at 70°C for 8h, and then coat the other side in the same way to obtain the diaphragm of Example 2.

[0036] Example 3 (technical solution of this application: modified nano-Al2O3 coating + diaphragm pre-irradiation + diaphragm surface grafting treatment):

[0037] Substrate pre-irradiation: This radiation uses Co60-γ rays, the radiation dose is 50-150kGy, the radiation time is 4-12h, the radiation electron beam is 0.5-2MeV, the radiation electron current is 0.5-5mA, the inert gas is nitrogen or argon, the diaphragm is made of PE or PP material, and the thickness is 6-15um;

[0038] Before starting the equipment, soak the cut diaphragms in acetone for 12 hours, deionized water for 12 hours, and finally wash with deionized water, dry, and put into radiation bags, fill with inert gas and seal in radiation polyethylene bags. Then, place the sealed bags in the radiation field, take them out after 4-12 hours of radiation, and store them in a freeze drying box.

[0039] Add 10.0g of irradiated PE membrane to a mixed solvent of 250ml methanol + 250ml 0.8mol / L concentrated sulfuric acid + 150ml oleic acid + 10ml 0.0004mol / L copper sulfate, introduce inert gas at room temperature for 20-30min, and then react in a water bath for 4-6h. After the reaction is completed, wash with a mixed solvent of permanent deionized water + ethanol for 3-5 times, and dry at 60℃ for 8-10h to obtain the grafted modified membrane;

[0040] Surface modification of nano-Al2O3: Dry 100g of nano-Al2O3 at 100℃ for 12h, place in a flask, add 350ml of ethanol, and ultrasonically disperse for 30min to form a nano-Al2O3 suspension, heat to 40-70℃, and connect to a condensation reflux device. Dissolve 1.14g of silane coupling agent KH570 in 50ml of ethanol, add it dropwise to the nano-Al2O3 suspension at a rate of 2ml / min, and react for 12-24h under an inert gas environment. After the reaction is completed, wash the Al2O3 precipitate with anhydrous ethanol for 3-5 times, and dry at 60℃ to obtain the initially modified nano-Al2O3;

[0041] Place the preliminarily modified nano-Al2O3 in a flask, add 200 ml of a mixed solvent of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, react at 60-80°C for 12-24 hours, wash the Al2O3 precipitate with anhydrous ethanol for 3-5 times after the reaction is completed, and dry at 60°C to obtain modified nano-Al2O3 with free radical functional groups;

[0042] Coating of ceramic particles: add 13.50g of modified nano-Al2O3 to 300ml of deionized water, stir for 12h, and then ultrasonically disperse for 1h, add 1.5g of lithium polyacrylate binder, stir for 4h, and then ultrasonically disperse for 30min to obtain modified nano-Al2O3 ceramic particle slurry; use a scraper to coat the slurry on one side of the diaphragm, dry the prepared diaphragm in a vacuum oven at 70°C for 8h, and then coat the other side in the same way to obtain the diaphragm of Example 3.

[0043] Example 4 (nano-Al2O3+diaphragm pre-irradiation+diaphragm surface grafting treatment):

[0044] Substrate pre-irradiation: This radiation uses Co60-γ rays, the radiation dose is 50-150kGy, the radiation time is 4-12h, the radiation electron beam is 0.5-2MeV, the radiation electron current is 0.5-5mA, the inert gas is nitrogen or argon, the diaphragm is made of PE or PP material, and the thickness is 6-15um;

[0045] Before starting the equipment, soak the cut diaphragms in acetone for 12 hours, deionized water for 12 hours, and finally wash with deionized water, dry, and put into radiation bags, fill with inert gas and seal in radiation polyethylene bags. Then, place the sealed bags in the radiation field, take them out after 4-12 hours of radiation, and store them in a freeze drying box.

[0046] Add 10.0g of irradiated PE membrane to a mixed solvent of 250ml methanol + 250ml 0.8mol / L concentrated sulfuric acid + 150ml oleic acid + 10ml 0.0004mol / L copper sulfate, introduce inert gas at room temperature for 20-30min, and then react in a water bath for 4-6h. After the reaction is completed, wash with a mixed solvent of permanent deionized water + ethanol for 3-5 times, and dry at 60℃ for 8-10h to obtain the grafted modified membrane;

[0047] Coating of ceramic particles: add 13.50g of nano-Al2O3 to 300ml of deionized water, stir for 12h, and then ultrasonically disperse for 1h, add 1.5g of lithium polyacrylate binder, stir for 4h, and then ultrasonically disperse for 30min to obtain Al2O3 ceramic particle slurry; use a scraper to coat the slurry on one side of the diaphragm, dry the prepared diaphragm in a vacuum oven at 70°C for 8h, and then coat the other side in the same way to obtain the diaphragm of Example 4.

[0048] Example 5 (modified nano-Al2O3 coating + diaphragm):

[0049] Surface modification of nano-Al2O3: Dry 100g of nano-Al2O3 at 100℃ for 12h, place in a flask, add 350ml of ethanol, and ultrasonically disperse for 30min to form a nano-Al2O3 suspension, heat to 40-70℃, and connect to a condensation reflux device. Dissolve 1.14g of silane coupling agent KH570 in 50ml of ethanol, add it dropwise to the nano-Al2O3 suspension at a rate of 2ml / min, and react for 12-24h under an inert gas environment. After the reaction is completed, wash the Al2O3 precipitate with anhydrous ethanol for 3-5 times, and dry at 60℃ to obtain the initially modified nano-Al2O3;

[0050] Place the preliminarily modified nano-Al2O3 in a flask, add 200 ml of a mixed solvent of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, react at 60-80°C for 12-24 hours, wash the Al2O3 precipitate with anhydrous ethanol for 3-5 times after the reaction is completed, and dry at 60°C to obtain modified nano-Al2O3 with free radical functional groups;

[0051] Coating of ceramic particles: add 13.50g of modified nano-Al2O3 to 300ml of deionized water, stir for 12h, and then ultrasonically disperse for 1h, add 1.5g of lithium polyacrylate binder, stir for 4h, and then ultrasonically disperse for 30min to obtain modified nano-Al2O3 ceramic particle slurry; use a scraper to coat the slurry on one side of the diaphragm that has not been treated in any way, dry the prepared diaphragm in a vacuum oven at 70°C for 8h, and then coat the other side in the same way to obtain the diaphragm of Example 5.

[0052] The diaphragms prepared in Examples 1 to 5 were subjected to rate performance and cycle tests. Figure 1 and Figure 2 As shown, from Figure 1 and Figure 2 It can be seen that the surface-modified ceramic diaphragm for lithium-ion batteries prepared in Example 3 with pre-radiation grafting is superior to the diaphragms in Example 1, Example 2, Example 4, and Example 5 in terms of rate performance and number of cycles. That is, the present application further improves the hydrophilicity and wettability of the diaphragm substrate, and significantly improves the rate and cycle performance of the battery.

Claims

1. A method for preparing a surface-modified diaphragm, characterized in that: The following steps are included: S1. Surface modification of nano-Al2O3: Prepare nano-Al2O3 into a suspension, dissolve a silane coupling agent in ethanol, and drop it into the suspension at a certain speed, react under an inert gas environment, and after the reaction is completed, wash and dry the Al2O3 precipitate to obtain preliminary modified nano-Al2O3; add the preliminary modified nano-Al2O3 into a mixed solvent of concentrated sulfuric acid and concentrated nitric acid, and after the reaction is completed, wash and dry the precipitate to obtain modified nano-Al2O3 with free radical functional groups; S2, substrate pre-irradiation: the radiation bag is filled with inert gas, the diaphragm is sealed in the radiation bag, and the sealed bag is placed in the radiation field and then taken out; S3, membrane surface grafting treatment: adding organic solvent, solvent, concentrated sulfuric acid and reaction inhibitor to the irradiated membrane, passing inert gas at room temperature, and then reacting under water bath heating conditions. After the reaction is completed, washing and drying are performed to obtain a grafted modified membrane; S4. Coating of ceramic particles: dissolve the modified nano-Al2O3 and add a binder to obtain a ceramic particle slurry, and apply the ceramic particle slurry on the grafted modified diaphragm to obtain a surface modified diaphragm.

2. The method for preparing a surface modified diaphragm according to claim 1, characterized in that: S1: After drying the nano-Al2O3, add ethanol and ultrasonically disperse it into a nano-Al2O3 suspension, heat it to 40-70°C, and connect it to a condensation reflux device.

3. The method for preparing a surface modified diaphragm according to claim 2, characterized in that: The silane coupling agent is KH570, which is added dropwise to the nano-Al2O3 suspension at a speed of 2-3 ml / min, and reacted for 12-24 hours in an inert gas environment. After the reaction is completed, the Al2O3 precipitate is washed 3-5 times with anhydrous ethanol and dried to obtain the initially modified nano-Al2O3.

4. The method for preparing a surface modified diaphragm according to claim 3, characterized in that: S1 is added with a mixed solvent of concentrated sulfuric acid and concentrated nitric acid in a volume ratio of 3:1, and reacted at 60-80°C for 12-24h. After the reaction is completed, the Al2O3 precipitate is washed 3-5 times with anhydrous ethanol and dried to obtain modified nano-Al2O3 with free radical functional groups.

5. The method for preparing a surface modified diaphragm according to claim 4, characterized in that: S2 radiation uses Co60-γ rays, the radiation dose is 50-150kGy, the radiation time is 4-12h, the radiation electron beam is 0.5-2MeV, the radiation electron current is 0.5-5mA, the inert gas is nitrogen or argon, the diaphragm is made of PE or PP material, and the thickness is 6-15um.

6. The method for preparing a surface-modified diaphragm according to claim 5, characterized in that: The organic solvent is oleic acid or acrylic acid or hydroxymethyl acrylic acid, the solvent is deionized water or methanol, and the reaction inhibitor is one or more of copper sulfate, ammonium ferrous sulfate or metal salts.

7. The method for preparing a surface modified diaphragm according to claim 6, characterized in that: S3 is introduced with inert gas at room temperature for 20 to 30 minutes, and then reacted in a water bath for 4 to 6 hours. After the reaction is completed, it is washed 3 to 5 times with a mixed solvent of permanent deionized water + ethanol, and dried for 8 to 10 hours to obtain a grafted modified diaphragm.

8. The method for preparing a surface modified diaphragm according to claim 7, characterized in that: S3 adds deionized water to dissolve the modified nano-Al2O3, adds lithium polyacrylate binder, and ultrasonically disperses to obtain modified nano-Al2O3 ceramic particle slurry.

9. The method for preparing a surface modified diaphragm according to claim 8, characterized in that: S4 uses a scraper to coat the modified nano-Al2O3 ceramic particle slurry on one side of the grafted modified diaphragm, and after drying, coats the other side of the grafted modified diaphragm in the same way.

10. A surface-modified diaphragm obtained by the method for preparing a surface-modified diaphragm according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Radiating modification lithium ion battery diaphragm and preparation method thereof

    CN104882581A

  • Lithium ion battery diaphragm coating and application thereof

    CN115000627A

  • Battery diaphragm, preparation method thereof and battery

    CN115275514A

  • Ceramic diaphragm for lithium ion battery and preparation method of ceramic diaphragm

    CN118507992A

  • Separator for cell

    JP1980105963A