Substrate and preparation method thereof

The ceramic plate is prepared by opening holes in raw ceramic sheets, laminated pressing and sintering, and filling the ceramic plate with conductors, which solves the problem of shrinkage and impedance of the probe card substrate in high-temperature tests and high-frequency tests, and achieves high mechanical Strength, low impedance and stable substrate for probe cards and 2D/3D packaging.

CN118946004APending Publication Date: 2024-11-12QIANYI SEMICON (SHANGHAI) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411016429.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-27
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing probe card substrates are prone to warping and poor flatness in the baking process, shrinkage occurs during high-temperature testing, and the conductivity and process limitations of the multi-layer ceramic substrates lead to high impedance instability during high-frequency testing.

Method used

The ceramic plate is prepared by opening holes of raw ceramic sheets, laminated pressing and sintering, and the conductor is filled in the straight holes of the ceramic plates. The substrate is formed by seed layer deposition and re-wiring layer, and isostatic bonding and double-sided electroplating are reduced. impedance.

Benefits of technology

The prepared substrate has high mechanical strength, good planarity, is not easy to shrink during high and low temperature tests, has a low impedance and is stable, meets the needs of high-frequency testing, and is suitable for 2D/3D packaging and other substrate production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946004A_ABST
    Figure CN118946004A_ABST
Patent Text Reader

Abstract

The invention discloses a substrate and a preparation method thereof, and the method comprises the steps: 1, providing a plurality of green ceramic chips, forming holes in each green ceramic chip, and enabling the green ceramic chips to form through holes; 2, filling the through holes in the green ceramic chip in the step 1 with a filler; step 3, laminating and pressing the plurality of green ceramic chips filled with the through holes in the step 2, and aligning the through holes in every two adjacent green ceramic chips one by one, so that the through holes in the plurality of green ceramic chips are connected to form a straight hole; 4, the raw ceramic chips laminated in the step 3 are subjected to isostatic pressing bonding and then sintered to obtain a sintered ceramic plate, and the filler in the straight holes of the ceramic plate is decomposed; 5, seed layer deposition is carried out on the two faces of the ceramic plate, and the straight holes are filled with conductors; and 6, manufacturing a rewiring layer on the surface of the ceramic plate to form the substrate. The substrate prepared by the method is high in mechanical strength, good in flatness and not easy to expand and shrink, and can meet the requirements of a probe card during high-frequency testing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of probe cards, and in particular to a probe card substrate and a preparation method thereof. Background Art

[0002] With the rapid development of the semiconductor industry, a large number of chips need to be tested for performance before packaging, and this process requires the use of probe cards. As the main component of the probe card, the substrate (adapter board) is currently mostly made of a multi-layered organic substrate (MLO) or a multi-layered ceramic substrate (MLC).

[0003] When making the MLO substrate, the multi-layer organic substrate will undergo multiple baking processes, resulting in warping and poor flatness of the MLO substrate after it is completed. In addition, during the high-temperature test of the probe card, the MLO often shrinks, which hinders the effective implementation of the high-temperature test of the probe card. When using MLC to make an adapter board, the MLC usually has a circuit inside. Due to the conductivity of the conductive paste (usually silver paste) used to make the circuit and the limitations of the MLC manufacturing process, the probe card (adapter card prepared by the MLC+PI rewiring process) has high impedance and unstable defects when responding to high-frequency testing. Summary of the invention

[0004] In order to overcome the defects in the prior art, an embodiment of the present invention provides a substrate and a preparation method thereof. The substrate prepared by the preparation method has the advantages of high mechanical strength, good flatness, and not easy to expand or shrink during high and low temperature tests. At the same time, its impedance is low and stable, which can meet the requirements of the probe card during high-frequency testing.

[0005] The present application discloses a method for preparing a substrate, comprising the following steps:

[0006] Step 1: providing a plurality of green ceramic sheets, and drilling a hole on each green ceramic sheet to form a through hole on the green ceramic sheet;

[0007] Step 2: Filling the through holes on the green ceramic sheet in step 1 with a filler;

[0008] Step 3: stacking and pressing the multiple green ceramic sheets after the through holes are filled in step 2, and aligning the through holes on two adjacent green ceramic sheets one by one, so that the through holes on the multiple green ceramic sheets are connected to form straight holes;

[0009] Step 4: the green ceramic sheets after lamination and pressing in step 3 are bonded by isostatic pressing and then sintered to obtain a sintered ceramic plate, and the filler in the straight hole of the ceramic plate is decomposed;

[0010] Step 5: depositing a seed layer on both sides of the ceramic plate and filling the straight hole with a conductor;

[0011] Step 6: Make a rewiring layer on the surface of the ceramic board to form a substrate.

[0012] Specifically, in step 1, holes are drilled on the green ceramic sheet by laser drilling.

[0013] Specifically, the filler is one or more of black carbon and silica gel.

[0014] Specifically, in step 2, the filler is filled into the through hole by screen printing.

[0015] Specifically, the thickness of the ceramic plate is greater than or equal to 1500 μm.

[0016] Specifically, in step 4, the isostatic pressing temperature is between 70 and 90°C, the pressure is between 20 and 70 MPa, and the holding time is 30 to 60 minutes; the sintering temperature is between 600 and 900°C, the sintering time is 60 to 120 minutes, the heating rate during sintering is between 0.2 and 2°C / min, the sintering atmosphere is nitrogen, and after sintering, the furnace is cooled to room temperature.

[0017] Specifically, in step 5, the metal used for the seed layer is copper, titanium-copper alloy or chromium-copper alloy, and the thickness of the seed layer is between 600 and 2400 nm.

[0018] Specifically, the conductor is filled into the straight hole by double-sided electroplating.

[0019] Specifically, in step 5, after the conductor is filled in the straight hole, the step further includes: annealing the conductor in the straight hole of the ceramic plate, the annealing temperature is between 80 and 150° C., and the annealing time is 10 to 30 minutes.

[0020] The embodiment of the present application also discloses: a substrate, which is prepared by the method described in the embodiment.

[0021] The present invention has at least the following beneficial effects:

[0022] 1. The substrate prepared in this embodiment uses a ceramic plate as a support body, which has the advantages of high mechanical strength, good flatness, and not easy to expand and shrink during high and low temperature tests. At the same time, in addition to setting the conductor in the straight hole, the ceramic plate has no other wiring, and its impedance is reduced and stable, which can meet the needs of the probe card in high-frequency testing. It also has sufficient application scenarios for 2D / 3D packaging and can also be used as the Core (core layer) when making some other substrates.

[0023] 2. This embodiment adopts the method of drilling holes in raw ceramic sheets and then stacking, pressing and sintering them to prepare ceramic plates with straight holes, which reduces the process difficulty of processing long straight holes on ceramic plates. Therefore, ceramic plates with larger thickness can be prepared. At the same time, the production of ceramic plates with smaller hole diameters and smaller hole spacings can be achieved.

[0024] In order to make the above and other purposes, features and advantages of the present invention more obvious and easy to understand, preferred embodiments are specifically cited below and described in detail with reference to the accompanying drawings. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0026] Figure 1 4 is a flow chart of a method for preparing a substrate in an embodiment of the present invention. DETAILED DESCRIPTION

[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0028] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "fixed", and "connected" should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be directly connected or indirectly connected through an intermediate medium, and it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in this application can be understood by specific circumstances.

[0029] In the present invention, unless otherwise clearly specified and limited, a first feature being “above” or “below” a second feature may include the first feature and the second feature being in direct contact, or may include the first feature and the second feature being in contact not directly but through another feature between them. Moreover, a first feature being “above”, “below”, and “above” a second feature includes the first feature being directly above and obliquely above the second feature, or simply indicates that the first feature is higher in level than the second feature. A first feature being “below”, “below”, and “below” a second feature includes the first feature being below and obliquely below the second feature, or simply indicates that the first feature is lower in level than the second feature.

[0030] In the description of this embodiment, it should be understood that the terms "center", "longitudinal", "lateral", "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside", "outside", etc., indicating the orientation or position relationship are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the present application and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as limiting the scope of protection of the present application.

[0031] In addition, the terms "first", "second", etc. are only used to distinguish in description and have no special meaning.

[0032] like Figure 1 As shown, the method for preparing the substrate of this embodiment mainly includes the following steps:

[0033] Step 1: Provide a plurality of raw ceramic sheets, and make holes on each raw ceramic sheet to form through holes on each raw ceramic sheet. Specifically, the raw ceramic sheet of this embodiment adopts LTCC (Low Temperature Co-fired Ceramic), which has a lower dielectric constant. The number and position of through holes on each raw ceramic sheet are preferably the same, and the diameter of the through hole is between 60 and 120 μm. The thickness of a single raw ceramic sheet is between 50 and 120 μm.

[0034] Step 2: Filling the through holes on the green ceramic sheet obtained in step 1 with a filler, wherein the filler can support the through holes in the subsequent pressing process.

[0035] Step 3: The multiple raw ceramic sheets obtained in step 2 are laminated and pressed, and the (multiple) through holes on two adjacent raw ceramic sheets are aligned one by one, so that the through holes on the multiple raw ceramic sheets are connected to form a straight hole. That is, when the multiple raw ceramic sheets are stacked, the through holes of one raw ceramic sheet are aligned with the through holes of the raw ceramic sheets above and below it, and after pressing, the through holes at the same position of the multiple raw ceramic sheets are substantially coaxial, thereby forming a longer straight hole.

[0036] Step 4: The raw ceramic sheets after lamination and pressing in step 3 are bonded by isostatic pressing and then sintered to obtain sintered ceramic plates. During the sintering process, the fillers in the straight holes (or through holes of the raw ceramic sheets) decompose and disappear, thereby forming through holes in the straight holes.

[0037] Step 5: Deposit a seed layer on the two bottom surfaces of the ceramic plate obtained in step 3, and fill the straight holes with a conductor, which may be copper.

[0038] Step 6: According to the design drawings, a rewiring layer is made on the surface of the ceramic board obtained in step 5 to form a substrate. In this step, a rewiring layer can be made on one or both sides of the ceramic board as needed, and the rewiring layers on the two sides are electrically connected through the conductors in the straight holes.

[0039] By adopting the above scheme, the substrate prepared in this embodiment uses a ceramic plate as a support body, which has the advantages of high mechanical strength, good flatness, and not easy to expand and shrink during high and low temperature tests. At the same time, the ceramic plate has no other wiring except for the conductor arranged in the straight hole, and its impedance is reduced and stabilized, which can meet the needs of the probe card during high-frequency testing.

[0040] Specifically, in this embodiment, it is preferred to use laser drilling to make holes in the green porcelain sheet. When using laser to drill holes in the green porcelain sheet, since the green porcelain sheet is relatively soft and has strong toughness, the green porcelain between the holes is not easy to break during laser drilling, so the hole spacing can be designed to be smaller and the hole diameter can also be designed to be smaller.

[0041] Since the present embodiment firstly makes holes in the raw ceramic sheets and then presses and sinters the multiple raw ceramic sheets to form a thicker ceramic plate, when a thicker ceramic plate (for example, a thickness greater than or equal to 1500 μm) needs to be manufactured, the difficulty of making holes will not increase due to the increase in the thickness of the ceramic plate. In other words, compared with the traditional method of making holes in cooked ceramic, the scheme of the present embodiment can produce thicker ceramic plates with lower processing difficulty.

[0042] At the same time, for finished products that require the same thickness of ceramic plates (for example, ceramic plates with a thickness of 50-500μm), this solution is prepared by stacking raw ceramics. Generally speaking, the thickness of raw ceramics is between 50-120μm, and raw ceramics with a thickness of 50μm can be used for drilling. In this way, the pitch can be made smaller. This method can be used in 2D / 3D packaging to further improve the density. The results of this solution have greater advantages compared to the TSV process currently used in 2D / 3D packaging.

[0043] Specifically, the filler in this embodiment can be one or more of black carbon and silica gel. The filler can be filled into the through hole of the green ceramic sheet by screen printing.

[0044] In step 4, the parameters of isostatic bonding are as follows: the isostatic pressing temperature is between 70 and 90°C, the pressure is between 20 and 70 MPa, and the holding time is 30 to 60 minutes. The sintering parameters are as follows: the sintering temperature is between 600 and 900°C, the sintering time is 60 to 120 minutes, the heating rate during sintering is between 0.2 and 2°C / min, the sintering atmosphere is nitrogen, and the furnace is cooled to room temperature after sintering.

[0045] In step 5, a deposited seed layer is made on both sides of the ceramic plate using one of copper, titanium copper alloy or chromium copper alloy. In other words, the metal used in the seed layer is one of copper, titanium copper alloy or chromium copper alloy. The thickness of the seed layer is between 600 and 2400 nm.

[0046] In step 5, a conductor is filled into the straight hole by double-sided electroplating to metalize the straight hole. Specifically, the electroplating parameters are: first electroplating at a current density of 0.08ASD for 30 minutes, and then electroplating at a current density of 0.15ASD for 110 minutes; or, first electroplating at a current density of 0.18ASD for 30 minutes, and then electroplating at a current density of 0.125ASD for 90 minutes. The corresponding selection can be made according to the depth H and diameter L of the straight hole. Preferably, after the conductor (preferably metal copper) is electroplated in the straight hole, the conductor in the straight hole of the ceramic plate is annealed, and the annealing temperature is between 80 and 150°C, and the annealing time is 10 to 30 minutes. Taking the conductor as metal copper as an example, after annealing, the average resistivity of the copper in the straight hole is 50 to 150mΩ. Compared with the average resistivity of the multilayer ceramic substrate made of traditional conductive silver paste as high as 1 to 10Ω, the impedance of the substrate prepared in this embodiment is very low and the impedance is stable.

[0047] Preferably, after step 5 and before step 6, the ceramic plate may be subjected to double-sided mechanical polishing. That is, after the conductor is electroplated in the straight hole of the ceramic plate and before the rewiring layer is made on the surface of the ceramic plate, the ceramic plate is first subjected to double-sided mechanical polishing. Diamond liquid, aluminum oxide and other polishing liquids are used during mechanical polishing, the polishing pressure is between 100 and 500N, and the speed ratio is 40 / 10 or 60 / 30.

[0048] The present invention uses specific embodiments to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. At the same time, for those skilled in the art, according to the idea of ​​the present invention, there will be changes in the specific implementation methods and application scope. In summary, the content of this specification should not be understood as a limitation on the present invention.

Claims

1. A method for preparing a substrate, characterized in that: The following steps are involved: Step 1: providing a plurality of green ceramic sheets, and drilling a hole on each green ceramic sheet to form a through hole on the green ceramic sheet; Step 2: Filling the through holes on the green ceramic sheet in step 1 with a filler; Step 3: stacking and pressing the multiple green ceramic sheets after the through holes are filled in step 2, and aligning the through holes on two adjacent green ceramic sheets one by one, so that the through holes on the multiple green ceramic sheets are connected to form straight holes; Step 4: the green ceramic sheets after lamination and pressing in step 3 are bonded by isostatic pressing and then sintered to obtain a sintered ceramic plate, and the filler in the straight hole of the ceramic plate is decomposed; Step 5: depositing a seed layer on both sides of the ceramic plate and filling the straight hole with a conductor; Step 6: Make a rewiring layer on the surface of the ceramic board to form a substrate.

2. The method for preparing a substrate according to claim 1, characterized in that: In step 1, holes are drilled on the green ceramic sheet by laser drilling.

3. The method for preparing a substrate according to claim 1, characterized in that: The filler is one or more of black carbon and silica gel.

4. The method for preparing a substrate according to claim 1, characterized in that: In step 2, the filler is filled into the through hole by screen printing.

5. The method for preparing a substrate according to claim 1, characterized in that: The thickness of the ceramic plate is greater than or equal to 1500 μm.

6. The method for preparing a substrate according to claim 1, characterized in that: In step 4, the isostatic pressing temperature is between 70 and 90°C, the pressure is between 20 and 70 MPa, and the holding time is 30 to 60 minutes; the sintering temperature is between 600 and 900°C, the sintering time is 60 to 120 minutes, the heating rate during sintering is between 0.2 and 2°C / min, the sintering atmosphere is nitrogen, and after sintering, the furnace is cooled to room temperature.

7. The method for preparing a substrate according to claim 1, characterized in that: In step 5, the metal used for the seed layer is copper, titanium-copper alloy or chromium-copper alloy, and the thickness of the seed layer is between 600 and 2400 nm.

8. The method for preparing a substrate according to claim 1, characterized in that: In step 5, the conductor is filled into the straight hole by double-sided electroplating.

9. The method for preparing a substrate according to claim 8, characterized in that: In step 5, after the conductor is filled in the straight hole, the method further includes: annealing the conductor in the straight hole of the ceramic plate, wherein the annealing temperature is between 80° C. and 150° C., and the annealing time is 10 to 30 minutes.

10. A substrate, characterized in that: Prepared by the method according to any one of claims 1 to 9.