Method for improving wettability of carrier transport layer and application thereof
By adjusting the surface roughness of the substrate, the super-immersion of the carrier transport layer is improved, and the structural defects caused by insufficient carrier transport layer are solved, and the performance and manufacturing yield of the optoelectronic devices are significantly improved.
Patent Information
- Application Number
- CN202410998174.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2024-06-02
- Filing Date
- 2024-07-24
- Publication Date
- 2024-11-12
AI Technical Summary
During the preparation of thin-film optoelectronic devices by solution method, insufficient wetting of the carrier transport layer leads to defects in the hole or pinhole structure, seriously reducing device performance, and existing methods are difficult to change the intrinsic properties of carrier transport materials without changing the intrinsic properties of carrier transport materials Super infiltration is achieved.
By regulating the surface roughness of the substrate, increasing the roughness of the carrier transport layer, and using the conformal effect between the nano-scale rough structure and the carrier transport layer, the super-immersion of the carrier transport layer is improved and structural defects are reduced.
It effectively reduces the pinhole and hole density in large-area photoelectric functional films, improves the film manufacturing yield and device performance, and significantly improves the photoelectric conversion efficiency and short-circuit current of perovskite solar cells.
Smart Images

Figure CN118946221A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of preparing thin-film photoelectric devices by a solution method, and specifically relates to a method for improving the wettability of a carrier transport layer and an application thereof. Background Art
[0002] Among many emerging optoelectronic materials, such as perovskites, organic matter and quantum dots, they have shown broad application prospects due to their advantages such as solution processing, excellent optoelectronic properties and low cost. These materials have become a research hotspot for scientific researchers. Under laboratory conditions, the highest certified efficiencies of perovskite solar cells and perovskite LEDs reached 26.1% and 32%, respectively. In particular, the performance of perovskite solar cells is very close to that of commercial crystalline silicon cells. Therefore, to realize the commercialization of thin-film optoelectronic devices prepared by solution method, it is necessary to develop scalable production technology to prepare large-area optoelectronic material films.
[0003] In order to commercialize thin-film optoelectronic devices prepared by solution method, it is necessary to develop large-area optoelectronic material thin film technology that can be mass-produced. However, as the area of the optoelectronic functional layer increases, the probability of structural defects such as holes or pinholes in the film increases, resulting in serious leakage or carrier recombination, significantly reducing device performance. The generation of these structural defects is closely related to the wettability of the carrier transport layer. Superwetting surfaces have higher surface energy than ordinary wetting surfaces, which makes the solution on its surface tend to spread outward automatically and exclude gas adsorption, thereby effectively inhibiting the generation of structural defects. However, it is more difficult to obtain superwetting surfaces than ordinary wetting surfaces. It is usually necessary to add special functional groups on the surface of carrier transport materials to enhance the affinity between the substrate and the target optoelectronic material.
[0004] These chemical methods may change the chemical or physical properties of the surface of the carrier transport material, making it difficult to simultaneously meet the requirements of the intrinsic properties of the carrier transport material and the superwetting surface state. Therefore, it is necessary to develop new methods to prepare optoelectronic thin films by achieving superwetting without changing the intrinsic properties of the carrier transport material. This will help solve the structural defect problems (such as pinholes or holes) encountered in the preparation of large-area optoelectronic material films and promote the commercialization of optoelectronic devices. Summary of the invention
[0005] In order to solve the problem that holes or pinholes are easily generated in the process of preparing large-area optoelectronic functional films due to the inability of the optoelectronic functional materials and the carrier transport layer to fully infiltrate, thereby causing the performance of the device to decline, the present invention provides a method for improving the wettability of the carrier transport layer and its application. The method improves the wettability of the bottom substrate by increasing the surface roughness of the bottom substrate without changing the intrinsic properties of the contact material (carrier transport layer) to achieve a super-wetting state. The method focuses on assisting the preparation of large-area high-quality perovskite films, reducing the density of pinholes and buried holes in large-area optoelectronic functional films, and improving the film manufacturing yield.
[0006] The characteristic of this technology is that the wettability of the carrier transport layer can be improved to achieve a super-wetting state by only regulating the surface roughness of the substrate on which the carrier transport layer is deposited. There is no need to dope or surface treat the carrier transport layer itself, so that it can contact the upper optoelectronic functional layer material with its intrinsic properties and reach the optimal state.
[0007] To achieve the above object, the present invention provides the following technical solutions:
[0008] The method for improving the wettability of the carrier transport layer provided by the present invention includes increasing the roughness of the carrier transport layer by increasing the surface roughness of the substrate, thereby improving the wettability of the carrier transport layer; the method specifically includes the following steps:
[0009] 1) Obtain a flat substrate;
[0010] 2) constructing a nanoscale rough structure on the surface of the substrate obtained in step 1), adjusting the roughness value of the nanoscale rough structure to an appropriate range, and then depositing a carrier transport layer on the nanoscale rough structure. Due to the conformal effect between the nanoscale rough structure and the carrier transport layer, the roughness of the deposited carrier transport layer is changed by adjusting the roughness value of the nanoscale rough structure, thereby improving the wettability of the carrier transport layer.
[0011] Preferably, in step 1), the substrate includes a glass substrate, a polyimide (PI) substrate, a polyethylene terephthalate (PET) substrate, a polyethylene naphthalate (PEN) substrate, and a transparent conductive film substrate on which indium tin oxide (ITO) or fluorine-doped tin oxide (FTO) is deposited on the surface of the above substrate.
[0012] In some specific embodiments, step 1) further includes: pre-treating the substrate to remove pollutants such as oil stains on the surface of the substrate.
[0013] Preferably, in step 2), the method of constructing the nanoscale rough structure includes: depositing a nanoparticle film on the substrate surface, or changing the surface roughness of the substrate by post-processing to obtain a nanoscale rough surface.
[0014] The method for depositing the nanoparticle film includes but is not limited to: a solution method (depositing the nanoparticle suspension onto a substrate by at least one of a scraping, spin coating, spraying, screen printing, slit coating, etc.), sputtering deposition, electrochemical deposition, physical vapor deposition, chemical vapor deposition, and a sol-gel method.
[0015] The post-processing methods include surface post-processing methods such as acid etching, electron beam etching, laser etching, plasma etching, etc.
[0016] Further preferably, the nanoparticle film material includes but is not limited to: inorganic nanoparticles (such as: metal particles such as gold, silver, platinum, etc.; metal oxides such as nickel oxide, titanium dioxide, zinc oxide, tin oxide, zirconium dioxide, hafnium dioxide, aluminum oxide, copper oxide, molybdenum oxide, tungsten oxide, vanadium oxide, strontium oxide, etc.), carbon-based nanoparticles (such as carbon nanotubes, graphene, etc.).
[0017] The roughness range of the nanoscale rough structure is RMS = 2-100 nm (RMS, Root Mean Square).
[0018] The carrier transport layer material is any existing carrier transport layer material.
[0019] In some specific embodiments, the carrier transport layer material includes self-assembled carrier transport materials, organic polymer or small molecule transport materials, organic electron transport materials and other transport materials. Among them, the self-assembled carrier transport material may have the following structural characteristics: (1) containing at least one chemical functional group that can be anchored on the surface of the metal oxide, including phosphonic acid group, bisphosphonic acid group, tripropylphosphonic acid group, cyanovinylphosphonic acid group, benzoic acid group, sulfonic acid group, choline group, aromatic group, carboxylic acid group, hydroxyl group, amine group, sulfur group, silane anchoring group, mercapto group, thiol group, etc.; (2) containing halogen atoms, ether groups, alcohol groups, alkyl groups, aromatic groups, ester groups, aldehyde groups, ketone groups, amide functional groups, nitric acid groups, phosphoric acid groups, sulfide compounds, carboxylic acid groups, amino functional groups, nitrogen-containing heterocyclic compounds (quinoline, benzimidazole, imidazole, pyridine, thiazole, triazacyclopentene, etc.) , nitrogen-containing aromatic compounds (aniline, hydrazine, imidazole, pyridine, pyrrole, thiophene, phenothiazine, carbazole, indolecarbazole, quinoline, isoquinoline, etc.), conjugated benzene molecules, 1,3-dimethoxybenzene, methoxy, dimethylacridine, triphenylamine, naphthalene, benzene ring, Lewis basic sulfur heteroatom, conjugated phenylene, PTZ-CPA, etc., at least one chemical functional group, asymmetric terminal conjugation; (3) including linkers (spacers) of different lengths (such as 2PACz, 3PACz, 4PACz, 5PACz and 6PACz, where PACz refers to carbazole-type phosphoric acid self-assembled molecules) and different carbazole terminal groups (such as H, Me, MeO, F, Cl, Br and I).
[0020] Specifically, the self-assembled carrier transport material can be, for example, Me-4PACz, MeO-2PACz, 2PACz, 4PACz, MeO-4PACz, MeO-6PACz, MeO-4PADBC, Ph-2PACz, 4,3BuPACz, Ph-4PACz, Poly-4PACz, MeO-PhPACz, DMAcPA, MPA-CPA, MPA-Ph-CA, EADR04, TPA-PT-C6, SA-BPP, V1036, Br-4PACz, Br-2EPT, Br-2P ACz, Br-2EPO, Br-2EPSe, DMAcPA, DC-PA, CbzPh, CbzBF, CbzBT, PPA, PPAOMe, 4PADCB, 2PADCB, 2PATPA, Me-2PATPA, DCB-BPA, 3P ATAT-C3, PTZ-CPA, 3PACz, Br-4PADBC, 4dp3PACz, BABBr-C4PA, 2PATPA, Me-2PATPA, MeO-2PATPA, F-2PACz, Cl-2PACz, I-2PACz, F-4PACz, Cl-4PACz, I-4PACz, MPA-Ph-CPA, CbzNap, BCB-C4PA, TPT-C6, TPT-S6, TPT-P6, Spiro-Acid, MC-43, TPA, EADR03, EAD R04, AC-1, AC-3, AC-5, MPA2FPh-BT-BA, MeTPA-CPA, FMPA2FPh-BT-CA, 2FMPA2FPh-BT-CA, PQxD, PQx, TQxD, TQx, MTPA-BA, MPA- CPA, etc.; organic polymer or small molecule hole transport materials may be, for example, PTAA, Poly-TPD, P3HT, c-OTPD, TPD, spiro-OMeTAD, PVK, etc.; organic electron transport materials may be, for example, PC71BM, PC61BM, ICBA, C60, PCBA, MeO-TPD, FPAC60, C60-SAM, DC-PA, CPTA, C9, C60-C6-PA, C60-bis, etc.; other transport materials may be, for example, copper phthalocyanine, nickel phthalocyanine, TPBi, BCP, PEDOT:PSS, etc.
[0021] The method is used in preparing photoelectric thin film materials or perovskite solar cells.
[0022] The principle involved in the present invention:
[0023] 1. The present invention deposits a nanoparticle film with a certain roughness on the surface of a flat substrate, or changes the surface roughness of the substrate by post-processing to obtain a nanoscale rough structure. The roughness value of the substrate can be adjusted by adjusting the preparation parameters of the nanoparticle film. The surface roughness value of the nanoparticle film is determined by the particle size of the nanoparticles (1-100nm) or the particle size after agglomeration, and the roughness range is RMS = 2-100nm.
[0024] 2. Subsequently, a carrier transport layer is further deposited on the nanoscale rough structure. Due to the conformal effect, the roughness of the deposited carrier transport layer can be changed by adjusting the roughness value of the nanoscale rough structure, so that the carrier transport layer reaches a superwetting state (contact angle <10°), and the substrate with the carrier transport layer deposited is used in the subsequent solution method to prepare thin-film optoelectronic devices.
[0025] 3. The mechanism of improving the wettability of the carrier transport layer by surface roughening is as follows: The equilibrium contact angle (θ) of a droplet on a smooth substrate is determined by the following Young's equation:
[0026]
[0027] In the formula, γ SG is the interfacial energy of the solid / gas interface, γ SL is the interfacial energy of the solid / liquid interface, Δγ S is the solid / gas interface (γ SG ) and solid / liquid interface (γ SL ) between the interfaces, γ LG is the interfacial energy of the liquid / gas interface.
[0028] In the Wenzel model, a droplet will form a larger solid / liquid interface area on a rough surface wetted substrate. As the effective area increases, the apparent contact angle decreases (e.g. Figure 1 The relationship between the equilibrium contact angles on a rough surface and a smooth surface can be expressed as follows:
[0029]
[0030] Where θ' is the contact angle on the rough substrate. r is the roughness coefficient, which is defined as the ratio of the effective area of the rough surface (A') to the area of the smooth surface (A). Figure 3 ), the increase of the roughness coefficient r will accelerate the decrease of the contact angle θ' of the rough substrate. Therefore, before depositing the carrier transport layer, constructing a nanoscale rough structure on the substrate and increasing its roughness can improve the wettability of the carrier transport layer and transform the carrier transport layer from the normal wetting state to the super wetting state. The critical value of the roughness coefficient (r0) for the transition between the normal wetting state and the super wetting state is determined by its initial contact angle:
[0031]
[0032] Beneficial effects of the present invention:
[0033] (1) The present invention is applicable to all material systems for preparing optoelectronic functional layers by solution method.
[0034] (2) The present invention can prepare a large-area optoelectronic functional film without pinholes / holes by simply increasing the roughness of the substrate without changing the properties of the material itself.
[0035] (3) The present invention is applicable to a variety of wet preparation technologies for large-area optoelectronic device thin films: scraping, spin coating, spraying, screen printing, slit coating and other methods.
[0036] The present invention can make the carrier transport layer with normal wetting have the characteristics of super-wetting coating by roughening the substrate, so as to prepare a large-area photoelectric functional film without pinholes and holes, and the bonding force between the film and the substrate is significantly enhanced. Taking the solar cell prepared by scraping two-dimensional perovskite as an example, the thin film device prepared on the substrate with nano-scale rough structure has higher comprehensive performance, and the short-circuit current is increased from 11.58mA cm -2 Increased to 18.43 mA cm -2 , the photoelectric conversion efficiency increased from 7.5% to 16.21%. The dark current of the device was significantly reduced, indicating that the leakage of the device was reduced. BRIEF DESCRIPTION OF THE DRAWINGS
[0037] Figure 1 The different wetting states of the perovskite solution on a flat surface and a surface with a nano-scale rough structure;
[0038] Figure 2 The different contact angles of the perovskite solution on a flat surface and a surface with a nanoscale rough structure;
[0039] Figure 3 is the calculation result of the change of substrate contact angle with substrate roughness coefficient;
[0040] Figure 4 The experimental characterization shows the variation trend of the contact angle of the carrier transport layer with the roughness of the nano-scale roughness structure on the substrate surface.
[0041] Figure 5 By NiO xThe nanoparticle film adjusts the roughness of the substrate, increases the wettability of PTAA, Me-4PACz, and MeO-2PACz, and enables the perovskite solution to achieve a self-spreading effect in these three carrier transport layers. The critical roughness for superwetting of the three carrier transport layers of PTAA, Me-4PACz, and MeO-2PACz is 5.3nm, 5.9nm, and 2.1nm, respectively.
[0042] Figure 6 To introduce NiO x Comparison of bubble adsorption effects of three carrier transport layers (PTAA, Me-4PACz, MeO-2PACz) before and after nanoscale rough structure. The rough structure enhances the bubble repulsion effect of the carrier transport layer, which is beneficial to suppress structural defects in optoelectronic device films.
[0043] Figure 7 The bottom scanning electron micrographs of the perovskite films prepared in Examples 1 to 3 and Comparative Examples 1 to 3 show that the film structural defects of Examples 1 to 3 are significantly reduced; the dotted circles are holes or pinholes in the film;
[0044] Figure 8 The cross-sectional scanning electron micrographs of the perovskite films obtained in Examples 1 to 3 and Comparative Examples 1 to 3 show that the film structural defects of Examples 1 to 3 are significantly reduced; the dotted circle indicates the holes at the film / carrier transport layer interface, and the arrow indicates the gap at the film / carrier transport layer interface;
[0045] Fig. 9 Photovoltaic performance of perovskite solar cells with / without nanoscale roughness structure: (ac) current density-voltage curve of the device under illumination, (de) current density-voltage curve of the device in the dark state. DETAILED DESCRIPTION
[0046] The full names and abbreviations of some chemical substances involved in the present invention are as follows:
[0047]
[0048]
[0049] Example 1
[0050] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of poly[bis(4-phenyl)(2,4,6-trimethylphenyl)amine] (PTAA), and the scraping coating of perovskite film is taken as an example, which specifically includes the following steps:
[0051] 1) Pretreatment of transparent ITO conductive substrate: Use ITO conductive glass with transmittance > 85% and square resistance < 10Ω as the substrate, and use detergent, deionized water, acetone, and isopropanol for ultrasonic cleaning for 15 minutes each, blow dry with nitrogen, and then treat with ultraviolet ozone for 15 minutes;
[0052] 2) Preparation of nanoscale rough structure: Prepare 35 mg / mL NiO x aqueous solution and ultrasonically dispersed for 1 h to obtain NiO x The solution was spin-coated on the ITO glass pretreated in step 1) at 1500 rpm for 30 seconds, and then annealed at 150°C for 30 minutes to obtain a NiO surface. x Nanoscale rough structured substrate;
[0053] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x PTAA coating on substrate: 2 mg / mL PTAA solution dissolved in chlorobenzene (CB) was spin-coated on NiO at 6000 rpm. x The nanoscale rough structure is then annealed at 80°C for 10 min to obtain a substrate with a super-wettable carrier transport layer.
[0054] 4) Preparation of perovskite solution: 1.4 M lead iodide (PbI2), 1.68 M methylamine iodide (MAI) and 0.7 M ammonium chloride (NH4Cl) were dissolved in N,N-dimethylformamide (DMF), heated to 70 °C, stirred, and after complete dissolution, 5 μL of 1,4-butanediamine (BDA) solution was added and stirred evenly to obtain (BDA)MA4Pb5I with a concentration of 1.4 M. 16 Perovskite solution;
[0055] 5) Preparation of perovskite film: The substrate with a superwetting carrier transport layer obtained in step 3) is placed on a doctor blade at a temperature of 50°C, and the slit height between the doctor blade and the substrate is 130 μm. The perovskite solution prepared in step 4) is sucked onto the superwetting carrier transport layer of the substrate with a pipette, and the solution is doctored at a speed of 35 mm / s. Hot air is blown to accelerate the evaporation of the solvent, and then annealed at 100°C for 30 min to obtain a large-area perovskite film.
[0056] Example 2
[0057] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of Me-4PACz. Taking the scraping of perovskite film as an example, the following steps are specifically included:
[0058] 1) Same as step 1) in Example 1;
[0059] 2) Preparation of nanoscale rough structure: Prepare 35 mg / mL NiO x aqueous solution and ultrasonically dispersed for 1 h to obtain NiO x The solution was spin-coated on the ITO glass pretreated in step 1) at 1300 rpm for 30 seconds, and then annealed at 150°C for 30 minutes to obtain a NiO surface. x Nanoscale rough structured substrate;
[0060] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x Coating Me-4PACz on the substrate: 0.2 mg / mL Me-4PACz solution dissolved in ethanol was spin-coated on the NiO substrate at 3000 rpm. x The nano-scale rough structure is then annealed at 80°C for 10 min to obtain a substrate with a super-wettable carrier transport layer;
[0061] 4) Preparation of perovskite solution: same as step 4) in Example 1;
[0062] 5) Preparation of perovskite film: same as step 5) in Example 1.
[0063] Example 3
[0064] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of MeO-2PACz. Taking the scraping of perovskite film as an example, the following steps are specifically included:
[0065] 1) Same as step 1) in Example 1;
[0066] 2) Preparation of nanoscale rough structure: Prepare 20 mg / mL NiO x aqueous solution and ultrasonically dispersed for 1 h to obtain NiO x The solution was spin-coated on the ITO glass pretreated in step 1) at 2000 rpm for 30 seconds, and then annealed at 150°C for 30 minutes to obtain a NiO surface. x Nanoscale rough structured substrate;
[0067] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x Coating MeO-2PACz on the substrate: 0.2 mg / mL MeO-2PACz solution dissolved in ethanol was spin-coated on the NiO substrate at 3000 rpm. x The nano-scale rough structure is then annealed at 80°C for 10 min to obtain a substrate with a super-wettable carrier transport layer;
[0068] 4) Preparation of perovskite solution: same as step 4) in Example 1;
[0069] 5) Preparation of perovskite film: same as step 5) in Example 1.
[0070] Example 4
[0071] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of MeO-2PACz, and spin-coated perovskite film is taken as an example, specifically including the following steps:
[0072] 1) Same as step 1) in Example 1;
[0073] 2) Preparation of nano-scale rough structure: same as step 2) in Example 3;
[0074] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x Coating MeO-2PACz on the substrate: same as step 3 of Example 3);
[0075] 4) Preparation of perovskite film: PbI2 / DMF solution with a concentration of 1.2 M was dropped onto the super-wetting substrate prepared in step 3) and spin-coated at 3000 rpm for 30 s; then 60 mg / mL MAI / DMF solution was spin-coated on PbI2 at 3000 rpm for 30 s, and then annealed at 100°C for 40 min to obtain a perovskite film.
[0076] Example 5
[0077] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of MeO-2PACz. The preparation of perovskite film by spraying method is taken as an example, which specifically includes the following steps:
[0078] 1) Same as step 1) in Example 1;
[0079] 2) Preparation of nano-scale rough structure: same as step 2) in Example 3;
[0080] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x Coating MeO-2PACz on the substrate: same as step 3 of Example 3);
[0081] 4) Preparation of perovskite film: (BDA)MA4Pb5I with a concentration of 1.2M 16The perovskite solution was deposited on the substrate prepared in step 3) using a nitrogen gun at a gas pressure of 3 psi at a discharge rate of 1 ml / min, and annealed at 100° C. for 40 min to obtain a large-area two-dimensional perovskite film.
[0082] Example 6
[0083] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of MeO-2PACz. The preparation of perovskite film by screen printing is taken as an example, which specifically includes the following steps:
[0084] 1) Same as step 1) in Example 1;
[0085] 2) Preparation of nano-scale rough structure: same as step 2) in Example 3;
[0086] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x Coating MeO-2PACz on the substrate: same as step 3 of Example 3);
[0087] 4) Preparation of perovskite film: The setting parameters of the screen are: 150T mesh / inch, tension 25N / cm, polyester wire with a diameter of 45mm; printing parameters are: printing speed 150mm / s; printing gap: 3mm; printing pressure: 5kg; (BDA)MA4Pb5I 16 The concentration of the perovskite solution is 1.0M. After printing, it is annealed at 100°C for 40 minutes to obtain a large-area two-dimensional perovskite film.
[0088] Example 7
[0089] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of MeO-2PACz, and the preparation of perovskite film by slit coating method is taken as an example, which specifically includes the following steps:
[0090] 1) Same as step 1) in Example 1;
[0091] 2) Preparation of nano-scale rough structure: same as step 2) in Example 3;
[0092] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x Coating MeO-2PACz on the substrate: same as step 3 of Example 3);
[0093] 4) Preparation of perovskite film: 1.2M (BDA)MA4Pb5I 16The perovskite solution was dripped into a syringe with a discharge rate of 100 μL / min. The superwetting substrate prepared in step 3) was moved at a speed of 10 mm / s, and a wind speed of 20 psi was used. Then, the film was annealed at 100°C for 40 min to obtain a large-area two-dimensional perovskite film.
[0094] Example 8
[0095] The ITO substrate is etched with sulfuric acid to increase the surface roughness of the ITO so as to improve the wettability of the PTAA carrier transport layer. Taking the scraping of the perovskite film as an example, the following steps are specifically included:
[0096] 1) Same as step 1) in Example 1;
[0097] 2) Preparation of nano-scale rough structure: Concentrated sulfuric acid and water are mixed in a volume ratio of 2:1 to obtain an acidic etching solution, and then the ITO to be washed is placed in the etching solution, and the entire container is placed in a water bath at 50-70°C for heating and ultrasonic treatment for 30 minutes. After the reaction is complete, ultrasonic cleaning is performed with deionized water for 15 minutes, and after drying with a nitrogen flow, an ITO substrate with a rough structure of 5.4 nm on the surface can be obtained.
[0098] 3) Preparation of PTAA carrier transport layer: same as step 3) in Example 1;
[0099] 4) Preparation of perovskite solution: same as step 4) in Example 1;
[0100] 5) Preparation of perovskite film: same as step 5) in Example 1.
[0101] Example 9
[0102] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of Poly-TPD. Taking the scraping of perovskite film as an example, the following steps are specifically included:
[0103] 1) Same as step 1) in Example 1;
[0104] 2) Preparation of nanoscale rough structure: Prepare 35 mg / mL NiO x aqueous solution and ultrasonically dispersed for 1 h to obtain NiO x The solution was spin-coated on the ITO glass pretreated in step 1) at 1300 rpm for 30 seconds, and then annealed at 150°C for 30 minutes to obtain a NiO surface. x Nanoscale rough structured substrate;
[0105] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO xPoly-TPD was coated on the substrate: 2 mg / mL Poly-TPD solution dissolved in chlorobenzene was spin-coated on the NiO substrate at 3500 rpm. x The nanoscale rough structure is then annealed at 80°C for 10 min to obtain a substrate with a super-wettable carrier transport layer.
[0106] 4) Preparation of perovskite solution: same as step 4) in Example 1;
[0107] 5) Preparation of perovskite film: same as step 5) in Example 1.
[0108] Example 10
[0109] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of MeO-4PADBC. Taking the scraping of perovskite film as an example, the following steps are specifically included:
[0110] 1) Same as step 1) in Example 1;
[0111] 2) Preparation of nanoscale rough structure: Prepare 20 mg / mL NiO x aqueous solution and ultrasonically dispersed for 1 h to obtain NiO x The solution was spin-coated on the ITO glass pretreated in step 1) at 2000 rpm for 30 seconds, and then annealed at 150°C for 30 minutes to obtain a NiO surface. x Nanoscale rough structured substrate;
[0112] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x Coating MeO-4PADBC on the substrate: 0.3 mg / mL MeO-4PADBC solution dissolved in ethanol was spin-coated on the NiO substrate at 4000 rpm. x The nanoscale rough structure is then annealed at 100°C for 10 min to obtain a substrate with a super-wettable carrier transport layer.
[0113] 4) Preparation of perovskite solution: same as step 4) in Example 1;
[0114] 5) Preparation of perovskite film: same as step 5) in Example 1.
[0115] Embodiment 11
[0116] Au nanoparticles with a particle size of about 20 nm are used as nanoscale roughness modulation materials to improve the surface wettability of Me-4PACz. Taking the scraping of perovskite film as an example, the following steps are specifically included:
[0117] 1) Same as step 1) in Example 1;
[0118] 2) Preparation of nanoscale rough structure: 0.1 mg / mL Au nanoparticle solution (or dispersion) was spin-coated on the ITO glass pretreated in step 1) at 3000 rpm for 30 seconds, and then annealed at 150° C. for 10 minutes to obtain a substrate with Au nanoscale rough structure on the surface;
[0119] 3) Coating Me-4PACz on the ITO / Au substrate with Au nanoscale rough structure: the process is the same as step 3) in Example 2.
[0120] 4) Preparation of perovskite solution: same as step 4) in Example 1;
[0121] 5) Preparation of perovskite film: same as step 5) in Example 1.
[0122] Example 12
[0123] Using Al2O3 nanoparticle dispersion (dispersed in isopropanol) with a particle size of <50nm as a nanoscale roughness modulation material to improve the surface wettability of Me-4PACz, and taking the scraping of perovskite film as an example, the specific steps include:
[0124] 1) Same as step 1) in Example 1;
[0125] 2) Preparation of nano-scale rough structure: 0.6 wt % Al2O3 isopropanol dispersion was spin coated on the ITO glass pretreated in step 1) at 4000 rpm for 30 seconds, and then annealed at 80° C. for 3 minutes to obtain a substrate with Al2O3 nano-scale rough structure on the surface;
[0126] 3) Coating Me-4PACz on an ITO / Al2O3 substrate having an Al2O3 nano-scale rough structure: the process is the same as step 3) of Example 2.
[0127] 4) Preparation of perovskite solution: same as step 4) in Example 1;
[0128] 5) Preparation of perovskite film: same as step 5) in Example 1.
[0129] Example 13
[0130] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of copper phthalocyanine. Taking the scraping of perovskite film as an example, the following steps are specifically included:
[0131] 1) Same as step 1) in Example 1;
[0132] 2) Preparation of nanoscale rough structure: Prepare 20 mg / mL NiO xaqueous solution and ultrasonically dispersed for 1 h to obtain NiO x The solution was spin-coated on the ITO glass pretreated in step 1) at 2000 rpm for 30 seconds, and then annealed at 150°C for 30 minutes to obtain a NiO surface. x Nanoscale rough structured substrate;
[0133] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x Coating copper phthalocyanine on the substrate: 10 mg / mL copper phthalocyanine dissolved in chlorobenzene solution was spin-coated on the NiO substrate at 4000 rpm. x The nanoscale rough structure is then annealed at 70°C for 10 minutes to obtain a substrate with a highly wettable copper phthalocyanine transport layer.
[0134] 4) Preparation of perovskite solution: same as step 4) in Example 1;
[0135] 5) Preparation of perovskite film: same as step 5) in Example 1.
[0136] Embodiment 14
[0137] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of 2PACz. Taking the scraping of perovskite film as an example, the following steps are specifically included:
[0138] 1) Same as step 1) in Example 1;
[0139] 2) Preparation of nano-scale rough structure: same as step 2) in Example 3;
[0140] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x Coating 2PACz on the substrate: Spin coat a 0.3 mg / mL 2PACz solution dissolved in ethanol on the NiO substrate at 3000 rpm. x The nanoscale rough structure is then annealed at 80°C for 10 min to obtain a substrate with a super-wettable carrier transport layer.
[0141] 4) Preparation of perovskite solution: same as step 4) in Example 1;
[0142] 5) Preparation of perovskite film: same as step 5) in Example 1.
[0143] Embodiment 15
[0144] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of Me-2PACz. Taking the scraping of perovskite film as an example, the following steps are specifically included:
[0145] 1) Same as step 1) in Example 1;
[0146] 2) Preparation of nano-scale rough structure: same as step 2) in Example 3;
[0147] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x Coating Me-2PACz on the substrate: 0.3 mg / mL Me-2PACz solution dissolved in ethanol was spin-coated on the NiO substrate at 3000 rpm. x The nanoscale rough structure is then annealed at 80°C for 10 min to obtain a substrate with a super-wettable carrier transport layer.
[0148] 4) Preparation of perovskite solution: same as step 4) in Example 1;
[0149] 5) Preparation of perovskite film: same as step 5) in Example 1.
[0150] Example 16
[0151] NiO with a particle size of about 10 nm x Nanoparticles are used as nanoscale roughness modulation materials to improve the surface wettability of MeO-4PACz. Taking the scraping of perovskite film as an example, the following steps are specifically included:
[0152] 1) Same as step 1) in Example 1;
[0153] 2) Preparation of nano-scale rough structure: same as step 2) in Example 3;
[0154] 3) In the presence of NiO x Nanoscale rough structure of ITO / NiO x Coating MeO-4PACz on the substrate: 0.3 mg / mL MeO-4PACz solution dissolved in ethanol was spin-coated on the NiO substrate at 3000 rpm. x The nanoscale rough structure is then annealed at 80°C for 10 min to obtain a substrate with a super-wettable carrier transport layer.
[0155] 4) Preparation of perovskite solution: same as step 4) in Example 1;
[0156] 5) Preparation of perovskite film: same as step 5) in Example 1.
[0157] Comparative Example 1
[0158] Taking PTAA as the carrier transport material and scraping the perovskite film as an example, the following steps are specifically included:
[0159] 1) Pretreatment of transparent ITO conductive substrate: ITO conductive glass was ultrasonically cleaned with detergent, deionized water, acetone, and isopropanol for 15 min in sequence, dried with nitrogen, and then treated with UV ozone for 15 min;
[0160] 2) Coating MeO-2PACz on an ITO substrate without nanoscale roughness: A 2 mg / mL PTAA solution dissolved in chlorobenzene (CB) was spin-coated on the ITO at 6000 rpm and then annealed at 80°C for 10 min.
[0161] 3) Preparation of perovskite solution: same as step 4) in Example 1;
[0162] 4) Preparation of perovskite film: same as step 5) in Example 1.
[0163] Comparative Example 2
[0164] Taking Me-4PACz as the carrier transport material and scraping the perovskite film as an example, the specific steps include:
[0165] 1) Pretreatment of transparent ITO conductive substrate: ITO conductive glass was ultrasonically cleaned with detergent, deionized water, acetone, and isopropanol for 15 min in sequence, dried with nitrogen, and then treated with UV ozone for 15 min;
[0166] 2) Coating Me-4PACz on an ITO substrate without nanoscale roughness structure: A 0.2 mg / mL Me-4PACz solution dissolved in ethanol was spin-coated on the ITO at 3000 rpm and then annealed at 80° C. for 10 min.
[0167] 3) Preparation of perovskite solution: same as step 4) in Example 1;
[0168] 4) Preparation of perovskite film: same as step 5) in Example 1.
[0169] Comparative Example 3
[0170] Taking MeO-2PACz as the carrier transport material and scraping the perovskite film as an example, the specific steps include:
[0171] 1) Pretreatment of transparent ITO conductive substrate: ITO conductive glass was ultrasonically cleaned with detergent, deionized water, acetone, and isopropanol for 15 min in sequence, dried with nitrogen, and then treated with UV ozone for 15 min;
[0172] 2) Coating MeO-2PACz on an ITO substrate without nanoscale roughness structure: A 0.2 mg / mL MeO-2PACz solution dissolved in ethanol was spin-coated on the ITO at 3000 rpm and then annealed at 80° C. for 10 min.
[0173] 3) Preparation of perovskite solution: same as step 4) in Example 1;
[0174] 4) Preparation of perovskite film: same as step 5) in Example 1.
[0175] Comparative Example 4
[0176] Taking 2PACz as the carrier transport material and scraping the perovskite film as an example, the specific steps include:
[0177] 1) Pretreatment of transparent ITO conductive substrate: ITO conductive glass was ultrasonically cleaned with detergent, deionized water, acetone, and isopropanol for 15 min in sequence, dried with nitrogen, and then treated with UV ozone for 15 min;
[0178] 2) Coating 2PACz on an ITO substrate without nanoscale roughness structure: A 0.3 mg / mL 2PACz solution dissolved in ethanol was spin-coated on the ITO at 3000 rpm and then annealed at 80° C. for 10 min.
[0179] 3) Preparation of perovskite solution: same as step 4) in Example 1;
[0180] 4) Preparation of perovskite film: same as step 5) in Example 1.
[0181] Comparative Example 5
[0182] Taking Me-2PACz as the carrier transport material and scraping the perovskite film as an example, the specific steps include:
[0183] 1) Pretreatment of transparent ITO conductive substrate: ITO conductive glass was ultrasonically cleaned with detergent, deionized water, acetone, and isopropanol for 15 min in sequence, dried with nitrogen, and then treated with UV ozone for 15 min;
[0184] 2) Coating Me-2PACz on an ITO substrate without nanoscale roughness structure: A 0.3 mg / mL Me-2PACz solution dissolved in ethanol was spin-coated on the ITO at 3000 rpm and then annealed at 80° C. for 10 min.
[0185] 3) Preparation of perovskite solution: same as step 4) in Example 1;
[0186] 4) Preparation of perovskite film: same as step 5) in Example 1.
[0187] Comparative Example 6
[0188] Taking MeO-4PACz as the carrier transport material and scraping the perovskite film as an example, the specific steps include:
[0189] 1) Pretreatment of transparent ITO conductive substrate: ITO conductive glass was ultrasonically cleaned with detergent, deionized water, acetone, and isopropanol for 15 min in sequence, dried with nitrogen, and then treated with UV ozone for 15 min;
[0190] 2) Coating MeO-4PACz on an ITO substrate without nanoscale roughness structure: A 0.3 mg / mL MeO-4PACz solution dissolved in ethanol was spin-coated on the ITO at 3000 rpm and then annealed at 80° C. for 10 min.
[0191] 3) Preparation of perovskite solution: same as step 4) in Example 1;
[0192] 4) Preparation of perovskite film: same as step 5) in Example 1.
[0193] Figure 1 The different wetting states of the perovskite solution of the present invention on a flat substrate surface and a surface with a nano-scale rough structure. As can be seen from the figure, by constructing a nano-scale rough structure under the carrier transport layer (such as PTAA, Me-4PACz, MeO-2PACz, etc.), it can be transformed from a normal wetting state to a super wetting state.
[0194] According to the methods of Examples 1, 2 and 3, other conditions are not changed, and only NiO is changed. x The process parameters for preparing the nano-scale rough structure regulate the roughness of the nano-scale rough structure, thereby changing the wettability of the carrier transport layer. Some specific process parameters and corresponding roughness are shown in Table 1.
[0195] Table 1 NiO x Nanoscale rough structure preparation process parameters and corresponding roughness
[0196]
[0197] Figure 4 The experimental characterization shows the variation trend of the contact angle of the carrier transport layer with the roughness of the nanoscale roughness structure on the substrate surface. Figure 4 It can be seen that as the roughness of the nanoscale rough structure on the substrate surface gradually increases, due to the conformal effect, the roughness of the carrier transport layer also gradually increases, the contact angle of the perovskite precursor solution on the carrier transport layer gradually decreases, and super wetting is achieved (contact angle <10°).
[0198] Figure 5 By changing NiO x The roughness of the nanoscale rough structure is used to adjust the roughness of the carrier transport layer, realizing the self-spreading effect of the perovskite solution on the carrier transport layer. Figure 5It can be seen that when the roughness reaches a critical value, the carrier transport layer changes from normal wetting to super wetting, causing the droplets to spread over the entire substrate coated with the carrier transport layer. The critical roughness of the three carrier transport layers of PTAA, Me-4PACz and MeO-2PACz to achieve super wetting is 5.3nm, 5.9nm and 2.1nm respectively.
[0199] Figure 6 To introduce NiO x Comparison of bubble adsorption effects of three carrier transport layers (PTAA, Me-4PACz, MeO-2PACz) before and after nanoscale roughness structure. Figure 6 It can be seen that the rough structure enhances the bubble repelling effect of the carrier transport layer, which is beneficial to suppress the formation of structural defects in the thin films of large-area optoelectronic devices. Figure 7 The bottom scanning electron micrographs of the perovskite films prepared in Examples 1 to 3 and Comparative Examples 1 to 3 are shown, and the dotted circles are holes or pinholes in the films; Figure 8 The cross-sectional scanning electron micrographs of the perovskite films obtained in Examples 1 to 3 and Comparative Examples 1 to 3 are shown. The dotted circles indicate the holes at the interface of the film / carrier transport layer, and the arrows indicate the gaps at the interface of the film / carrier transport layer. Figure 7 , Figure 8 It can be seen that the perovskite films prepared in Example 1, Example 2 and Example 3 have less pinholes and buried hole density than the films prepared in the corresponding comparative examples.
[0200] Application: Preparation of perovskite solar cells
[0201] The substrates coated with carrier transport prepared in Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2 and Comparative Example 3 were respectively used for scraping to prepare perovskite solar cells, and the specific steps were as follows:
[0202] 1) Preparation of carrier transport layer + perovskite film: the same as Example 1, Example 2, Example 3, Comparative Example 1, Comparative Example 2, and Comparative Example 3 respectively;
[0203] 2) Preparation of electron transport layer: prepare 15 mg / mL PCBM in CB, heat until completely dissolved, and then spin-coat on the perovskite film in step 1) at 3000 rpm for 30 seconds, and then anneal at 80° C. for 10 minutes;
[0204] 3) Preparation of barrier layer: 7nm BCP was evaporated on PCBM with a vacuum degree of 10 -4 Pa, the rate is
[0205] 4) Preparation of top electrode: 100 nm Cu was evaporated on BCP with a vacuum degree of 10-4 Pa, the rate is
[0206] The photovoltaic performance of the perovskite solar cell prepared above was tested, and the results are shown in Fig. 9 As shown. Fig. 9 It can be seen that the performance of the device prepared by the carrier transport layer + perovskite film prepared in Example 1, Example 2 and Example 3 is significantly higher than that of the device prepared in the corresponding comparative example. The improvement of the short-circuit current of the device prepared by the carrier transport layer + perovskite film prepared in Example 1, Example 2 and Example 3 comes from the conversion improvement of the entire spectrum. The open circuit voltage of the device is also significantly improved, which is due to the reduction of non-radiative recombination after the bottom defects are suppressed. It can also be seen from the dark current curve that the leakage of the device prepared by the carrier transport layer + perovskite film prepared in Example 1, Example 2 and Example 3 is significantly smaller. This shows that the present invention can effectively reduce the density of pinholes and holes in the large-scale preparation of large-area optoelectronic functional films, and significantly improve device performance.
Claims
1. A method for improving the wettability of a carrier transport layer, characterized in that: The method includes increasing the roughness of the carrier transport layer by increasing the surface roughness of the substrate, thereby improving the wettability of the carrier transport layer; the method specifically includes the following steps: 1) Obtain a flat substrate; 2) constructing a nanoscale rough structure on the surface of the substrate obtained in step 1), adjusting the roughness value of the nanoscale rough structure to an appropriate range, and then depositing a carrier transport layer on the nanoscale rough structure. Due to the conformal effect between the nanoscale rough structure and the carrier transport layer, the roughness of the deposited carrier transport layer is changed by adjusting the roughness value of the nanoscale rough structure, thereby improving the wettability of the carrier transport layer.
2. The method according to claim 1, characterized in that In step 1), the substrate includes a glass substrate, a PI substrate, a PET substrate, a PEN substrate, and a transparent conductive film substrate on which indium tin oxide or fluorine-doped tin oxide is deposited on the surface of the above substrates.
3. The method according to claim 1, characterized in that In step 2), the method of constructing the nano-scale rough structure includes: depositing a nano-particle film on the substrate surface, or changing the surface roughness of the substrate by post-processing to obtain a nano-scale rough surface.
4. The method according to claim 1 or 3, characterized in that: The roughness range of the nanoscale rough structure is RMS = 2-100 nm.
5. The method according to claim 3, characterized in that: The method for depositing the nanoparticle film includes, but is not limited to, a solution method, sputtering deposition, electrochemical deposition, physical vapor deposition, chemical vapor deposition, and a sol-gel method.
6. The method according to claim 3, characterized in that The post-processing methods include surface post-processing methods such as acid etching, electron beam etching, laser etching, plasma etching, etc.
7. The method according to claim 3, characterized in that The nanoparticle film material includes but is not limited to inorganic nanoparticles and carbon-based nanoparticles.
8. The method according to claim 7, characterized in that The inorganic nanoparticles include metal particles or metal oxides; the metal particles include gold, silver, and platinum metal particles; the metal oxides include nickel oxide, titanium dioxide, zinc oxide, tin oxide, zirconium dioxide, hafnium dioxide, aluminum oxide, copper oxide, molybdenum oxide, tungsten oxide, vanadium oxide, and strontium oxide; the carbon-based nanoparticles include carbon nanotubes and graphene.
9. Use of the method according to any one of claims 1 to 8 in the preparation of photovoltaic thin film materials or perovskite solar cells.
Citation Information
Cited By
Self-organizing material and perovskite solar cell using same
WO2026160165A1