Printed circuit board and deep micropore wall copper plating method thereof
By performing copper depositing, hole filling plating and pulse plating on the printed circuit board, the copper-free and crab legs problems caused by the difficulty of exchange of Chinese medicine in deep micro-blind holes are solved, and the reliability of the hole wall and the uniformity of the copper layer are improved. sex.
Patent Information
- Application Number
- CN202411119779.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-12
AI Technical Summary
During the copper plating process of deep micro-blind holes on printed circuit boards, due to the increase in the number of blind hole interconnection layers and thickness-diameter ratio, it is difficult to exchange potions at the bottom of the blind hole, resulting in no adverse defects such as copper and crab legs in the hole, affecting the reliability of the product sex.
After preparing blind holes and through holes on the printed circuit board, copper deposits are performed first and hole-filled using vertical continuous plating lines for electroplating, the blind hole type is corrected, and the secondary copper deposits are performed, and the plate surface is performed using pulse plating technology Electroplating ensures copper ion exchange efficiency inside and outside the blind hole.
It effectively solves the problem of copper and crab legs in deep microblind holes, improves the reliability of deep microblind hole walls and the uniformity of copper layer, and meets customers' requirements for copper thickness.
Smart Images

Figure CN118946036A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of printed circuit board preparation, in particular to a printed circuit board and a method for copper plating deep micro-hole walls thereof. Background Art
[0002] In today's era, communication technology is developing rapidly, information transmission speed is getting faster and faster, and the development trend of miniaturization, multi-function and high performance of electronic products is becoming more and more obvious, which puts forward higher requirements for dense wiring and signal integrity for printed circuit boards. In this context, high-density interconnection (HDI) technology is gradually applied to printed circuit board design. Deep micro blind vias are beneficial to save space, increase line filling and insertion loss control due to their "zero" residual stub advantage. Among them, the number of interconnected layers of cross-layer blind vias is also increasing, from L1-3 at the beginning, to L1-4, and even L1-5 layers of interconnection have appeared. The blind hole thickness-to-diameter ratio has also gradually increased from about 0.85:1 to 1.2:1, or even higher.
[0003] In the blind hole copper plating process, the exchange of chemicals inside and outside the blind hole is mainly achieved through the circulation and concentration diffusion in the hole. When producing printed circuit boards containing deep micro blind holes, it is difficult to exchange chemicals at the bottom of the blind holes due to the large number of interconnected layers of the blind holes and the high thickness-diameter ratio of the blind holes. In the copper deposition and electroplating process, the concentration of the chemicals changes from high to low from the blind hole mouth to the bottom of the hole, resulting in defects such as no copper in the hole and crab feet in the blind hole, which affects product reliability. Summary of the invention
[0004] The present invention provides a printed circuit board and a method for copper plating the wall of a deep micro-hole thereof, so as to solve the problems existing in the prior art, so that the bottom corners and the hole wall of the deep micro-hole of the printed circuit board are smooth and rounded, effectively solve the problem of no copper and crab feet in the deep micro blind hole, and improve the reliability of the wall of the deep micro-hole.
[0005] In a first aspect, the present invention provides a method for copper plating on the wall of a deep micro-hole of a printed circuit board, comprising:
[0006] After blind holes and through holes are prepared on the printed circuit board, copper deposition is performed to metallize the blind holes and through holes;
[0007] A vertical continuous electroplating line is used to perform hole-filling electroplating on the printed circuit board after the copper deposition to correct the blind hole shape;
[0008] Performing secondary copper deposition on the printed circuit board after the hole filling electroplating;
[0009] The printed circuit board after the secondary copper deposition is subjected to board surface electroplating; the board surface electroplating adopts a pulse electroplating process, and the pulse waveform of the pulse electroplating includes a positive pulse, a negative pulse and a zero pulse in sequence.
[0010] Optionally, the current density ratio of the positive pulse, the negative pulse and the zero pulse is: 1:3:0.
[0011] Optionally, in a pulse cycle, the durations of the positive pulse, the negative pulse and the zero pulse are 120 ms, 6 ms and 5 ms respectively.
[0012] Optionally, the first copper deposition and / or the second copper deposition is horizontal copper deposition.
[0013] Optionally, when performing the first copper deposition and / or the second copper deposition, the flow rate of each chemical tank is in the range of 80L / min-100L / min.
[0014] Optionally, when performing the first copper deposition and / or the second copper deposition, the flow rate of each water jet washing ranges from 80 L / min to 100 L / min.
[0015] Optionally, during the hole-filling electroplating, the hole-filling solution used includes copper sulfate pentahydrate; the concentration range of the copper sulfate pentahydrate is 230 g / L-250 g / L.
[0016] Optionally, during hole filling electroplating, the jet frequency of the jet tube is 40HZ-50HZ.
[0017] Optionally, before copper deposition, the following steps are also included:
[0018] A laser drilling process is used to prepare blind holes and through holes on the printed circuit board.
[0019] In a second aspect, the present invention further provides a printed circuit board, comprising deep microvias; the hole wall copper of the deep microvias is prepared by using any of the above-mentioned methods for copper plating of the hole wall of deep microvias of a printed circuit board.
[0020] The technical solution of the present invention is to perform copper plating once after blind holes and through holes are prepared on a printed circuit board to metalize the blind holes and through holes, and then use a vertical continuous electroplating line to perform hole-filling electroplating on the printed circuit board after the copper plating, so as to make certain modifications to the rough position of the blind hole wall and the bottom corner position to make them round, so as to achieve the purpose of correcting the blind hole shape and preliminarily eliminate the bad crab foot phenomenon at the bottom of the blind hole, and then perform secondary copper plating on the printed circuit board after the hole-filling electroplating, so as to thicken the copper thickness of the blind hole and through hole wall to meet the customer's requirements for copper thickness, and finally perform board surface electroplating on the printed circuit board after the secondary copper plating, and the board surface electroplating adopts a pulse electroplating process, and the pulse electroplating pulse waveform includes positive pulses, negative pulses and zero pulses in sequence, so that the copper ions in the electroplating solution can diffuse freely in the short zero pulse time, and the copper ions in the low current area in the blind hole are supplemented, so as to improve the copper ion supply inside and outside the blind hole, improve the solution exchange efficiency in the blind hole, effectively solve the problem of no copper and crab feet in the deep micro blind hole, and improve the reliability of the deep micro hole wall.
[0021] It should be understood that the contents described in this section are not intended to identify the key or important features of the embodiments of the present invention, nor are they intended to limit the scope of the present invention. Other features of the present invention will become easily understood through the following description. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] In order to more clearly illustrate the technical solutions in the embodiments of the present invention, the following briefly introduces the drawings required for use in the description of the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work.
[0023] Figure 1 A flow chart of a method for copper plating deep micro-hole walls of a printed circuit board provided by an embodiment of the present invention;
[0024] Figure 2 The effect diagram of the blind hole wall state after hole-filling electroplating provided by the embodiment of the present invention;
[0025] Figure 3 This is a rendering of the state of the blind hole wall after the board surface is electroplated according to an embodiment of the present invention. DETAILED DESCRIPTION
[0026] In order to enable those skilled in the art to better understand the scheme of the present invention, the technical scheme in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0027] It should be noted that the terms "first", "second", etc. in the specification and claims of the present invention and the above-mentioned drawings are used to distinguish similar objects, and are not necessarily used to describe a specific order or sequence. It should be understood that the numbers used in this way can be interchanged where appropriate, so that the embodiments of the present invention described herein can be implemented in an order other than those illustrated or described herein.
[0028] As information transmission speeds become faster and faster, HDI technology is gradually being applied to printed circuit board design, and the number of interconnected layers of deep micro blind vias is also increasing. In the blind via copper plating process, the exchange of liquid inside and outside the blind via is mainly achieved through the circulation and concentration diffusion in the via. As the number of interconnected layers and the thickness-diameter ratio of deep micro blind vias increase, it will become difficult to exchange liquid at the bottom of the blind via.
[0029] In the copper deposition and electroplating process, the concentration of the solution changes from high to low from the hole mouth to the bottom of the blind hole, which makes the material adsorption and copper deposition chemical reaction in the corner area at the bottom of the blind hole insufficient, resulting in poor copper deposition effect, resulting in the phenomenon of no copper in the blind hole. In addition, due to insufficient solution exchange at the bottom of the blind hole, during the electroplating process, the electroplating rate of the corner area at the bottom of the blind hole is slower than that of the blind hole wall and the middle area at the bottom of the blind hole, resulting in the formation of coating cracks in the corner area at the bottom of the blind hole, namely, the blind hole crab feet. At the same time, when blind holes and through holes are formed by laser drilling process, the rough hole walls of the blind holes and through holes will also increase the risk of blind hole crab feet.
[0030] In order to solve the above problems, this embodiment provides a method for copper plating on the wall of deep micro-holes of a printed circuit board. Figure 1 A flowchart of a method for copper plating deep micro-hole walls of a printed circuit board provided by an embodiment of the present invention, referring to Figure 1 As shown, the deep micro-hole wall copper plating method of the printed circuit board comprises:
[0031] S110, after blind holes and through holes are prepared on the printed circuit board, copper deposition is performed to metalize the blind holes and through holes.
[0032] Among them, the copper deposition in one time can be, but is not limited to, a horizontal copper deposition process or a vertical copper deposition process. In an optional embodiment, the copper deposition in one time adopts a horizontal copper deposition process, so as to improve the coating coverage, make the inner copper and the hole copper have better bonding strength, and increase the copper deposition rate, thereby improving the quality and preparation efficiency of the printed circuit board.
[0033] It can be understood that the production line steps of the horizontal copper deposition process include the following: feeding → bulking → flushing sewage → water jet washing 1 → water jet washing 2 → degumming → flushing sewage → water jet washing 3 → water jet washing 4 → neutralization → water jet washing 5 → ultrasonic water washing → water jet washing 6 → (closed) high-pressure water washing → clean water washing → hole filling → flushing sewage → water jet washing 7 → water jet washing 8 → micro-etching → water jet washing 9 → water jet washing 10 → water jet washing 11 → pre-impregnation → activation → flushing sewage → water jet washing 12 → water jet washing 13 → water jet washing 14 → reduction → water jet washing 15 → water jet washing 16 → water jet washing 17 → copper deposition → water jet washing 18 → water jet washing 19 → water jet washing 20 → water jet washing 21 → drying → lowering the board. Among them, in the steps of bulking, degumming, neutralization, hole filling, micro-etching, pre-impregnation, activation, reduction and copper deposition, the reaction cylinder is filled with a certain flow of medicine to achieve horizontal copper deposition.
[0034] Since the number of interconnected layers and the thickness-diameter ratio of the deep micro blind hole are relatively large, it is difficult to exchange the solution at the bottom of the blind hole. In an optional embodiment, the flow rate of each solution tank and water jet washing can be increased to enhance the exchange inside and outside the blind hole, thereby providing sufficient material components at the bottom of the blind hole for adsorption or chemical reaction, thereby achieving a good copper deposition effect.
[0035] Optionally, when performing a copper deposition, the value range of the medicine flow rate of each medicine tank is 80L / min-100L / min. In the prior art, the flow rate of each medicine tank in the copper deposition process is generally 40L / min-50L / min, which makes it difficult to exchange the medicine at the bottom of the deep micro blind hole with a large number of interconnected layers and a relatively large thickness, resulting in poor copper deposition effect. It is understandable that the larger the medicine flow rate of each medicine tank, the more sufficient the medicine exchange at the bottom of the deep micro hole, so that sufficient material components can be provided for the bottom of the blind hole to achieve a good copper deposition effect. However, the larger the medicine flow rate of each medicine tank, for example, when the medicine flow rate exceeds 100L / min, the impact force of the medicine is too strong, which is easy to change the position of the printed circuit board, thereby causing the phenomenon of skewed board, stuck board or stacked board, affecting the copper deposition effect. In addition, when the medicine flow rate is too large, the medicine cannot be fully utilized, resulting in waste of resources and increased production costs. Therefore, this embodiment limits the range of the flow rate of each solution tank during copper deposition to 80L / min-100L / min. It can reduce the occurrence of deflection, jamming or overlapping of plates while ensuring sufficient solution exchange at the bottom of the deep microholes to effectively deposit copper at the bottom of the deep microholes, thereby improving the copper deposition effect and achieving the effect of saving resources and controlling production costs.
[0036] Optionally, when performing a copper deposition, the flow rate of each water jet washing ranges from 80L / min to 100L / min. In the prior art, the flow rate of each water jet washing step in the copper deposition process is generally 40L / min-50L / min, so that the medicine at the bottom of the deep micro blind hole cannot be rinsed clean before entering the next medicine tank, thereby affecting the process effect of the next medicine tank. It can be understood that the larger the flow rate of each water jet washing, the less medicine residue at the bottom of the deep micro hole, so that when the printed circuit board enters the next medicine tank, the process effect of the medicine tank is better, so that a good copper deposition effect can be achieved. However, the larger the flow rate of the water jet washing, for example, when the flow rate exceeds 100L / min, the impact force of the water jet washing is too strong, which is easy to change the position of the printed circuit board, thereby causing the phenomenon of skewed board, stuck board or stacked board, affecting the copper deposition effect. In addition, when the flow rate is too large, there will be a problem of wasting resources and increasing production costs. Therefore, this embodiment limits the range of the flow rate of each water jet washing during one copper deposition to 80L / min-100L / min. It can reduce the occurrence of deflection, jamming or overlapping of boards while ensuring that the medicine in each medicine tank is rinsed clean and copper is effectively deposited at the bottom of deep microholes, thereby improving the copper deposition effect and achieving the effect of saving resources and controlling production costs.
[0037] In an optional embodiment, when copper deposition is performed once, the flow rate of the flushing sewage is in the range of 4L / min-6L / min. It is understandable that the flow rate of the flushing sewage in the prior art is generally controlled at 2L / min-4L / min. In this embodiment, by increasing the flow rate of the flushing sewage to 4L / min-6L / min, the activation liquid at the bottom of the blind hole can be cleaned, and palladium-containing precipitates are avoided from remaining at the bottom of the blind hole, thereby improving the reliability of the copper layer at the bottom of the blind hole.
[0038] In an optional embodiment, before performing a copper deposition, the method for copper plating of deep micro-hole walls of a printed circuit board further includes the following process steps: cutting → making inner layer circuits → pressing → outer layer drilling, etc. These process steps can be implemented using existing process steps, and this embodiment will not describe them in detail.
[0039] In an optional embodiment, the outer layer drilling step includes: using a laser drilling process to prepare blind holes and through holes on the printed circuit board.
[0040] The laser drilling process includes but is not limited to carbon dioxide laser drilling and / or ultraviolet laser drilling. The laser drilling process can make the blind hole or through hole have a higher aspect ratio and a higher hole accuracy. In addition, since the drill bit of the laser drilling does not physically contact the printed circuit board, it can reduce the wear problem of the printed circuit board, as well as the possibility of cracking and delamination. At the same time, the high speed of laser drilling is conducive to improving the preparation efficiency of the printed circuit board and shortening the preparation cycle.
[0041] S120, using a vertical continuous electroplating line, the printed circuit board after a copper deposition is filled with electroplating to correct the blind hole shape.
[0042] in, Figure 2 The effect diagram of the blind hole wall state after the hole filling electroplating provided by the embodiment of the present invention is shown in FIG. Figure 2 As shown, the hole filling electroplating adopts a high-copper and low-acid solution composition ratio, which can improve the copper plating effect of the blind hole, modify the rough position of the hole wall and the corner position of the bottom of the deep micro blind hole, and make it round, thereby correcting the blind hole shape and preliminarily eliminating the crab foot defect at the bottom of the blind hole.
[0043] Optionally, during hole-filling electroplating, the hole-filling solution used includes copper sulfate pentahydrate, and the concentration range of copper sulfate pentahydrate is 230g / L-250g / L, thereby increasing the content of copper ions in the hole-filling solution to increase the supply of copper ions in the blind hole, thereby enhancing the easy exchange inside and outside the blind hole, providing sufficient material components for the bottom of the blind hole, and achieving a good hole-filling electroplating effect.
[0044] Optionally, during hole-filling electroplating, the jet frequency of the jet tube is 40HZ-50HZ, thereby increasing the supply of copper ions in the blind hole by increasing the jet frequency of the jet tube, thereby enhancing the easy exchange inside and outside the blind hole, providing sufficient material components for the bottom of the blind hole, and achieving a good hole-filling electroplating effect.
[0045] It should be noted that the current density and time of the via-filling electroplating can be determined according to the process requirements of the printed circuit board, and this embodiment does not specifically limit this. In an optional embodiment, the current density of the via-filling electroplating is 16ASF-18ASF, and the time of the via-filling electroplating is 60 minutes.
[0046] It is understandable that in deep micro-holes with large interconnection layers and relatively large thickness-diameter ratio, the diameter of the blind hole is generally 8mil-12mil, which is much larger than the diameter of the conventional blind hole (3mil-5mil). Therefore, it is impossible to plate the copper thickness required by the customer in one time by filling the hole electroplating. In addition, in the case of coexistence of through holes and blind holes, because the deep plating ability of filling the hole electroplating is low, the copper thickness of the through hole generally cannot be electroplated to meet the customer's requirements in one time during the filling hole electroplating process. Therefore, it is necessary to perform electroplating again so that the copper thickness of the through hole and the copper thickness of the blind hole meet the customer's requirements.
[0047] S130, performing secondary copper deposition on the printed circuit board after the via-filling electroplating.
[0048] The secondary copper deposition may be, but is not limited to, a horizontal copper deposition process or a vertical copper deposition process. In an optional embodiment, the primary copper deposition adopts a horizontal copper deposition process, thereby improving the coating coverage and copper deposition rate, thereby improving the quality and production efficiency of the printed circuit board.
[0049] In an optional embodiment, the process parameters of the secondary copper deposition are the same as the process parameters of the primary copper deposition. Please refer to the description of the relevant part in the primary copper deposition process, which will not be repeated here.
[0050] In this embodiment, through the secondary copper plating, on the one hand, the board surface dirt and oxidation that may be generated after the hole filling electroplating can be removed, and on the other hand, the hole wall of the deep micro blind hole can be further modified, thereby further reducing the phenomenon of poor copper plating at the bottom of the blind hole that may occur during the primary copper plating process.
[0051] S140, electroplating the printed circuit board after the secondary copper deposition.
[0052] Among them, the plate surface electroplating adopts pulse electroplating process, and the pulse electroplating pulse waveform includes positive pulse, negative pulse and zero pulse in sequence. Pulse electroplating refers to electroplating using pulse power supply instead of DC power supply. During the electroplating process, the electrodeposition process can be changed in a wide range by controlling parameters such as waveform, frequency, on-off ratio and average current density, so as to obtain a coating with certain characteristics in a certain plating solution. Positive pulse refers to the pulse current as positive current, negative pulse refers to the pulse current as negative current, and zero pulse refers to the pulse current as zero. In the positive pulse stage, copper is deposited by normal electroplating on the printed circuit board. In the negative pulse stage, the high current area is dissolved by anodic dissolution, thereby playing a leveling role to improve the distribution of the coating thickness and make the coating uniform. In the zero pulse stage, since the pulse current is zero, the copper ions diffuse freely, and the copper ions in the low current area in the hole are supplemented, thereby improving the distribution uniformity of copper plating on the hole wall and ensuring the reliability of the hole wall.
[0053] By using a vertical continuous electroplating line to electroplate the printed circuit board after secondary copper deposition, copper can be plated uniformly on the entire board surface (including the inside of the hole and the surface of the board). The electroplating solution generally uses a high-acid and low-copper solution component ratio, combined with pulse current equipment and special electroplating additives, which can improve the deep plating ability of the through-hole, thereby improving the copper plating effect of the through-hole wall.
[0054] In an optional embodiment, the current density ratio of the positive pulse, the negative pulse and the zero pulse is 1:3:0, so that in the positive pulse stage, the formation rate of the copper nucleus is much greater than the growth rate of the original crystal, thereby forming a deposition layer with a finer grain structure, improving the quality of copper plating. In the negative pulse stage, due to the large current density of the negative pulse, the copper ions near the cathode are consumed at a very fast rate, and the copper ions are transferred to the cathode, so that the concentration of copper ions in the diffusion layer is restored, and the concentration polarization is eliminated, thereby effectively improving the thickness distribution of the floating layer. In the zero pulse stage, since the current density is 0, the copper ions can diffuse freely, thereby increasing the supply of copper ions inside and outside the blind hole, and then improving the copper plating effect of the hole wall.
[0055] It is understandable that the time ratio of the positive pulse, the negative pulse and the zero pulse can be set according to the requirements for the electroplating efficiency and the electroplating effect. In an optional embodiment, the time ratio of the positive pulse, the negative pulse and the zero pulse is 120ms, 6ms and 5ms respectively, so that the electroplating efficiency and the electroplating effect can be taken into account.
[0056] It should be noted that the current density of the board surface electroplating and the ratio of the electroplating solution can be determined according to the process requirements of the printed circuit board, and this embodiment does not specifically limit this. In an optional embodiment, the current density of the board surface electroplating is 13ASF-26ASF, the content of copper sulfate pentahydrate in the electroplating solution is 60g / L-90g / L, and the content of sulfuric acid is 110ml / L-140ml / L.
[0057] Figure 3 The effect diagram of the blind hole wall state after the plate surface electroplating provided by the embodiment of the present invention is shown in FIG. Figure 3 As shown, after copper plating the deep micro-hole walls of the printed circuit board using the deep micro-hole copper plating method provided in this embodiment, the blind hole walls are smooth and round, and there is no copper-free and crab-leg problem in the blind hole.
[0058] Based on the same concept, this embodiment also provides a printed circuit board, including: deep micro-holes; the hole wall copper of the deep micro-holes adopts the deep micro-hole wall copper plating method of the printed circuit board provided by any of the above embodiments. Therefore, the printed circuit board provided by the embodiment of the present invention has the beneficial effects of the deep micro-hole wall copper plating method of the printed circuit board provided by any of the above embodiments, and the similarities can be referred to the above description.
[0059] The above specific implementations do not constitute a limitation on the protection scope of the present invention. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for copper plating of deep micro-hole walls of a printed circuit board, characterized in that: include: After blind holes and through holes are prepared on the printed circuit board, copper deposition is performed to metallize the blind holes and through holes; A vertical continuous electroplating line is used to perform hole-filling electroplating on the printed circuit board after the copper deposition to correct the blind hole shape; Performing secondary copper deposition on the printed circuit board after the hole filling electroplating; Electroplating the printed circuit board after the secondary copper deposition; The plate surface electroplating adopts a pulse electroplating process, and the pulse waveform of the pulse electroplating includes a positive pulse, a negative pulse and a zero pulse in sequence.
2. The method for copper plating deep micro-hole walls of a printed circuit board according to claim 1, characterized in that: The current density ratio of the positive pulse, the negative pulse and the zero pulse is 1:3:
0.
3. The method for copper plating deep micro-hole walls of a printed circuit board according to claim 2, characterized in that: In a pulse cycle, the durations of the positive pulse, the negative pulse and the zero pulse are 120 ms, 6 ms and 5 ms respectively.
4. The method for copper plating deep micro-hole walls of a printed circuit board according to claim 1, characterized in that: The first copper deposition and / or the second copper deposition is horizontal copper deposition.
5. The method for copper plating deep micro-hole walls of a printed circuit board according to claim 1, characterized in that: When performing the primary copper deposition and / or the secondary copper deposition, the flow rate of each chemical tank is in the range of 80L / min-100L / min.
6. The method for copper plating deep micro-hole walls of a printed circuit board according to claim 1, characterized in that: When performing the first copper deposition and / or the second copper deposition, the flow rate of each water jet washing ranges from 80L / min to 100L / min.
7. The method for copper plating deep micro-hole walls of a printed circuit board according to claim 1, characterized in that: When performing hole-filling electroplating, the hole-filling solution used includes copper sulfate pentahydrate; the concentration range of the copper sulfate pentahydrate is 230g / L-250g / L.
8. The method for copper plating deep micro-hole walls of a printed circuit board according to claim 1, characterized in that: When performing hole filling electroplating, the jet frequency of the jet tube is 40HZ-50HZ.
9. The method for copper plating deep micro-hole walls of a printed circuit board according to claim 1, characterized in that: Before copper deposition, it also includes: A laser drilling process is used to prepare blind holes and through holes on the printed circuit board.
10. A printed circuit board, characterized in that: It comprises deep micro-holes; the hole wall copper of the deep micro-holes is prepared by the deep micro-hole wall copper plating method of a printed circuit board as described in any one of claims 1-9.
Citation Information
Cited By
Method and apparatus for manufacturing HDI circuit board, and printed circuit board
WO2026166096A1