Carbon dioxide immobilization device and carbon dioxide immobilization method
Through the simple process of adding water, supplying carbon dioxide and dehydrating concrete sludge, the problem of complex and high cost of carbon dioxide fixation process in the existing technology is solved, and the production of fixed carbon dioxide powders is achieved at low cost, which is suitable for a variety of applications. It also reduces carbon dioxide emissions and improves CO2 capture and utilization efficiency.
Patent Information
- Application Number
- CN202380030378.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-27
- Publication Date
- 2024-11-12
AI Technical Summary
The prior art has complex processes and high costs in carbon dioxide immobilization, making it difficult to produce high-purity calcium carbonate powders in large quantities at low cost, especially in low purity, which cannot meet the quality requirements of certain uses.
A carbon dioxide immobilization device and method are designed to produce carbonate powders containing light calcium carbonate and cement components by adding water to concrete sludge that removes coarse aggregate and fine aggregate. The powder adopts a simple process of room temperature and pressure to reduce equipment investment and power consumption.
It has achieved the mass production of fixed carbon dioxide powder at low cost, has the function of carbon dioxide adsorption, is suitable for a variety of applications, effectively utilizes industrial waste, reduces carbon dioxide emissions, and improves CO2 capture and utilization efficiency.
Smart Images

Figure CN118946394A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a carbon dioxide fixation device and a carbon dioxide fixation method for producing powder from concrete sludge. Background Art
[0002] Conventionally, there is known a carbon dioxide fixation apparatus for obtaining calcium carbonate by reacting carbon dioxide with a calcium component of concrete sludge (cement slurry) generated in a concrete production process (for example, see Patent Documents 1 to 3).
[0003] Prior art literature
[0004] Patent Literature
[0005] Patent Document 1: Japanese Patent No. 5072090
[0006] Patent Document 2: Japanese Patent No. 4892520
[0007] Patent Document 3: Japanese Patent Application Publication No. 2010-76976 Summary of the invention
[0008] Problems to be solved by the invention
[0009] Under the situation of the formation of recording in the above-mentioned each patent documentation, although can obtain highly purified calcium carbonate, the manufacturing process is complicated, will cost, and is not easy to increase output.Even if the purity of calcium carbonate is low particularly, according to its purposes, also fully satisfy desired quality sometimes, even therefore require not to reach the necessary above high purity also can low cost mass production.
[0010] The present invention has been made in view of this point, and an object of the present invention is to provide a carbon dioxide fixation apparatus and a carbon dioxide fixation method that can fix carbon dioxide at low cost and mass-produce powder having carbon dioxide fixed therein at low cost.
[0011] Means for solving problems
[0012] The carbon dioxide fixation device according to claim 1 comprises the following mechanisms: a water adding mechanism for adding water to cement paste sludge while stirring to obtain a first intermediate, wherein the cement paste sludge is concrete sludge from which coarse aggregate and fine aggregate have been removed; a supply mechanism for supplying a gas containing carbon dioxide to the first intermediate to obtain a second intermediate; and a dehydrating mechanism for dehydrating the second intermediate to produce a powder containing light calcium carbonate as crystals of calcium carbonate, a cement component carbonated powder in which the calcium component of cement particles is carbonated on the surface of the cement particles, and a powder of unreacted cement particles.
[0013] The carbon dioxide fixation device described in claim 2 is the following device: in the carbon dioxide fixation device described in claim 1, the water adding mechanism adds water in an amount of not less than 4 times and not more than 15 times the weight of cement slurry sludge, wherein the cement slurry sludge is concrete sludge having a water-cement ratio of approximately 1 from which coarse aggregate and fine aggregate are removed.
[0014] The carbon dioxide fixation device according to claim 3 is the device according to claim 1 or 2, wherein the dehydration mechanism dehydrates the second intermediate by utilizing its own weight.
[0015] The carbon dioxide fixation method according to claim 4 comprises the following steps: a water adding step of adding water to cement slurry sludge while stirring to obtain a first intermediate, wherein the cement slurry sludge is concrete sludge from which coarse aggregate and fine aggregate have been removed; a supplying step of supplying a gas containing carbon dioxide to the first intermediate to obtain a second intermediate; and a dehydrating step of dehydrating the second intermediate to produce a powder containing light calcium carbonate as crystals of calcium carbonate, a cement component carbonated powder in which the calcium component of cement particles is carbonated on the surface of the cement particles, and unreacted cement particles.
[0016] The carbon dioxide fixation method described in claim 5 is the following method: in the carbon dioxide fixation method described in claim 4, in the water adding step, water in an amount of not less than 4 times and not more than 15 times the weight of cement slurry sludge is added, and the cement slurry sludge is concrete sludge with a water-cement ratio of approximately 1 from which coarse aggregate and fine aggregate are removed.
[0017] The carbon dioxide fixation method according to claim 6 is the method according to claim 4 or 5, wherein in the dehydration step, the second intermediate is dehydrated by its own weight.
[0018] Effects of the Invention
[0019] According to the present invention, powder containing light calcium carbonate, carbonated cement component powder, and unreacted carbonated cement component powder in which carbon dioxide is fixed can be mass-produced at low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0020] Figure 1 This is an explanatory diagram showing a carbon dioxide fixation device according to one embodiment of the present invention. DETAILED DESCRIPTION
[0021] The following reference Figure 1 One embodiment of the present invention will be described.
[0022] Figure 1 In the figure, 1 is a carbon dioxide fixation device. The carbon dioxide fixation device 1 is a powder production device that produces a dry powder 3 in which carbon dioxide is fixed, using concrete sludge 2 as a raw material.
[0023] Concrete sludge 2 is concrete sludge produced when manufacturing secondary concrete products. Concrete secondary products refer to products such as concrete columns and concrete piles that are formed by solidifying concrete materials composed of cement, water, fine aggregate, coarse aggregate, and admixtures. In particular, concrete sludge 2 is produced in the centrifugal forming process when manufacturing secondary concrete products. The concrete sludge produced in the centrifugal forming process is equivalent to mortar sludge and even cement slurry sludge in quality. Therefore, coarse aggregate and fine aggregate are removed from the concrete sludge 2 and the powder 3. The powder 3 manufactured using the carbon dioxide fixation device 1 of this embodiment does not contain aggregates (stone powder, etc.) with a particle size of more than 0.5 mm. The powder 3 is a carbon dioxide fixation powder in which carbon dioxide is fixed, and is a carbon dioxide adsorbent having a carbon dioxide adsorption function.
[0024] Concrete sludge 2 is a highly alkaline material rich in calcium (Ca) components derived from cement. This calcium component is a component effective for the adsorption of carbon dioxide.
[0025] In the concrete sludge 2 used in the present embodiment, the water-cement ratio (W / C) is approximately 1. For example, the component ratio of the concrete sludge 2 is 49.9% of cement component, 49.9% of water, and 0.2% of fine sand component.
[0026] It should be noted that the concrete sludge 2 can be a material obtained by separating the coarse aggregate and the fine aggregate from the concrete sludge generated in the concrete secondary product factory, or the residual concrete (waste) or recycled concrete (recycled material) in the raw concrete factory. That is, the concrete sludge 2 is the remaining component of the fresh concrete. In addition, the concrete sludge 2 is used directly at room temperature without being subjected to heating treatment or drying treatment.
[0027] The carbon dioxide fixation device 1 is provided with a water adding mechanism 5. The water adding mechanism 5 is a mechanism for obtaining a first intermediate 6 by adding water WI to the non-heated concrete sludge 2 while stirring. As an example, the water adding mechanism 5 has a dissolution tank 8 and a stirring mechanism 9 provided in the dissolution tank 8. As the stirring mechanism 9, for example, a rotary blade is used. The smaller the amount of water added relative to the weight of the concrete sludge 2, the higher the efficiency of the carbon dioxide adsorption amount, and the larger the amount of water added, the more the strength expression based on the hydration reaction is suppressed. In this embodiment, water WI of 4 times or more and 15 times or less of the weight of the concrete sludge 2 is added by the water adding mechanism 5. When the amount of water added is less than 4 times the weight of the concrete sludge 2, the adhesion of the concrete sludge 2 increases, and when it is greater than 15 times, the calcium ion concentration decreases, and the carbon dioxide adsorption efficiency decreases. Therefore, for example, when the amount of water added is 10 times the weight of the concrete sludge 2, the component ratio of the first intermediate 6 is 5% cement, 95% water, and 0% fine sand component.
[0028] In addition, the carbon dioxide fixation device 1 includes a supply mechanism 11. The supply mechanism 11 is directly connected to the water adding mechanism 5, and supplies a gas G containing carbon dioxide to the first intermediate 6 directly obtained by the water adding mechanism 5, thereby obtaining a second intermediate 12. As an example, the supply mechanism 11 includes a reaction tank 14 and a gas supply mechanism 15 provided in the reaction tank 14.
[0029] The reaction tank 14 is also called, for example, a vertical silo, and is formed in a long strip shape in the vertical direction. The first intermediate 6 is put into the reaction tank 14 from the top through the discharge portion 16 from the dissolution tank 8 of the water adding mechanism 5. In the present embodiment, the reaction tank 14 has a reaction tank main body 17 with a cylindrical outer surface and a reduction portion 18 with a conical outer surface, which are integrally arranged from top to bottom, so that the axial direction is arranged along the vertical direction. The reaction tank main body 17 is cylindrical with a fixed or approximately fixed barrel diameter. The reduction portion 18 is coaxially connected to the lower part of the reaction tank main body 17 and is reduced in diameter toward the bottom.
[0030] The gas supply mechanism 15 is a mechanism for fixing the carbon dioxide by reacting the carbon dioxide in the gas G with the calcium component of the concrete sludge 2 to generate calcium carbonate. The gas supply mechanism 15 includes a pipe, a valve, and a nozzle connected to a gas supply source. The gas supply mechanism 15 is connected to the lower part of the reaction tank 14, and the gas G is ejected from the lower part of the reaction tank 14 for a predetermined time, for example, 15 minutes to 120 minutes. The ejection of the gas G by the gas supply mechanism 15 may be continuous or intermittent.
[0031] The gas G supplied by the gas supply mechanism 15 can appropriately utilize exhaust gas from a gas supply source such as a boiler or a power plant. As an example, the gas G contains 5% to 25% of carbon dioxide.
[0032] In addition, the carbon dioxide fixation device 1 is provided with a dehydration mechanism 20. The dehydration mechanism 20 is a mechanism for directly obtaining the second intermediate 12 from the supply mechanism 11, and dehydrating the second intermediate 12 to produce the powder 3. In the present embodiment, the dehydration mechanism 20 dehydrates the second intermediate 12 by the weight of the second intermediate 12 (natural dehydration). That is, the dehydration mechanism 20 of the present embodiment is a non-driven mechanism without power, heat source, etc. As the dehydration mechanism 20, for example, a flexible container bag can be appropriately used. That is, the dehydration mechanism 20 is a mechanism that uses a non-woven fabric composed of chemical fibers or the like to form a bag shape, holds the powder 3 inside, and discharges water WO and the like whose particles are smaller than the powder 3 from the bottom and the peripheral part. The second intermediate 12 discharged from the outlet 22 at the bottom of the reaction tank 14 of the supply mechanism 11 to the outside of the reaction tank 14 is supplied to the dehydration mechanism 20. It should be noted that the dehydration mechanism 20 can also be forced to dry according to the use of the powder 3 to be produced.
[0033] Next, a method for fixing carbon dioxide (a method for producing the powder 3 ) using the carbon dioxide fixing apparatus 1 of the present embodiment will be described.
[0034] First, the concrete sludge 2 is introduced into the dissolution tank 8 of the water adding mechanism 5. When a predetermined amount of the concrete sludge 2 is introduced into the dissolution tank 8, the concrete sludge 2 in the dissolution tank 8 is stirred by the stirring mechanism 9 while adding a predetermined amount of water WI to the concrete sludge 2 by the water adding mechanism 5, thereby obtaining a first intermediate 6. This water adding step (water adding stirring step) is performed at room temperature.
[0035] Next, the first intermediate 6 is introduced from the top into the reaction tank 14 of the supply mechanism 11 via the discharge portion 16. In the supply mechanism 11, the gas G containing carbon dioxide is pressurized and supplied to the first intermediate 6 in the reaction tank 14 by the gas supply mechanism 15, thereby utilizing the carbon dioxide adsorption function (DAC (Direct Air Capture) function) of the concrete sludge 2 contained in the first intermediate 6 to cause the calcium component contained in the first intermediate 6 to react with carbon dioxide to generate calcium carbonate, thereby fixing carbon dioxide in the first intermediate 6.
[0036] Then, by operating the carbon dioxide fixation device 1 for a predetermined time, the second intermediate 12 in which carbon dioxide is adsorbed to the concrete sludge 2 is produced in the reaction tank 14. Then, the second intermediate 12 is introduced into the dehydration mechanism 20 via the outlet 22 of the reaction tank 14 of the supply mechanism 11, and the water WO is dehydrated by the dehydration mechanism 20 to produce the powder 3. The water content of the powder 3 produced by the dehydration mechanism 20 is in the range of 4% to 40%, and can be set according to the use of the powder 3.
[0037] The manufactured powder 3 is a composite carbon dioxide fixed powder containing three components, namely, light calcium carbonate, cement component carbonated powder, and cement component carbonated unreacted powder, with a particle size of 1 μm or more and 50 μm or less. It should be noted that the powder 3 will contain a very small amount of fine sand components, but in terms of the component ratio, it can be essentially ignored. Light calcium carbonate refers to the crystals of calcium carbonate generated by the reaction of the calcium component dissolved from cement particles into water with carbon dioxide. The cement component carbonated powder refers to a powder formed by the reaction of the calcium component of cement particles with the introduced carbon dioxide and carbon dioxide fixation (carbonation) in the form of calcium carbonate on the surface of the particles. The cement component carbonated unreacted powder refers to a powder that "has not undergone" the above-mentioned "reaction", that is, in this embodiment, it is the cement particles (unreacted sludge) themselves.
[0038] Regarding the composition ratio of light calcium carbonate, cement component carbonated powder, and cement component carbonated unreacted powder in the manufactured powder 3, light calcium carbonate is 2%, cement component carbonated powder is 94% or more, and cement component carbonated unreacted powder is 4% or less. In addition, regarding the weight ratio of carbon dioxide components due to carbon dioxide adsorption reaction, light calcium carbonate is 44wt%-CO2, cement component carbonated powder is 25wt%-CO2, and cement component carbonated unreacted powder is 1wt%-CO2. Therefore, the fixed weight of carbon dioxide per unit weight of the powder 3 is equivalent to 24.4wt%.
[0039] It should be noted that the manufactured powder 3 not only fixes carbon dioxide during the manufacturing process, but also has a carbon dioxide adsorption function inside thereof, and exhibits a function of adsorbing carbon dioxide over time, that is, a slow carbon dioxide adsorption function.
[0040] For example, the powder 3 produced by this embodiment can be used as an admixture during concrete mixing, asphalt paving sealing material, auxiliary material for soil improvement material, and auxiliary material for backfill grouting materials for tunnels, etc. It is easy to use, and through these applications, fixed objects containing fixed carbon dioxide can be effectively utilized.
[0041] Therefore, not only can concrete sludge 2, which is discharged as industrial waste in an amount of more than 3 million tons per year, be effectively utilized to produce powder, but it is also effective in countermeasures against global warming caused by carbon dioxide, and can be appropriately used in CCU (Carbon Dioxide Capture and Utilization) for collecting carbon dioxide and effectively utilizing it.
[0042] Thus, according to the present embodiment, water is added to the concrete sludge 2 from which the coarse aggregate and the fine aggregate have been removed while being stirred by means of the water adding mechanism 5, a gas G containing carbon dioxide is supplied to the first intermediate 6 by means of the supply mechanism 11 to generate a second intermediate 12, and the second intermediate 12 is dehydrated by means of the dehydration mechanism 20 to produce the powder 3. Thus, in the overall reaction process, there is no need for, for example, a solid-liquid separation mechanism, a solid separation mechanism, a powder and particle crushing mechanism, a forced drying mechanism, etc., that is, the equipment investment is small, and carbon dioxide can be fixed at low cost through a simple process at normal temperature and pressure, and the powder 3 with fixed carbon dioxide can be produced in large quantities at low cost.
[0043] Furthermore, since the concrete sludge 2 as a raw material can be used directly without performing a heating treatment or the like, the powder can be produced (carbon dioxide fixation) by a simple configuration and process that suppresses an increase in carbon dioxide emissions due to power consumption required for heating.
[0044] In the water adding mechanism 5 (water adding process), water of 4 to 15 times the weight is added to the concrete sludge 2 having a water-cement ratio of approximately 1 after removing the coarse aggregate and the fine aggregate, thereby stirring the concrete sludge 2 with an appropriate water content to produce the first intermediate 6 sent to the supply mechanism 11 (supply process).
[0045] In the dehydration mechanism 20 (dehydration step), the second intermediate body 12 is dehydrated by its own weight, thereby eliminating the need to use power and suppressing an increase in carbon dioxide emission due to power consumption when carbon dioxide is fixed.
[0046] Although the powder 3 produced by the carbon dioxide fixation device 1 of this embodiment cannot obtain high-purity light calcium carbonate to become a composite carbon dioxide fixation powder, the manufacturing process is simplified. The powder is a composite of three powders with a particle size of less than 50 μm, and the carbon dioxide fixation weight ratio can be maintained at about 25% of the weight. Moreover, the production volume of light calcium carbonate produced by the existing light calcium carbonate manufacturing method can be more than 50 times.
[0047] Even if the powder 3 has low purity, it can fully meet the required quality for use, such as asphalt pavement sealing materials, etc. That is, the powder 3 of a quality suitable for the application can be mass-produced at low cost, and the carbon dioxide fixing material can be widely and effectively utilized.
[0048] According to the above characteristics, the powder can be provided at a lower cost than light calcium carbonate. In addition, it can also be highly evaluated as a device and technology for effectively utilizing CO2 fixation.
[0049] Explanation of symbols
[0050] 1. Carbon dioxide fixation device
[0051] 2Concrete sludge
[0052] 3. Powder
[0053] 5. Water adding mechanism
[0054] 6First intermediate
[0055] 11 Supply Agency
[0056] 12 Second Intermediate
[0057] 20Dehydration mechanism
[0058] G Gas
Claims
1. A carbon dioxide fixation device, characterized in that: It has the following institutions: a water adding mechanism for adding water to cement slurry sludge while stirring it to obtain a first intermediate, wherein the cement slurry sludge is concrete sludge from which coarse aggregate and fine aggregate are removed; a supply mechanism that supplies a gas containing carbon dioxide to the first intermediate to obtain a second intermediate; as well as A dehydration mechanism dehydrates the second intermediate to produce a powder, the powder comprising: light calcium carbonate as a crystal of calcium carbonate; cement component carbonated powder in which calcium components of cement particles are carbonated on the surface of the cement particles; and unreacted cement particles.
2. The carbon dioxide fixation device according to claim 1, characterized in that: The water adding mechanism adds water in an amount of not less than 4 times and not more than 15 times the weight of the cement slurry sludge, wherein the cement slurry sludge is concrete sludge having a water-cement ratio of approximately 1 from which coarse aggregate and fine aggregate are removed.
3. The carbon dioxide fixation device according to claim 1 or 2, characterized in that: The dehydration mechanism dehydrates the second intermediate body by utilizing its own weight.
4. A method for fixing carbon dioxide, characterized in that: It has the following processes: a water adding step of adding water to cement slurry sludge while stirring to obtain a first intermediate, wherein the cement slurry sludge is concrete sludge from which coarse aggregate and fine aggregate have been removed; a supplying step of supplying a gas containing carbon dioxide to the first intermediate to obtain a second intermediate; and The dehydration step dehydrates the second intermediate to produce a powder, the powder comprising: light calcium carbonate as a crystal of calcium carbonate; cement component carbonated powder in which the calcium component of cement particles is carbonated on the surface of the cement particles; and unreacted cement particles.
5. The method for fixing carbon dioxide according to claim 4, characterized in that: In the water adding step, water in an amount of 4 to 15 times the weight is added to the cement slurry sludge, which is concrete sludge having a water-cement ratio of approximately 1 from which coarse aggregate and fine aggregate are removed.
6. The method for fixing carbon dioxide according to claim 4 or 5, characterized in that: In the dehydration step, the second intermediate is dehydrated by its own weight.