Method for preparing electroactive material for metal ion battery

By controlling the temperature difference between the inner surface of the reaction zone and the porous particles and optimizing the deposition conditions, the problems of silicon deposition in the CVI method are solved, and efficient and uniform silicon deposition is achieved, which is suitable for large-scale production.

CN118946524APending Publication Date: 2024-11-12NEXEON LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030112.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-04-08
Filing Date
2023-04-11
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

Existing chemical vapor-phase permeability (CVI) methods are difficult to control silicon deposition in large-scale production, resulting in pollution in reaction zones and product inhomogeneity, limiting production scale, and high-temperature operations increase energy consumption and pollution risks.

Method used

By controlling the temperature difference between the inner surface of the reaction zone and the porous particles at ≤+90°C, the relatively high concentration of porous particles with high surface area and silicon-containing precursor gas is used, combined with continuous stirring technology, the silicon deposition conditions are optimized to avoid dyeing in the reaction zone. and improve product uniformity.

Benefits of technology

It effectively avoids the adverse phenomenon of silicon deposition on the surface of the reaction zone, ensures high quality and production efficiency of the products, extends the equipment operation time, and reduces cleaning and maintenance costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946524A_ABST
    Figure CN118946524A_ABST
Patent Text Reader

Abstract

The present invention relates to a method for preparing composite particles, the method comprising contacting a plurality of particles in a reaction zone with a gas comprising at least 25% by volume of a silicon-containing precursor at a temperature effective to cause deposition of silicon in pores of the porous particles. A controlled temperature difference between a maximum temperature of the inner surface of the reaction zone and a contemporaneous minimum temperature within the plurality of porous particles is maintained during the contacting step.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to methods and systems for preparing electroactive materials suitable for metal ion batteries by depositing silicon into the pores of porous particulate materials using chemical vapor infiltration (CVI). Background Art

[0002] The present inventors have previously reported the development of a class of electroactive materials having a composite structure in which nanometer-sized electroactive materials such as silicon are deposited into the pores of highly porous particulate materials such as porous carbon materials.

[0003] For example, WO 2020 / 128495 discloses such a granular material comprising a plurality of composite particles.

[0004] The material described in WO 2020 / 128495 has been prepared using CVI. The porous particles are contacted with monosilane gas at a temperature of 400 to 500° C. A low concentration of monosilane is used, such as 1.25% by volume. Such existing CVI methods are sufficient for laboratory-scale production, but are not suitable for large-scale manufacturing.

[0005] For example, the use of such low concentrations of silicon-containing precursors means that the production time of the composite particles is unacceptable on a large scale.

[0006] Furthermore, it has been found that existing methods of depositing silicon into the pores of porous particles using the CVI process result in uncontrolled soiling of the reaction zone. In particular, relatively large flakes of the silicon-rich composite material may form on the inner surface of the reaction zone.

[0007] Such flaking behavior is detrimental to production because even after post-production processes such as screening, the contaminated material may break up and mix into the granular material. This reduces the quality of the granular material and may cause undesirable effects within the electrode formulation, such as uneven expansion and loss of contact.

[0008] It has also been determined that the formation of silicon flakes on the inner surface of the reaction zone is associated with the formation of composite particles having a high content of coarse silicon, as defined herein. The inventors believe that coarse silicon is an indication of inhomogeneous silicon deposition. Therefore, contamination of the reaction zone is believed to be associated with poor control of silicon deposition in the porous particles.

[0009] In large-scale production, contamination may completely stop production. Stopping production to remove the contaminated material causes unacceptable delays and cumbersome cleaning procedures.

[0010] Some CVI processes such as fixed bed, conveyor bed and vibrating fluidized bed processes rely on a high ratio of reactor surface area to porous particle mass and low bed thickness to achieve adequate heat transfer to the porous particles. In addition to the risk of contamination, this limits the scalability of such processes. To increase the throughput of technologies that rely on a relatively high ratio between reactor surface area and porous particle mass, a proportional increase in reactor surface area is required.

[0011] Therefore, it is necessary to solve the above problems. Summary of the invention

[0012] In a first aspect, the present invention provides a method for preparing composite particles, the method comprising the following steps:

[0013] (a) providing a plurality of porous particles in a reaction zone, the reaction zone having an inner surface; and

[0014] (b) contacting the plurality of particles in the reaction zone with a gas comprising at least 25% by volume of a silicon-containing precursor at a temperature effective to cause deposition of silicon in the pores of the porous particles;

[0015] During step (b), ΔT≤+90°C is maintained, wherein ΔT represents the temperature difference between the maximum temperature of the inner surface of the reaction zone and the simultaneous minimum temperature within the plurality of porous particles, and wherein a positive value of ΔT indicates that the maximum temperature of the inner surface of the reaction zone is higher than the minimum temperature within the plurality of particles.

[0016] In another aspect, the present invention provides a system for preparing composite particles, the system comprising:

[0017] (a) a reaction zone, the reaction zone being configured to accommodate a plurality of porous particles, the reaction zone having:

[0018] (i) at least one heat source configured to heat the plurality of porous particles;

[0019] (ii) at least one gas inlet for receiving a gas comprising at least 25% by volume of a silicon-containing precursor;

[0020] (iii) at least one gas outlet for removing exhaust gas from said reaction zone;

[0021] (b) at least one sensor configured to acquire temperature data within the plurality of porous particles;

[0022] (c) at least one sensor configured to acquire temperature data of an inner surface of the reaction zone; and

[0023] (d) processor;

[0024] The at least one sensor configured to obtain temperature data within the plurality of porous particles and the at least one sensor configured to obtain temperature data of the inner surface of the reaction zone are configured to send corresponding temperature data to the processor, and the processor is configured to control the heat source so as to maintain ΔT≤+90°C, wherein ΔT represents the temperature difference between the highest temperature of the inner surface of the reaction zone and the lowest temperature within the plurality of porous particles during the same period, wherein a positive value of ΔT indicates that the highest temperature of the inner surface of the reaction zone is higher than the lowest temperature within the plurality of particles. The system can be used to perform the method of the present invention.

[0025] The method and system of the present invention have been developed to achieve simultaneous control of product quality while avoiding undesirable deposition of silicon onto reactor surfaces.

[0026] The deposition of silicon in the process of the present invention occurs due to thermal decomposition of the silicon-containing precursor at the surface. The relative amount of silicon deposited on the pore surfaces of the porous particles and on the inner surface of the reaction zone depends on:

[0027] (i) the relative surface area of ​​the porous particle and the interior surface of the reaction zone; and

[0028] (ii) the relative temperature of the porous particle and the inner surface of the reaction zone; and

[0029] Porous particles are very high surface area materials, so at the same temperature, it is expected that silicon deposition will occur almost entirely on the inner surface of the porous particles. However, porous particles, particularly porous carbon particles, have very poor thermal conductivity, so a large temperature difference may be formed between the reactor surface as a heat source for the reaction and the porous particles. It is believed that this temperature difference explains the formation of silicon flakes on the inner surface of the reaction zone. Another consequence of this temperature difference is that it is associated with a large temperature gradient within the porous particle mass in the reaction zone. Particles adjacent to the inner reactor surface become overheated and have the problem of uncontrolled deposition of silicon (causing the excessive coarse silicon formation described herein), while particles further away from the inner reactor surface are significantly colder, thereby making silicon deposition minimal or even non-existent.

[0030] The above problem is still further exacerbated when the loading of the porous particles of the reactor increases, because the particle bed depth increases, thereby increasing the maximum distance between the particles and the internal reactor surface as a heat source. The problem is also exacerbated when the concentration of silicon precursors in the gas fed to the reactor increases. Both of these factors are necessary to ensure high throughput in the reaction zone, but both increase the possibility of reactor contamination and product non-uniformity.

[0031] The process of the present invention solves these problems by controlling the temperature difference between the porous particles and the inner surface of the reaction zone so that it does not exceed +90°C. This has been found to be an effective upper limit at which the relatively high surface area of ​​the porous particles is the dominant factor in determining the location of silicon deposition. As the reactor loading and / or the surface area of ​​the porous particles begin to increase, the balance shifts still further in favor of deposition onto the pore surfaces of the porous particles.

[0032] According to the present invention, a ΔT of ≤ +90° C. is maintained during step (b) so that the temperature of the inner surface of the reaction zone never exceeds the lowest temperature within the plurality of porous particles by more than 90° C. This can also be expressed as a requirement to maintain the following conditions during contact of the gas containing the silicon-containing precursor with the plurality of porous particles:

[0033] T IS ≤[T P +90℃]

[0034] Where T IS is the maximum temperature of the inner surface of the reaction zone, T P It is the lowest temperature within multiple particles during the same period.

[0035] Therefore, ΔT is equivalent to T IS -T P .

[0036] Without being bound by theory, when reaction conditions are controlled in this manner, it is believed that the relatively higher surface area of ​​the porous particles compared to the inner surface of the reaction zone results in preferential deposition within the pores of the porous particles even when the maximum temperature of the inner surface of the reaction zone exceeds the minimum temperature within the plurality of particles by up to 90°C.

[0037] Thus, it was observed that maintaining ΔT ≤ +90°C resulted in reduced flake formation in the reaction zone. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 is a graph showing representative temperatures of the inner surface of a reaction zone and temperatures within a plurality of particles for a comparative process.

[0039] Figure 2 It is shown Figure 1 Shown are graphs of representative temperatures of the interior surface of the reaction zone and the temperatures within a plurality of particles during one silicon deposition cycle of a comparative process.

[0040] Figure 3 is a graph showing representative temperatures of the inner surface of a reaction zone and temperatures within a plurality of particles for a comparative process.

[0041] Figure 4 It is shown Figure 3Shown are graphs of representative temperatures of the interior surface of the reaction zone and the temperatures within a plurality of particles during one silicon deposition cycle of a comparative process.

[0042] Figure 5 is a graph showing representative temperatures of an interior surface of a reaction zone and temperatures within a plurality of particles according to a method of the present invention.

[0043] Figure 6 It is shown Figure 5 A graph of representative temperatures of the interior surface of the reaction zone and the temperatures within a plurality of particles during one silicon deposition cycle of the process is shown.

[0044] Figure 7 is a graph showing representative temperatures of an interior surface of a reaction zone and temperatures within a plurality of particles according to a method of the present invention.

[0045] Figure 8 It is shown Figure 7 A graph of representative temperatures of the interior surface of the reaction zone and the temperatures within a plurality of particles during one silicon deposition cycle of the process is shown.

[0046] Fig. 9 is a graph showing representative temperatures of an interior surface of a reaction zone and temperatures within a plurality of particles according to a method of the present invention.

[0047] Fig.10 It is shown Fig. 9 A graph of representative temperatures of the interior surface of the reaction zone and the temperatures within a plurality of particles during one silicon deposition cycle of the process is shown.

[0048] Fig.11 is a graph showing representative temperatures of an interior surface of a reaction zone and temperatures within a plurality of particles according to a method of the present invention. DETAILED DESCRIPTION

[0049] As used herein, "reaction zone" means an at least partially enclosed volume in which a deposition reaction occurs. The reaction zone can be any suitable form of reaction vessel. The reaction zone can be a batch reactor or a continuous reactor. The reaction zone can be a tubular reactor, a fixed bed reactor, a fluidized bed reactor, or a continuous stirred tank reactor.

[0050] Preferably, during step (b), ΔT≤+85°C, or ΔT≤+80°C, or ΔT≤+75°C, or ΔT≤+70°C, or ΔT≤+65°C, or ΔT≤+60°C, or ΔT≤+55°C is maintained. More preferably, during step (b), ΔT≤+50°C, or ΔT≤+45°C, or ΔT≤+40°C, or ΔT≤+35°C, or ΔT≤+30°C, or ΔT≤+25°C is maintained. Still more preferably, during step (b), ΔT≤+20°C, or ΔT≤+15°C, or ΔT≤+10°C, or ΔT≤+5°C is maintained. Most preferably, during step (b), ΔT≤0°C, or ΔT≤-5°C, or ΔT≤-10°C is maintained.

[0051] ΔT≤+90°C can be achieved in a variety of ways.

[0052] The deposition reaction is exothermic, which increases the temperature of the plurality of particles.

[0053] The plurality of porous particles and / or the gas containing the silicon-containing precursor may be preheated. The preheating may contribute to the temperature of the plurality of particles.

[0054] The plurality of porous particles and the gas containing the silicon-containing precursor may be contacted, i.e. mixed together, and preheated together. The plurality of porous particles and the gas containing the silicon-containing precursor may be preheated together before providing the plurality of porous particles in the reaction zone. Alternatively, the plurality of porous particles and the gas containing the silicon-containing precursor may be preheated together in the reaction zone.

[0055] The plurality of porous particles and / or the gas containing the silicon-containing precursor may be preheated separately.

[0056] The plurality of porous particles may be preheated before being provided in the reaction zone. For example, the porous particles may be conveyed through a heating zone before entering the reaction zone. The plurality of porous particles may be preheated to a temperature of 300 to 480°C, or 320 to 450°C, or 330 to 400°C, or 340 to 390°C, or 345 to 390°C, or 350 to 400°C, or 350 to 390°C, or 350 to 385°C, or 350 to 380°C, or 355 to 390°C, or 355 to 385°C, or 355 to 380°C, or 360 to 390°C, or 360 to 385°C, or 360 to 380°C.

[0057] The reaction zone may include a heat source, and step (a) may include operating the heat source to heat the plurality of porous particles. The heat source may heat the plurality of porous particles to 340 to 400°C, or 340 to less than 395°C, or 340 to 390°C, or 345 to 400°C, or 345 to less than 395°C, or 345 to 390°C, or 350 to 400°C, or 350 to less than 395°C, or 350 to 390°C, or 350 to 385°C, or 350 to 380°C, or 355 to 400°C, or 355 to less than 395°C, or 355 to 390°C, or 355 to 385°C. , or 355 to 380°C, or 360 to 400°C, or 360 to less than 395°C, or 360 to 390°C, or 360 to 385°C, or 360 to 380°C, or 365 to 400°C, or 365 to less than 395°C, or 365 to 390°C, or 365 to 385°C, or 365 to 380°C, or 370 to 400°C, or 370 to less than 395°C, or 370 to 390°C, or 370 to 385°C, or 370 to 380°C. The heat source can be a convection or conduction heat source. A temperature range of 370 to less than 395°C is particularly preferred.

[0058] The gas containing the silicon-containing precursor may be preheated prior to said contacting. Step (b) may include preheating the gas to a temperature of 100 to 350° C., or 110 to 340° C., or 120 to 330° C., or 130 to 320° C., or 140 to 310° C., or 150 to 300° C. prior to said contacting. Preheating the gas prior to contacting reduces temperature fluctuations within the plurality of porous particles that would otherwise result from contacting the particles with the gas. In this way, preheating the gas may help maintain the temperature of the plurality of particles.

[0059] Preferably, the ΔT maintained during step (b) is between +90°C and -110°C, or +85°C and -110°C, or +80°C and -110°C, or +75°C and -110°C, or +70°C and -110°C, or +65°C and -110°C, or +60°C and -110°C, or +55°C and -110°C, or +50°C and -110°C, or +45°C and -110°C, or +40°C and -110°C, or +35°C and -110°C, or +30°C and -110°C, or +25°C and -110°C, or +20°C and -110°C, or +15°C and -110°C, or +10°C and -110°C, or +5°C and -110°C. or -5°C to -60°C, or -5°C to -55°C, or -5°C to -50°C, or -5°C to -45°C, or -5°C to -40°C, or -5°C to -35°C, or -5°C to -30°C, or -5°C to -25°C, or -5°C to -20°C, or -5°C to -15°C, or -5°C to -10°C.

[0060] In some cases, sufficient silicon may be deposited in the pores of the porous particles in one deposition cycle. In other cases, it may be desirable to operate the method as a multi-cycle deposition, where successive deposition steps are used to deposit a target amount of silicon. In the multi-cycle deposition, the method may include:

[0061] (c) interrupting the deposition of silicon to form intermediate particles, and optionally separating by-products from the intermediate particles; and

[0062] (d) contacting the intermediate particles from step (c) with a gas comprising a silicon-containing precursor in a reaction zone at a temperature effective to cause further deposition of the silicon in the pores of the intermediate particles;

[0063] During step (d), ΔT≤+90°C is maintained, wherein ΔT represents the temperature difference between the maximum temperature of the inner surface of the reaction zone and the minimum temperature within the plurality of porous particles, wherein a positive value of ΔT indicates that the maximum temperature of the inner surface of the reaction zone is higher than the minimum temperature within the plurality of particles.

[0064] The reaction zone in step (d) may be the same reaction zone as in step (b). Alternatively, steps (b) and (d) may be carried out in different reaction zones.

[0065] Steps (c) and (d) can each be repeated as many times as desired to deposit a target amount of silicon. For example, steps (c) and (d) can each be performed 2 to 15 times, resulting in a total of 3 to 16 silicon deposition steps including step (b) and repeated step (d). When steps (c) and (d) are repeated, each instance of steps (c) and (d) is independently as described herein. For example, the silicon-containing precursor used in each repetition of step (d) can be the same or different. Preferably, the silicon-containing precursor used in each repetition of step (d) is monosilane.

[0066] The interruption of deposition in step (c) can be achieved in a variety of ways. Interruption of deposition can be achieved by allowing the silicon-containing precursor to be completely consumed by the deposition reaction. Alternatively, deposition can be interrupted while unreacted silicon-containing precursor is still present, such as by reducing the temperature. In this case, the gas containing the silicon-containing precursor used in step (d) may contain the silicon-containing precursor that was not consumed in step (b).

[0067] Preferably, during step (d), ΔT≤+85°C, or ΔT≤+80°C, or ΔT≤+75°C, or ΔT≤+70°C, or ΔT≤+65°C, or ΔT≤+60°C, or ΔT≤+55°C is maintained. More preferably, during step (d), ΔT≤+50°C, or ΔT≤+45°C, or ΔT≤+40°C, or ΔT≤+35°C, or ΔT≤+30°C, or ΔT≤+25°C is maintained. Still more preferably, during step (d), ΔT≤+20°C, or ΔT≤+15°C, or ΔT≤+10°C, or ΔT≤+5°C is maintained. Most preferably, during step (d), ΔT≤0°C, or ΔT≤-5°C, or ΔT≤-10°C is maintained.

[0068] During steps (b) and / or (d), the minimum temperature within the plurality of porous particles may be maintained at 340 to 400°C, or 340 to 395°C, or 340 to 390°C, or 345 to 400°C, or 345 to 395°C, or 345 to 390°C, or 350 to 400°C, or 350 to 395°C, or 350 to 390°C, or 350 to 385°C, or 350 to 380°C, or 355 to 400°C, or 355 to 395°C, or 355 to 390°C, or 355 to 390°C. or 370 to 400° C., or 370 to 395° C., or 370 to 390° C., or 370 to 385° C., or 370 to 380° C., or 370 to 400° C., or 370 to 395° C., or 370 to 390° C., or 370 to 385° C., or 370 to 380° C. It is particularly preferred that during steps (b), (c) and / or (d), the minimum temperature within the plurality of porous particles is maintained at a temperature of 370 to below 395° C.

[0069] More preferably, during steps (b) and / or (d), all of the plurality of porous particles are maintained at 340 to 400°C, or 340 to 395°C, or 340 to 390°C, or 345 to 400°C, or 345 to 395°C, or 345 to 390°C, or 350 to 400°C, or 350 to 395°C, or 350 to 390°C, or 350 to 385°C, or 350 to 380°C, or 355 to 400°C, or 355 to 395°C, or 355 to 390°C, or 355 to 390°C. 385° C., or 370 to 400° C., or 370 to 395° C., or 370 to 390° C., or 370 to 385° C., or 370 to 380° C., or 370 to 400° C., or 370 to 395° C., or 370 to 390° C., or 370 to 385° C., or 370 to 380° C. It is particularly preferred that during steps (b), (c) and / or (d), the minimum temperature within the plurality of porous particles is maintained at a temperature of 370 to below 395° C.

[0070] Reducing or eliminating temperature fluctuations across multiple porous particles can reduce energy consumption and contribute to improved production efficiency, especially for large-scale systems.

[0071] Conventional CVI processes using monosilane are carried out at temperatures above 400°C. Surprisingly, it has been found that CVI can be carried out at lower temperatures. Carrying out CVI at such high temperatures (e.g., 420 to 450°C) results in poor penetration of silicon. In addition, the use of such high temperatures requires the operation of heating and cooling cycles in the reaction zone and may exacerbate uncontrolled contamination of the reaction zone. In general, these problems limit production rates. The use of the above temperatures solves these problems.

[0072] The maximum temperature of the inner surface of the reaction zone during the contacting in steps (b) and / or (d) may be from 150 to 480°C, or from 150 to 460°C, or from 150 to 440°C, or from 150 to 420°C, or from 150 to 400°C, or from 150 to 390°C, or from 200 to 390°C, or from 250 to 390°C, or from 300 to 390°C, or from 340 to 375°C, or from 340 to 370°C, or from 345 to 370°C, or from 345 to 365°C, or from 350 to 400°C, or from 350 to 390°C, or from 350 to 380°C, or from 350 to 370°C, or from 350 to 365°C.

[0073] The maximum temperature of the inner surface of the reaction zone during the contacting in steps (b) and / or (d) may be no more than 480°C, or no more than 460°C, or no more than 440°C, or no more than 420°C, or no more than 400°C, or no more than 395°C, or no more than 390°C, or no more than 385°C, or no more than 380°C.

[0074] Step (d) may comprise preheating the gas to a temperature of 100 to 350°C, or 110 to 340°C, or 120 to 330°C, or 130 to 320°C, or 140 to 310°C, or 150 to 300°C prior to said contacting.

[0075] Step (a) may comprise providing a batch of a plurality of porous particles in a reaction zone.

[0076] The method may be operated in batch mode. In this case, step (b) or step (d) may comprise interrupting the deposition of silicon to form the composite particles, and removing the composite particles from the reaction zone.

[0077] The method may be operated in a continuous mode. In this case, step (a) may comprise:

[0078] providing a chemical vapor permeation unit including the reaction zone;

[0079] providing a raw material comprising the porous particles; and

[0080] continuously introducing the porous particles into the reaction zone;

[0081] And step (b) may include:

[0082] continuously introducing the gas comprising the silicon-containing precursor into the reaction zone;

[0083] providing conditions in the reaction zone effective to cause deposition of silicon in the pores of the porous particles;

[0084] continuously removing composite particles from the reaction zone, the composite particles comprising a porous particle skeleton and elemental silicon within pores of the porous particle skeleton; and

[0085] Exhaust gas is continuously withdrawn from the reaction zone.

[0086] The method may be operated batchwise for porous particles and continuously for silicon precursors. Step (a) may comprise providing a batch of a plurality of porous particles in a reaction zone. Step (b) may comprise continuously introducing a gas comprising a silicon-containing precursor into the reaction zone.

[0087] Step (b) and / or step (d) preferably comprises continuously stirring the porous particles. More preferably, step (b) and / or step (d) may comprise continuously mechanically stirring the porous particles during said contacting. Preferably, stirring is performed by a high shear mixer.

[0088] Agitation of the porous particles is preferred in the method of the present invention because it reduces temperature gradients within the porous particle mass and promotes uniform penetration of the silicon precursor gas throughout the porous particle mass. Both factors contribute to improved uniformity of silicon deposition throughout the porous particle mass, thereby reducing both flaking on the surfaces of the reactor and the formation of coarse silicon in the composite particles.

[0089] Preferably, the reaction zone comprises an agitator for continuously stirring the porous particles during said contacting. Any suitable agitator may be used, such as a turbine agitator, a paddle agitator, an anchor agitator, a propeller agitator or a spiral agitator. Preferably, the agitator is a high shear mixer.

[0090] Mechanical agitation of the porous particles decouples the silicon precursor gas supply rate from the mixing efficiency of the porous particles. In the case of a vertical fluidized bed reactor, agitation of the porous particles can only be achieved by supplying the silicon precursor gas at a rate sufficient to fluidize the porous particles. Therefore, the use of mechanical agitation enables the method to function at lower silicon precursor gas velocities than a vertical fluidized bed reactor process and enables the residence time of the silicon precursor to be adjusted independently of agitation.

[0091] The use of a high shear mixer provides continuous mechanical agitation and effectively breaks up agglomerates that naturally form due to the cohesive nature of the porous particles. Thus, both heat and mass transfer challenges are addressed.

[0092] The combination of temperature control of the present invention (ie maintaining ΔT≤+90° C.) and continuous stirring minimizes the risk of uneven silicon penetration and contamination of the reactor.

[0093] In step (a), the volume of the plurality of porous particles in the reaction zone is preferably at least 100 cm 3 Reaction zone volume per liter (cm 3 / L RV ), or at least 150cm 3 / L RV , or at least 200cm 3 / L RV , or at least 250cm 3 / L RV , or at least 300cm 3 / L RV , or at least 400cm 3 / L RV , or at least 500cm 3 / L RV , or at least 600cm 3 / L RV , or at least 700cm 3 / L RV , or at least 800cm 3 / L RV , or at least 900cm 3 / L RV .

[0094] Preferably, the volume of the plurality of porous particles is at least 500 cm 3 / L RV , and in some embodiments optionally is sufficient to substantially fill the volume of the reaction zone.

[0095] As used herein, the volume of a porous particle refers to the equivalent volume of the porous particle determined by the particle mass and tap density. For example, 200 g of a porous particle material having a tap density of 1000 g / L is considered to be 200 cm 3 porous particle material.

[0096] In the case of a continuous reactor in which the porous particles are moved through a reaction zone, the equivalent volume of the porous particles in the reactor is based on the feed rate (in g·min) of the porous particles into the reaction zone. -1 The average residence time of the particles in the reaction zone is calculated based on the tap density of the porous particles as described above.

[0097] The ratio of the internal surface area of ​​the reaction zone to the mass of the porous particles in the reaction zone may not exceed 1 m 2 / kg, or not more than 0.9m 2 / kg, or not more than 0.8m 2 / kg, or not more than 0.7m 2 / kg, or not more than 0.6m 2 / kg, or not more than 0.5m 2 / kg, or not more than 0.4m 2 / kg, or not more than 0.3m 2 / kg, or not more than 0.2m 2 / kg, or not more than 0.1m 2 / kg.

[0098] The ratio of the internal surface area of ​​the reaction zone to the mass of the porous particles in the reaction zone may be at least 0.001 m 2 / kg, or at least 0.002m 2 / kg, or at least 0.003m 2 / kg, or at least 0.004m 2 / kg, or at least 0.006m 2 / kg, or at least 0.008m 2 / kg, or at least 0.01m 2 / kg.

[0099] For example, the ratio of the internal surface area of ​​the reaction zone to the mass of the porous particles in the reaction zone may be 0.001 m 2 / kg to 1m 2 / kg, or 0.002m 2 / kg to 0.9m 2 / kg, or 0.003m 2 / kg to 0.8m 2 / kg, or 0.004m 2 / kg to 0.7m 2 / kg, or 0.006m 2 / kg to 0.6m 2 / kg, or 0.008m 2 / kg to 0.5m 2 / kg, or 0.01m 2 / kg to 0.4m 2 / kg, or 0.01m 2 / kg to 0.3m 2 / kg range.

[0100] The bed depth of porous particles in the reaction zone may be at least 11 cm, or at least 15 cm, or at least 20 cm, or at least 25 cm, or at least 30 cm.

[0101] Preferably, the aforementioned porous particle volume per liter of reaction zone, the ratio of the internal surface area of ​​the reaction zone to the mass of porous particles in the reaction zone and / or the bed depth of porous particles in the reaction zone are combined with continuous stirring as described herein.

[0102] The volume of the plurality of porous particles in the reaction zone in step (a) may be at least 100 cm 3 / L RV , and the bed depth of porous particles in the reaction zone can be at least 11 cm.

[0103] In step (a), the volume of the plurality of porous particles in the reaction zone may be at least 200 cm 3 / L RV , and the bed depth of porous particles in the reaction zone can be at least 15 cm.

[0104] In step (a), the volume of the plurality of porous particles in the reaction zone may be at least 300 cm 3 / L RV , and the bed depth of porous particles in the reaction zone can be at least 20 cm.

[0105] The volume of the plurality of porous particles in the reaction zone in step (a) may be at least 400 cm 3 / L RV , and the bed depth of porous particles in the reaction zone can be at least 25 cm.

[0106] The volume of the plurality of porous particles in the reaction zone in step (a) may be at least 500 cm 3 / L RV , and the bed depth of porous particles in the reaction zone can be at least 30 cm.

[0107] The volume of the plurality of porous particles in the reaction zone in step (a) may be at least 100 cm 3 / L RV , and the ratio of the internal surface area of ​​the reaction zone to the mass of the porous particles in the reaction zone may not exceed 1 m 2 / kg.

[0108] In step (a), the volume of the plurality of porous particles in the reaction zone may be at least 200 cm 3 / L RV , and the ratio of the internal surface area of ​​the reaction zone to the mass of the porous particles in the reaction zone may not exceed 0.9 m 2 / kg.

[0109] In step (a), the volume of the plurality of porous particles in the reaction zone may be at least 300 cm 3 / L RV , and the ratio of the internal surface area of ​​the reaction zone to the mass of the porous particles in the reaction zone may not exceed 0.8 m 2 / kg.

[0110] The volume of the plurality of porous particles in the reaction zone in step (a) may be at least 400 cm 3 / L RV , and the ratio of the internal surface area of ​​the reaction zone to the mass of the porous particles in the reaction zone may not exceed 0.7 m 2 / kg.

[0111] The volume of the plurality of porous particles in the reaction zone in step (a) may be at least 500 cm 3 / L RV , and the ratio of the internal surface area of ​​the reaction zone to the mass of the porous particles in the reaction zone may not exceed 0.6 m 2 / kg.

[0112] The volume of the plurality of porous particles in the reaction zone in step (a) may be at least 600 cm 3 / L RV , and the ratio of the internal surface area of ​​the reaction zone to the mass of the porous particles in the reaction zone may not exceed 0.5 m 2 / kg.

[0113] Suitable silicon precursors include: monosilane (SiH 4 ), disilane (Si 2 H 6 ), trisilane (Si 3 H 8 ), butadienesilane (Si 4 H 10 ), methylsilane (CH 3 S H 3 ), dimethylsilane ((CH 3 ) 2 S H 2 ) or chlorosilanes such as trichlorosilane (HSiCl 3 ) or methylchlorosilane such as methyltrichlorosilane (CH 3 SiCl 3 ) or dimethyldichlorosilane ((CH 3 ) 2 SiCl 2 ). A preferred silicon precursor is monosilane.

[0114] The silicon-containing precursors used in steps (b) and (d) may be the same or different. Preferably, the silicon-containing precursor used in each of steps (b) and (d) is monosilane.

[0115] The pressure in steps (b) and / or (d) may be 10 to 10000 kPa, or 100 to 5000 kPa, or 100 to 4000 kPa, or 100 to 3000 kPa, or 100 to 2000 kPa, or 100 to 1000 kPa, or 100 to 500 kPa.

[0116] The pressure in steps (b) and / or (d) may be 10 to 15000 kPa, or 50 to 10000 kPa, or 120 to 5000 kPa, or 150 to 2000 kPa, or 200 to 1800 kPa, or 200 to 1600 kPa, or 250 to 1500 kPa, or 300 to 1200 kPa, or 400 to 1000 kPa, or 500 to 900 kPa, or 600 to 800 kPa.

[0117] The pressures referred to in any step of the claimed process refer to the absolute pressure in the reaction zone which may comprise any suitable form of reaction vessel.

[0118] The silicon-containing precursor in step (b) and / or (d) can be used in pure form (or substantially pure form), or as a mixture diluted with an inert carrier gas such as nitrogen or argon. The carrier gas can also be hydrogen that is inert under reaction conditions. In the case of a mixture diluted with a carrier gas, the silicon-containing precursor in step (b) is used in an amount of at least 25 volume %. The gas can comprise a silicon-containing precursor having a total volume of at least 30 volume % based on the gas, or a silicon-containing precursor having a total volume of at least 40 volume %, or at least 50 volume %, or at least 60 volume %, or at least 70 volume %, or at least 80 volume %, or at least 90 volume %, or at least 95 volume %, or at least 97 volume %, or at least 99 volume %. The volume % of the silicon-containing precursor based on the total volume of the gas refers to the concentration of the silicon-containing precursor in the gas supplied to the reaction zone.

[0119] In the case of a mixture diluted with an inert carrier gas, the amount of the silicon-containing precursor used in step (d) may be preferably in the range of 1% to 95% by volume, or 1% to 85% by volume, or 1% to 70% by volume, or 1% to 50% by volume, or 2% to 40% by volume, or 5% to 30% by volume, or 5% to 25% by volume, based on the total gas volume of the precursor and the inert carrier gas. The gas used in step (d) may contain at least 25% by volume of the silicon-containing precursor based on the total volume of the gas, or at least 30% by volume, or at least 40% by volume, or at least 50% by volume, or at least 60% by volume, or at least 70% by volume, or at least 80% by volume, or at least 90% by volume, or at least 95% by volume, or at least 97% by volume, or at least 99% by volume of the silicon-containing precursor based on the total volume of the gas.

[0120] According to the conventional procedure of working in an inert atmosphere, the presence of oxygen should be minimized to prevent undesirable oxidation of the deposited silicon. Preferably, the oxygen content is less than 0.01% by volume, more preferably less than 0.001% by volume, based on the total volume of the gas used in steps (b) and (d).

[0121] The term "BET surface area" as used herein should be taken to mean the surface area per unit mass calculated from the measurement of the physical adsorption of gas molecules on a solid surface according to ISO 9277 using the Brunauer-Emmett-Teller principle.

[0122] The BET surface area of ​​porous particles can be 100 m 2 / g to 4,000m 2 Preferably, the BET surface area of ​​the porous particles is 500 m 2 / g to 4,000m 2 / g, or 750m 2 / g to 3,500m 2 / g, or 1,000m 2 / g to 3,250m 2 / g, or 1,000m 2 / g to 3,000m 2 / g, or 1,000m 2 / g to 2,500m 2 / g, or 1,000m 2 / g to 2,000m 2 The high surface area of ​​the porous particles compared to the internal surface of the reactor results in preferential deposition within the pores of the porous particles, especially at high particle loadings relative to the reactor volume and internal surface area.

[0123] The porous particles include a three-dimensional interconnected open pore network. The porous particles may include micropores and / or mesopores. Typically, the porous particles include both micropores and mesopores. However, it is not excluded that porous particles including micropores but not mesopores or porous particles including mesopores but not micropores may be used. According to conventional IUPAC terminology, the term "micropore" is used herein to refer to pores with a diameter less than 2 nm, the term "mesopore" is used herein to refer to pores with a diameter of 2-50 nm, and the term "macroporous" is used to refer to pores with a diameter greater than 50 nm.

[0124] References herein to the volumes of micropores, mesopores and macropores in porous particles and any reference to the distribution of pore volumes within porous particles relate to the internal pore volume of the porous particles used as the starting material in step (a) of the claimed method (i.e., before silicon is deposited into the pore volume in step (b)).

[0125] The quenched solid density functional theory (QSDFT) was used according to the standard method described in ISO 15901-2 and ISO 15901-3, using nitrogen adsorption at 77 K down to 10 -6 Relative pressure p / p 0 To determine the total volume of micropores and mesopores and the pore size distribution of micropores and mesopores. Nitrogen adsorption is a technique for characterizing the porosity and pore size distribution of a material by condensing a gas in the pores of a solid. As the pressure increases, the gas first condenses in the pores with the smallest diameter, and the pressure increases until a saturation point is reached, at which all pores are filled with liquid. The nitrogen pressure is then gradually reduced to evaporate the liquid from the system. Analysis of the adsorption and desorption isotherms and the hysteresis between them enables the determination of pore volume and pore size distribution. Suitable instruments for measuring pore volume and pore size distribution by nitrogen adsorption include TriStar II and TriStar II Plus porosity analyzers (which are available from Micromeritics Instrument Corporation in the United States), and Autosorb IQ porosity analyzers (which are available from Quantachrome Instruments).

[0126] Nitrogen adsorption is effective for measuring pore volume and pore size distribution for pores up to 50 nm in diameter, but is less reliable for pores with much larger diameters. For the purposes of the present invention, therefore, pore volume and pore size distribution are determined using nitrogen adsorption only for pores up to and including 50 nm in diameter (i.e., only for micropores and mesopores). 50 The values ​​are likewise determined only relative to the total volume of micropores and mesopores.

[0127] Given the limitations of available analytical techniques, it is not possible to measure pore volume and pore size distribution over the entire range of micropores, mesopores and macropores using a single technique. Where the porous particles include macropores, the volume of pores with diameters in the range of greater than 50 nm to 100 nm can be measured by mercury intrusion porosimetry, and preferably not more than 0.3 cm 3 / g, or not more than 0.2cm 3 / g, or not more than 0.1cm 3 / g, or not more than 0.05cm 3 / g. A small fraction of macropores can be useful in facilitating the entry of electrolytes into the pore network.

[0128] Any pore volume below 50 nm in size as measured by mercury intrusion is not considered (as described above, nitrogen adsorption is used to characterize mesopores and micropores). For the purposes of this invention, the pore volume above 100 nm as measured by mercury intrusion is assumed to be interparticle porosity and is also ignored.

[0129] Mercury intrusion porosimetry is a technique for characterizing the porosity and pore size distribution of a material by applying varying levels of pressure to a sample of the material immersed in mercury. The pressure required to cause mercury to penetrate into the pores of the sample is inversely proportional to the size of the pores. The values ​​obtained by mercury intrusion porosimetry reported herein are obtained according to ASTM UOP578-11, where for mercury at room temperature, the surface tension γ is 480 mN / m and the contact angle is is 140°. The density of mercury at room temperature is 13.5462 g / cm 3 A variety of high-precision mercury intrusion instruments are commercially available, such as the AutoPore IV series of automated mercury porosimeter, which is available from Micromeritics Instrument Corporation in the United States. For a complete overview of mercury intrusion, reference can be made to "Analytical Methods in Fine Particle Technology" by PA Webb and C. Orr, 1997, Micromeritics Instrument Corporation, ISBN 0-9656783-0.

[0130] It should be understood that intrusion techniques such as gas adsorption and mercury intrusion are only valid for determining the pore volume of pores accessible to nitrogen or mercury from outside the porous particle. The porosity values ​​specified herein should be understood to refer to the volume of open pores (i.e., pores accessible to fluid from outside the porous particle). In this context, completely enclosed pores that cannot be identified by nitrogen adsorption or mercury intrusion should not be considered when determining porosity values. Likewise, any pore volume located in pores so small as to be below the detection limit of nitrogen adsorption is also not considered.

[0131] The total pore volume of micropores and mesopores measured by nitrogen adsorption can range from 0.4 to 2.2 cm 3 / g, or 0.45 to 2.2 cm 3 / g, or 0.5 to 2cm 3 / g, or 0.55 to 2cm 3 / g, or 0.6 to 1.8 cm 3 / g, or 0.65 to 1.8 cm 3 / g, or 0.7 to 1.6 cm 3 / g, or 0.7 to 1.5 cm 3 / g, or 0.7 to 1.4 cm 3 The use of high porosity particles can be advantageous because it enables a larger amount of silicon to be accommodated within the pore volume.

[0132] The umbrella term “PD n The term "pore size" as used herein refers to the volume nth percentile pore size based on the total volume of micropores and mesopores. For example, as used herein, the term "PD 50 The term "pore size" refers to the pore size below which 50% of the total micropore and mesopore volume is measured.

[0133] PD of porous particles 50 The pore size may be no more than 30 nm, or no more than 25 nm, or no more than 20 nm, or no more than 15 nm, or no more than 12 nm, or no more than 10 nm, or no more than 8 nm, or no more than 6 nm, or no more than 5 nm, or no more than 4 nm, or no more than 3 nm, or no more than 2.5 nm, or no more than 2 nm, or no more than 1.5 nm.

[0134] PD of porous particles 30 The pore size may be no more than 25 nm, or no more than 20 nm, or no more than 15 nm, or no more than 12 nm, or no more than 10 nm, or no more than 8 nm, or no more than 6 nm, or no more than 5 nm, or no more than 4 nm, or no more than 3 nm, or no more than 2.5 nm, or no more than 2 nm, or no more than 1 nm.

[0135] As used herein, the term "particle size" refers to the equivalent spherical diameter (esd), i.e., the diameter of a sphere having the same volume as a given particle, wherein the particle volume is understood to include the volume of any intraparticle pores. As used herein, the term "D 50 ” and “D 50 The term "particle size" refers to the volume median particle size, i.e., the diameter below which 50% of the volume of the particle population is measured.

[0136] Particle size and particle size distribution can be determined by standard laser diffraction techniques according to ISO 13320:2009. Laser diffraction relies on the principle that particles will scatter light at angles that vary depending on the size of the particle, and that a collection of multiple particles will produce a scattered light pattern defined by intensity and angle that can be related to the particle size distribution. A wide variety of laser diffraction instruments are commercially available for rapid and reliable determination of particle size distribution. Unless otherwise stated, particle size distribution measurements indicated or reported herein were obtained by a laser diffraction analyzer from Malvern Instruments. TM The regular Malvern Mastersizer TM Measured by Malvern Mastersizer 3000 particle size analyzer. TM The 3000 particle size analyzer operates by projecting a helium-neon gas laser beam through a transparent cell containing the particles of interest suspended in an aqueous solution. The light impinging on the particles is scattered through angles inversely proportional to the particle size, and an array of photodetectors measures the intensity of the light at a number of predetermined angles, and the measured intensities at different angles are processed by computer using standard theoretical principles to determine the particle size distribution. The laser diffraction values ​​reported herein were calculated using an aqueous solution with 5% by volume of the surfactant SPAN added. TM The particle wet dispersion of 1,4-dihydro- ...

[0137] Usually, the D of porous particles 50 The particle size can be in the range of 0.5 to 200 μm. 50 The particle size may be in the range of 0.5 to 30 μm, or 1 to 25 μm, or 1 to 20 μm, or 2 to 25 μm, or 2 to 20 μm, or 2 to 18 μm, or 2 to 15 μm, or 2 to 12 μm, or 2.5 to 15 μm, or 2.5 to 12 μm, or 2 to 10 μm.

[0138] Porous particles act as a skeleton for silicon, which is generally deposited in the form of multiple silicon domains. As used herein, the term "silicon domain" refers to a silicon body, such as elemental silicon, with a maximum size determined by the size of the pores (such as micropores and / or mesopores) of the porous particles in which they are located. Therefore, the silicon domain can be described as a nano-sized silicon domain, wherein the term "nano-sized" is understood to generally refer to a size less than 100nm. However, due to the size of micropores and mesopores, the maximum size of the silicon domain in any direction is less than 50nm, and is generally significantly less than 50nm. The domain, for example, can take the form of a bounded layer or region of a regular or irregular particle or coating.

[0139] The porous particles preferably comprise a conductive material.The use of conductive porous particles is advantageous because the porous particles form a conductive framework within the composite particles, which facilitates the flow of electrons between the lithium atoms / ions embedded in the silicon and the current collector.

[0140] A preferred type of conductive porous particle is a particle comprising or consisting of a conductive carbon material, which is referred to herein as a conductive porous carbon particle.

[0141] The conductive porous carbon particles preferably contain at least 80% by weight carbon, more preferably at least 90% by weight carbon, more preferably at least 95% by weight carbon, and optionally at least 98% by weight or at least 99% by weight carbon. The carbon may be crystalline carbon or amorphous carbon, or a mixture of amorphous carbon and crystalline carbon. The porous carbon particles may be hard carbon particles or soft carbon particles.

[0142] As used herein, the term "hard carbon" refers to a disordered carbon matrix in which the carbon atoms are found primarily as sp 2 Hybrid state (trigonal bond). The polyaromatic domains are cross-linked using chemical bonds such as C-O-C bonds. Due to the chemical cross-linking between the polyaromatic domains, hard carbon cannot be converted into graphite at high temperatures. Hard carbon has graphite-like properties, which is reflected by the large G band (~1600 cm) in the Raman spectrum. -1 However, the carbon is not completely graphitic, as evidenced by the distinct D band (~1350 cm -1 ) is demonstrated. The graphitic properties of the carbon material can be evaluated by monitoring the peak intensity ratio of the D band to the G band (ID / IG). The porous carbon particles may include an ID / IG of no more than 0.84.

[0143] As used herein, the term "soft carbon" also refers to a disordered carbon matrix in which carbon atoms are found primarily in sp 2The polyaromatic domains in the hybrid state (triangular bonds) are in the size range of 5 to 200 nm. Compared with hard carbon, the polyaromatic domains in soft carbon are associated by intermolecular forces rather than cross-linked by chemical bonds. This means that they will graphitize at high temperatures. The porous carbon particles preferably contain at least 50% sp 2 Hybridized carbon (measured by XPS). For example, the porous carbon particles may suitably contain 50% to 98% sp 2 Hybridized carbon, 55% to 95% sp 2 Hybridized carbon, 60% to 90% sp 2 Hybridized carbon, or 70% to 85% sp 2 Hybridized carbon.

[0144] Suitable porous carbon particles can be prepared by pyrolysis using a variety of different materials. Examples of organic materials that can be used include: plant biomass, including lignocellulosic materials (such as coconut shells, rice husks, wood, etc.), and fossil carbon sources, such as coal. Examples of resins and polymer materials that form porous carbon particles during pyrolysis include: phenolic resins, novolac resins, asphalt, melamine materials, polyacrylate materials, polystyrene materials, polyvinyl alcohol (PVA), polyvinyl pyrrolidone (PVP), and various copolymers of monomer units comprising acrylic ester monomers, styrene monomers, α-olefins, vinyl pyrrolidone and other ethylenically unsaturated monomers. Various carbon materials are available in the art, depending on the raw materials and conditions of the pyrolysis process. Porous carbon particles of various specifications are available from commercial suppliers.

[0145] The porous carbon particles can be subjected to chemical or gas activation processes to increase the volume of the mesopores and micropores. Suitable activation processes include: exposing the pyrolyzed carbon to oxygen, water vapor, CO, CO 2 and one or more of KOH at a temperature in the range of 600 to 1000°C.

[0146] Mesopores can also be obtained by known templating processes using removable pore formers such as MgO and other colloidal or polymer templates that can be removed by thermal or chemical means after pyrolysis or activation.

[0147] Alternatives to carbon-based conductive particles include porous particles comprising titanium nitride (TiN), titanium carbide (TiC), silicon carbide (SiC), nickel oxide (NiOx), titanium silicon nitride (TiSiN), nickel nitride (Ni 3 N), molybdenum nitride (MoN), titanium oxynitride (TiO x N 1-x), silicon oxycarbide (SiOC), boron nitride (BN) or vanadium nitride (VN). Preferably, the porous particles comprise titanium nitride (TiN), silicon oxycarbide (SiOC) or boron nitride (BN).

[0148] The total volume of the micropores and mesopores in the porous particles may be at least 0.45 cm 3 / g, or at least 0.5cm 3 / g, at least 0.55cm 3 / g, or at least 0.6cm 3 / g, or at least 0.65cm 3 / g, or at least 0.7cm 3 / g, or at least 0.75cm 3 / g, or at least 0.8cm 3 / g, at least 0.85cm 3 / g, or at least 0.9cm 3 / g, or at least 0.95cm 3 / g, or at least 1cm 3 / g.

[0149] The internal pore volume of the porous particles may be suitably limited to a value at which the increased fragility of the particle structure outweighs the advantages of increased pore volume to accommodate larger amounts of electroactive material. Preferably, the combined volume of micropores and mesopores in the porous particles does not exceed 2 cm 3 / g, or not more than 1.8cm 3 / g, or not more than 1.6cm 3 / g, or not more than 1.5cm 3 / g, or not more than 1.45cm 3 / g, or not more than 1.4cm 3 / g, or not more than 1.35cm 3 / g, or not more than 1.3cm 3 / g, or not more than 1.25cm 3 / g, or not more than 1.2cm 3 / g, or not more than 1.1, or not more than 1, or not more than 0.95.

[0150] Preferably, the total volume of micropores and mesopores in the porous particles is between 0.45 and 2.2 cm 3 / g, or 0.5 to 2cm 3 / g, or 0.55 to 2cm 3 / g, or 0.6 to 1.8 cm 3 / g, or 0.65 to 1.8 cm 3 / g, or 0.7 to 1.6 cm 3 / g, or 0.7 to 1.5 cm3 / g, or 0.7 to 1.4 cm 3 / g range.

[0151] The total volume of micropores and mesopores in porous particles can also be between 0.55 and 1.4 cm 3 / g, or 0.6 to 1.4 cm 3 / g, or 0.6 to 1.3 cm 3 / g, or 0.65 to 1.3 cm 3 / g, or 0.65 to 1.2 cm 3 / g, or 0.7 to 1.2 cm 3 / g, or 0.7 to 1.1 cm 3 / g, or 0.7 to 1cm 3 / g, or 0.75 to 0.95 cm 3 / g range.

[0152] The total volume of micropores and mesopores in porous particles can also be between 0.4 and 0.75 cm 3 / g, or 0.4 to 0.7 cm 3 / g, or 0.4 to 0.65cm 3 / g, 0.45 to 0.75 cm 3 / g, or 0.45 to 0.7 cm 3 / g, or 0.45 to 0.65cm 3 / g, or 0.45 to 0.6 cm 3 / g range.

[0153] The total volume of micropores and mesopores in porous particles can also be between 0.6 and 2 cm 3 / g, or 0.6 to 1.8 cm 3 / g, or 0.7 to 1.8 cm 3 / g, or 0.7 to 1.6 cm 3 / g, or 0.8 to 1.6 cm 3 / g, or 0.8 to 1.5 cm 3 / g, or 0.8 to 1.4 cm 3 / g, or 0.9 to 1.5cm 3 / g, or 0.9 to 1.4 cm 3 / g, or 1 to 1.4cm 3 / g range.

[0154] PD of porous particles 90The pore size may be no more than 35 nm, or no more than 30 nm, or no more than 25 nm, or no more than 20 nm, or no more than 15 nm, or no more than 12 nm, or no more than 10 nm, or no more than 8 nm, or no more than 6 nm, or no more than 5 nm, or no more than 4 nm, or no more than 3 nm, or no more than 2.5 nm, or no more than 2 nm. Preferably, the PD of the porous particle 90 The pore size is at least 2.5 nm, or at least 3 nm, or at least 3.5 nm, or at least 4 nm. For example, the PD of the porous particle 90 The pore size is preferably in the range of 2.5 to 20 nm, or 3 to 15 nm, or 3.5 to 10 nm, or 4 to 8 nm.

[0155] PD of porous particles 10 The pore size may be no more than 10 nm, or no more than 9 nm, or no more than 8 nm, or no more than 7 nm, or no more than 6 nm, or no more than 5 nm, or no more than 4 nm, or no more than 3 nm, or no more than 2.5 nm, or no more than 2 nm, or no more than 1.5 nm, or no more than 1 nm. Preferably, the PD of the porous particle is 10 The pore size is at least 0.3 nm, or at least 0.4 nm, or at least 0.5 nm. For example, the PD of the porous particle 10 The pore size is preferably in the range of 0.3 to 10 nm, or 0.3 to 5 nm, or 0.3 to 1 nm, or 0.4 to 1 nm, or 0.5 to 1 nm.

[0156] For the avoidance of doubt, in order to determine the PD n value, without taking into account any macropore volume (pores larger than 50 nm).

[0157] The volume ratio of micropores to mesopores in the porous particles can in principle be in the range of 100:0 to 0: 100. Preferably, the volume ratio of micropores to mesopores is 90:10 to 55:45, or 90:10 to 60:40, or 85:15 to 65:35.

[0158] The pore size distribution of the porous particles may be unimodal, bimodal or multimodal. As used herein, the term "pore size distribution" relates to the distribution of pore sizes of the porous particles relative to the cumulative total internal pore volume. Bimodal or multimodal pore size distributions may be preferred because the close proximity between micropores and pores with larger diameters provides the advantage of efficient ion transport from the porous network to the electroactive material.

[0159] As used herein, the term "D 10 ” and “D 10The term "particle size" as used herein refers to the 10th percentile volume median particle size, i.e., the diameter at which 10% of the volume of the particle population is below a certain diameter. 90 ” and “D 90 The term "particle size" refers to the 90th percentile volume median particle size, i.e., the diameter below which 90% of the volume of the particle population is measured.

[0160] Optionally, the D of the porous particle 50 The particle size may be at least 1 μm, or at least 1.5 μm, or at least 2 μm, or at least 2.5 μm, or at least 3 μm, or at least 4 μm, or at least 5 μm. Optionally, the D 50 The particle size may be no more than 150 μm, or no more than 100 μm, or no more than 70 μm, or no more than 50 μm, or no more than 40 μm, or no more than 30 μm, or no more than 25 μm, or no more than 20 μm, or no more than 18 μm, or no more than 15 μm, or no more than 12 μm, or no more than 10 μm, or no more than 8 μm.

[0161] For example, the D 50 The particle size may be in the range of 0.5 to 150 μm, or 0.5 to 100 μm, or 0.5 to 50 μm, or 0.5 to 30 μm, or 1 to 25 μm, or 1 to 20 μm, or 2 to 25 μm, or 2 to 20 μm, or 2 to 18 μm, or 2 to 15 μm, or 2 to 12 μm, or 2.5 to 15 μm, or 2.5 to 12 μm, or 2 to 10 μm, or 3 to 20 μm, or 3 to 18 μm, or 3 to 15 μm, or 4 to 18 μm, or 4 to 15 μm, or 4 to 12 μm, or 5 to 15 μm, or 5 to 12 μm, or 5 to 10 μm, or 5 to 8 μm. Particles within these size ranges and having the porosity and pore size distribution described herein are ideally suited for making composite particles for use in anodes of metal ion batteries by the CVI process.

[0162] D of porous particles 10 The particle size is preferably at least 0.2 μm, or at least 0.5 μm, or at least 0.8 μm, or at least 1 μm, or at least 1.5 μm, or at least 2 μm. 10 The particle size is maintained above 0.2 μm, reducing the possibility of undesirable agglomeration of submicron-sized particles and improving the dispersibility of the formed composite particles.

[0163] D of porous particles 90The particle size is preferably no more than 300 μm, or no more than 250 μm, or no more than 200 μm, or no more than 150 μm, or no more than 100 μm, or no more than 80 μm, or no more than 60 μm, or no more than 40 μm, or no more than 30 μm, or no more than 25 μm, or no more than 20 μm.

[0164] The porous particles preferably have a narrow size distribution span. For example, the particle size distribution span (defined as (D 90 -D 10 ) / D 50 ) is preferably 5 or less, more preferably 4 or less, more preferably 3 or less, more preferably 2 or less, and most preferably 1.5 or less. By maintaining a narrow size distribution span, efficient packing of particles into a dense powder bed can be more easily achieved.

[0165] The average sphericity (as defined herein) of the porous particles may exceed 0.5. Preferably, their average sphericity is at least 0.55, or at least 0.6, or at least 0.65, or at least 0.7, or at least 0.75, or at least 0.8, or at least 0.85. Preferably, the average sphericity of the porous particles is at least 0.90, or at least 0.92, or at least 0.93, or at least 0.94, or at least 0.95. Spherical particles are believed to contribute to uniformity of deposition and at the same time facilitate denser packing in the reaction zone and in the final product when incorporated into an electrode.

[0166] Highly accurate two-dimensional projections of micrometer-scale particles can be obtained by scanning electron microscopy (SEM) or by dynamic image analysis, where a digital camera is used to record the shadow of the particle projection. The term "sphericity" as used herein is understood to be the ratio of the area of ​​the particle projection (obtained by such imaging techniques) to the area of ​​a circle, where the particle projection and the circle have the same circumference. Thus, for an individual particle, the sphericity S can be defined as:

[0167]

[0168] Among them A m is the measured area of ​​the particle projection, and C m is the measured circumference of the particle projection. As used herein, the average sphericity S of a plurality of particles av is defined as:

[0169]

[0170] wherein n represents the number of particles in the population. The average sphericity of the plurality of particles is preferably calculated from two-dimensional projections of at least 50 particles.

[0171] The BET surface area of ​​the porous particles may be at least 100 m2 / g, or at least 500m 2 / g, or at least 750m 2 / g, or at least 1,000m 2 / g, or at least 1,250m 2 / g, or at least 1,500m 2 / g. The BET surface area of ​​the porous particles may not exceed 4,000 m 2 / g, or not more than 3,500m 2 / g, or not more than 3,250m 2 / g, or not more than 3,000m 2 / g, or not more than 2,500m 2 / g, or not more than 2,000m 2 / g. For example, the BET surface area of ​​a porous particle can be 100m 2 / g to 4,000m 2 / g, or 500m 2 / g to 4,000m 2 / g, or 750m 2 / g to 3,500m 2 / g, or 1,000m 2 / g to 3,250m 2 / g, or 1,000m 2 / g to 3,000m 2 / g, or 1,000m 2 / g to 2,500m 2 / g, or 1,000m 2 / g to 2,000m 2 / g range.

[0172] The particle density of the porous particles is preferably at least 0.35 and preferably less than 3 g / cm 3 , more preferably less than 2g / cm 3 , more preferably less than 1.5 g / cm 3 , most preferably 0.35 to 1.2 g / cm 3 As used herein, the term "particle density" refers to the "apparent particle density" measured by mercury porosimetry (i.e., the mass of the particle divided by the particle volume, where the particle volume is taken to be the sum of the volume of the solid material and any closed pores or blind pores ("blind pores" are pores that are too small to be measured by mercury porosimetry). Preferably, the particle density of the porous particles is at least 0.4 g / cm 3 , or at least 0.45g / cm 3 , or at least 0.5g / cm 3 , or at least 0.55g / cm 3, or at least 0.6g / cm 3 , or at least 0.65g / cm 3 , or at least 0.7g / cm 3 Preferably, the particle density of the porous particles does not exceed 1.15 g / cm 3 , or not more than 1.1g / cm 3 , or not more than 1.05g / cm 3 , or not more than 1g / cm 3 , or not more than 0.95g / cm 3 , or not more than 0.9g / cm 3 .

[0173] Preferably, the porous particles have:

[0174] (i) 0.4 to 2.2 cm 3 The total pore volume of micropores and mesopores measured by nitrogen adsorption in the range of 1 / g;

[0175] (ii) PD no larger than 20nm 50 Pore ​​size, preferably no more than 30nm PD 90 Pore ​​size, preferably no more than 15 nm PD 30 Aperture;

[0176] (iii) D in the range of 0.5 to 30 μm 50 Particle size.

[0177] More preferably, the porous particles have a BET surface area of ​​1,000 to 3,000 m 2 / g.

[0178] More preferably, the porous particles have:

[0179] (i) 0.6 to 1.8 cm 3 The total pore volume of micropores and mesopores measured by nitrogen adsorption in the range of 1 / g;

[0180] (ii) PDs not exceeding 10nm 50 Pore ​​size, preferably no more than 20 nm PD 90 Pore ​​size, preferably no more than 8nm PD 30 Aperture; and

[0181] (iii) D in the range of 1 to 25 μm 50 Particle size.

[0182] More preferably, the porous particles have a BET surface area of ​​1,000 to 3,000 m 2 / g.

[0183] More preferably, the porous particles have:

[0184] (i) 0.7 to 1.6 cm 3 The total pore volume of micropores and mesopores measured by nitrogen adsorption in the range of 1 / g;

[0185] (ii) PDs not exceeding 10nm 50 Pore ​​size, preferably no more than 20 nm PD 90 Pore ​​size, preferably no more than 8nm PD 30 Aperture; and

[0186] (iii) D in the range of 1 to 20 μm 50 Particle size.

[0187] More preferably, the porous particles have a BET surface area of ​​1,000 to 3,000 m 2 / g.

[0188] More preferably, the porous particles have:

[0189] (i) 0.7 to 1.5 cm 3 The total pore volume of micropores and mesopores measured by nitrogen adsorption in the range of 1 / g;

[0190] (ii) PD no larger than 5nm 50 Pore ​​size, preferably no more than 10 nm PD 90 Pore ​​size, preferably no more than 3nm PD 30 Aperture; and

[0191] (iii) D in the range of 2 to 20 μm 50 Particle size.

[0192] More preferably, the porous particles have a BET surface area of ​​1,000 to 3,000 m 2 / g.

[0193] More preferably, the porous particles have:

[0194] (i) 0.7 to 1.4 cm 3 The total pore volume of micropores and mesopores measured by nitrogen adsorption in the range of 1 / g;

[0195] (ii) PD no larger than 5nm 50 Pore ​​size, preferably no more than 10 nm PD 90 Pore ​​size, preferably no more than 3nm PD 30 Aperture; and

[0196] (iii) D in the range of 2 to 20 μm 50 Particle size.

[0197] More preferably, the porous particles have a BET surface area of ​​1,000 to 2,500 m 2 / g.

[0198] More preferably, the porous particles have:

[0199] (i) 0.7 to 1.4 cm 3 The total pore volume of micropores and mesopores measured by nitrogen adsorption in the range of 1 / g;

[0200] (ii) PD no larger than 5nm 50 Pore ​​size, preferably no more than 10 nm PD 90 Pore ​​size, preferably no more than 3nm PD 30 Aperture; and

[0201] (iii) D in the range of 2 to 18 μm 50 Particle size.

[0202] More preferably, the porous particles have a BET surface area of ​​1,000 to 2,500 m 2 / g.

[0203] More preferably, the porous particles have:

[0204] (i) 0.7 to 1.4 cm 3 The total pore volume of micropores and mesopores measured by nitrogen adsorption in the range of 1 / g;

[0205] (ii) PD no larger than 2nm 50 Pore ​​size, preferably no more than 5 nm PD 90 Pore ​​size, preferably no more than 1 nm PD 30 Aperture; and

[0206] (iii) D in the range of 2 to 15 μm 50 Particle size.

[0207] More preferably, the porous particles have a BET surface area of ​​1,000 to 2,500 m 2 / g.

[0208] In the case where the silicon-containing precursor is a chlorinated compound such as chlorosilane, the silicon-containing precursor may be used in admixture with hydrogen, preferably at an atomic ratio of hydrogen to chlorine of at least 1:1.

[0209] Optionally, the silicon-containing precursor is free of chlorine. Chlorine-free means that the silicon-containing precursor contains less than 1 wt%, preferably less than 0.1 wt%, preferably less than 0.01 wt% of chlorine-containing compounds.

[0210] The temperature effective to cause silicon deposition in steps (b) and (d) is any temperature effective to decompose the silicon-containing precursor to form silicon. Preferably, the temperature effective to cause silicon deposition in steps (b) and (d) is 340 to 400°C, or 340 to 395°C, or 340 to 390°C, or 345 to 400°C, or 345 to 395°C, or 345 to 390°C, or 350 to 400°C, or 350 to 395°C, or 350 to 390°C, or 350 to 385°C, or 350 to 380°C, or 355 to 400°C, or 355 to 395°C, or 355 to 390°C, or 355 to 390°C. The temperature range of 370 to below 395° C. is particularly preferred.

[0211] The deposition of silicon by CVI results in the elimination of byproducts, particularly byproduct gases such as hydrogen. Step (c) preferably comprises at least separating the byproducts from the formed intermediate particles. The separation of the byproducts from the formed intermediate particles can be achieved by flushing the reaction zone with an inert gas and / or by discharging the reaction zone by reducing the pressure. For example, the separation of the byproducts from the formed intermediate particles can be achieved by evacuating the reaction zone to a pressure lower than 100 kPa, or lower than 80 kPa, or lower than 60 kPa, or lower than 40 kPa, or lower than 20 kPa, or lower than 10 kPa, or lower than 5 kPa, or lower than 2 kPa, or lower than 10 kPa. Evacuating the reaction zone to a low pressure can not only effectively remove the byproducts in the gas phase, but also effectively desorb any byproducts that may be adsorbed on the surface of the deposited silicon.

[0212] According to a preferred embodiment of the present invention:

[0213] (i) The BET surface area of ​​the porous particles is 500 m 2 / g to 4,000m 2 / g range,

[0214] (ii) ΔT≤+80°C in step (b)

[0215] (iii) maintaining the plurality of porous particles at a temperature in the range of 340 to 395° C. during step (b);

[0216] (iv) the volume of the plurality of porous particles in the reaction zone of step (a) is at least 100 cm 3 / L RV ;as well as

[0217] (v) Step (b) comprises continuously stirring the porous particles.

[0218] According to another preferred embodiment of the present invention:

[0219] (i) The BET surface area of ​​the porous particles is 750 m 2 / g to 3,500m 2 / g range,

[0220] (ii) ΔT≤+60°C in step (b)

[0221] (iii) maintaining the plurality of porous particles at a temperature in the range of 350 to 395° C. during step (b);

[0222] (iv) the volume of the plurality of porous particles in the reaction zone of step (a) is at least 200 cm 3 / L RV ;as well as

[0223] (v) Step (b) comprises continuously stirring the porous particles.

[0224] According to another preferred embodiment of the present invention:

[0225] (i) The BET surface area of ​​the porous particles is 1,000 m 2 / g to 3,250m 2 / g range,

[0226] (ii) ΔT≤+40°C in step (b)

[0227] (iii) maintaining the plurality of porous particles at a temperature in the range of 360 to 395° C. during step (b);

[0228] (iv) the volume of the plurality of porous particles in the reaction zone of step (a) is at least 300 cm 3 / L RV ;as well as

[0229] (v) Step (b) comprises continuously stirring the porous particles.

[0230] According to another preferred embodiment of the present invention:

[0231] (i) The BET surface area of ​​the porous particles is 1,000 m 2 / g to 3,000m 2 / g range,

[0232] (ii) ΔT≤+20°C in step (b)

[0233] (iii) maintaining the plurality of porous particles at a temperature in the range of 370 to 395° C. during step (b);

[0234] (iv) the volume of the plurality of porous particles in the reaction zone of step (a) is at least 400 cm 3 / L RV ;as well as

[0235] (v) Step (b) comprises continuously stirring the porous particles.

[0236] According to another preferred embodiment of the present invention:

[0237] (i) The BET surface area of ​​the porous particles is 1,000 m 2 / g to 2,500m 2 / g range,

[0238] (ii) ΔT≤+10°C in step (b)

[0239] (iii) maintaining the plurality of porous particles at a temperature in the range of 370 to 390° C. during step (b);

[0240] (iv) the volume of the plurality of porous particles in the reaction zone of step (a) is at least 500 cm 3 / L RV ;as well as

[0241] (v) Step (b) comprises continuously stirring the porous particles.

[0242] According to a preferred embodiment of the present invention:

[0243] (i) The BET surface area of ​​the porous particles is 500 m 2 / g to 4,000m 2 / g range,

[0244] (ii) ΔT≤+80°C in step (b)

[0245] (iii) maintaining the plurality of porous particles at a temperature in the range of 340 to 395° C. during step (b);

[0246] (iv) the ratio of the internal surface area of ​​the reaction zone in step (a) to the mass of the porous particles in the reaction zone is no more than 1 m 2 / kg; and

[0247] (v) Step (b) comprises continuously stirring the porous particles.

[0248] According to another preferred embodiment of the present invention:

[0249] (i) The BET surface area of ​​the porous particles is 750 m 2 / g to 3,500m 2 / g range,

[0250] (ii) ΔT≤+60°C in step (b)

[0251] (iii) maintaining the plurality of porous particles at a temperature in the range of 350 to 395° C. during step (b);

[0252] (iv) the ratio of the internal surface area of ​​the reaction zone in step (a) to the mass of the porous particles in the reaction zone is not more than 0.8 m 2 / kg; and

[0253] (v) Step (b) comprises continuously stirring the porous particles.

[0254] According to another preferred embodiment of the present invention:

[0255] (i) The BET surface area of ​​the porous particles is 1,000 m 2 / g to 3,250m 2 / g range,

[0256] (ii) ΔT≤+40°C in step (b)

[0257] (iii) maintaining the plurality of porous particles at a temperature in the range of 360 to 395° C. during step (b);

[0258] (iv) the ratio of the internal surface area of ​​the reaction zone in step (a) to the mass of the porous particles in the reaction zone is not more than 0.6 m 2 / kg; and

[0259] (v) Step (b) comprises continuously stirring the porous particles.

[0260] According to another preferred embodiment of the present invention:

[0261] (i) The BET surface area of ​​the porous particles is 1,000 m 2 / g to 3,000m 2 / g range,

[0262] (ii) ΔT≤+20°C in step (b)

[0263] (iii) maintaining the plurality of porous particles at a temperature in the range of 370 to 395° C. during step (b);

[0264] (iv) The ratio of the internal surface area of the reaction zone in step (a) to the mass of the porous particles in the reaction zone does not exceed 0.4 m 2 / kg; and

[0265] (v) Step (b) includes continuously stirring the porous particles.

[0266] According to another preferred embodiment of the present invention:

[0267] (i) The BET surface area of the plurality of porous particles is in the range of 1,000 m 2 / g to 2,500 m 2 / g,

[0268] (ii) ΔT in step (b) ≤ +10 °C

[0269] (iii) During step (b), the plurality of porous particles are maintained in a temperature range of 370 to 390 °C;

[0270] (iv) The ratio of the internal surface area of the reaction zone in step (a) to the mass of the porous particles in the reaction zone does not exceed 0.2 m 2 / kg; and

[0271] (v) Step (b) includes continuously stirring the porous particles.

[0272] The method of the present invention may further include the following step:

[0273] Forming a modification material on the surface of the silicon deposited in step (b) and / or step (d).

[0274] The modification material may be a passivation layer formed on the surface of the silicon deposited in step (b) or (d). Thus, the method may further include contacting the particles from step (b) or (d) with a passivating agent. As defined herein, a passivating agent is a compound or mixture of compounds capable of reacting with the surface of the deposited silicon to form a modified surface.

[0275] One type of passivation layer is a native oxide layer. The native oxide layer can be formed, for example, by exposing the surface of the silicon to a passivating agent selected from air or other oxygen-containing gases. This passivation layer may contain silicon oxide of the formula SiO x where 0 < x ≤ 2. The silicon oxide is preferably amorphous silicon oxide. The formation of the native oxide layer is exothermic, so careful process control is required to prevent overheating or even combustion of the particulate material. In the case where the formed modification material is a native oxide layer, the method may include: before contacting the surface of the silicon domain with the oxygen-containing gas, cooling the material formed in step (b) or (d) to a temperature below 300 °C, preferably below 200 °C, optionally below 100 °C.

[0276] Another type of passivation layer is a nitride layer formed, for example, by exposing the surface of silicon to a passivating agent selected from ammonia or other nitrogen-containing molecules. The passivation layer may comprise silicon nitride of the formula SiN x where 0 < x ≤ 4 / 3. The silicon nitride is preferably amorphous silicon nitride. The nitride layer can be formed by contacting the surface of the silicon domain with ammonia at a temperature in the range of 200 - 700 °C, preferably 400 - 700 °C, more preferably 400 - 600 °C. Then, the temperature can be raised to the range of 500 to 1,000 °C if necessary to form a nitride surface (e.g., a silicon nitride surface of the formula SiNx where x ≤ 4 / 3). Nitride passivation can be superior to oxide passivation. Since sub-stoichiometric nitrides (such as SiN x where 0 < x ≤ 4 / 3) are conductive, the nitride interlayer acts as a conductive network that allows for faster charging and discharging of the silicon. As a phosphorus analogue of ammonia, phosphine can also be used as a passivating agent.

[0277] Another type of passivation layer is an oxynitride layer formed, for example, by exposing the surface of silicon to a passivating agent comprising ammonia (or other nitrogen-containing molecules) and oxygen. The passivation layer may comprise silicon oxynitride of the formula SiO x N y where 0 < x < 2, 0 < y < 4 / 3, and 0 < (2x + 3y) ≤ 4). The silicon nitride is preferably amorphous silicon oxynitride.

[0278] Another type of passivation layer is a carbide layer. The passivation layer may comprise silicon carbide of the formula SiC x where 0 < x ≤ 1. The silicon carbide is preferably amorphous silicon carbide. The carbide layer can be formed by contacting the surface of silicon with a passivating agent selected from carbon-containing precursors (such as methane or ethylene) at a high temperature in the range of 250 to 700 °C. At lower temperatures, covalent bonds are formed between the surface of the silicon and the carbon-containing precursor, which transforms into a single crystal silicon carbide monolayer as the temperature increases. The modified material domain may comprise silicon carbide of the formula SiCx where 0 < x ≤ 1.

[0279] Other suitable passivating agents include: compounds containing alkene, alkyne or carbonyl functional groups, more preferably terminal alkenes, terminal alkynes, aldehyde groups or ketone groups.

[0280] Preferred passivating agents include one or more compounds having the following formula:

[0281] (i) R 1 -CH=CH-R 1 ;

[0282] (ii) R 1-C≡CR 1 ;as well as

[0283] (iii) O=CR 1 R 1 ;

[0284] Each R 1 independently represent H or an unsubstituted or substituted aliphatic or aromatic hydrocarbon group having 1 to 20 carbon atoms, or two R 1 The groups form unsubstituted or substituted ring structures containing from 3 to 8 carbon atoms in the ring.

[0285] Particularly preferred deactivators include one or more compounds having the formula:

[0286] (i)CH 2 =CH-R 1 ;as well as

[0287] (ii) HC≡CR 1 ;

[0288] Where R 1 As defined above. Preferably, R 1 is unsubstituted.

[0289] Examples of suitable deactivators include: ethylene, propylene, 1-butene, butadiene, 1-pentene, 1,4-pentadiene, 1-hexene, 1-octene, styrene, divinylbenzene, acetylene, phenylacetylene, norbornene, norbornadiene and bicyclo[2.2.2]oct-2-ene. Optionally, mixtures of different deactivators can also be used.

[0290] It is believed that the passivating agent containing olefin, alkyne or carbonyl groups undergoes an insertion reaction with MH groups (wherein M represents a silicon atom) on the silicon surface to form a covalently passivated surface resistant to air oxidation. The passivation reaction between the silicon surface and the passivating agent can be understood as a form of hydrosilylation, as schematically shown below.

[0291]

[0292] Other suitable passivating agents include compounds containing active hydrogen atoms bonded to oxygen, nitrogen, sulfur or phosphorus. For example, the passivating agent may be an alcohol, an amine, a thiol or a phosphine. The reaction of the group -XH with the hydride groups on the silicon surface is understood to result in H 2 elimination of X and formation of a direct bond between X and the silicon surface.

[0293] Suitable deactivators within this class include compounds having the formula:

[0294] (iv)HX-R2 ,as well as

[0295] (v)HX-C(O)-R 1 ,

[0296] Where X represents O, S, NR 1 or PR 1 ; Each R 1 are independently as defined above; and R 2 represents an unsubstituted or substituted aliphatic or aromatic hydrocarbon group having 1 to 20 carbon atoms, or R 1 and R 2 Together they form an unsubstituted or substituted ring structure containing from 3 to 8 carbon atoms in the ring.

[0297] Preferably, X represents O or NH.

[0298] Preferably, R 2 represents an optionally substituted aliphatic or aromatic group having 2 to 10 carbon atoms. The amine group may also be incorporated into a 4-10 membered aliphatic or aromatic ring structure, as in pyrrolidine, pyrrole, imidazole, piperazine, indole or purine.

[0299] Contacting of silicon with the passivating agent may be carried out at a temperature in the range of 25 to 700°C, preferably in the range of 50 to 500°C, more preferably in the range of 100 to 300°C.

[0300] The modified material formed may optionally comprise a pyrolytic carbon material deposited onto the surface of the silicon by thermal decomposition of a carbon-containing precursor (i.e., by chemical vapor infiltration (CVI)). Deposition of the pyrolytic carbon material may be advantageous because it forms a conductive network between the silicon domains, which may facilitate electron transport within the composite particle. Thus, the method may comprise contacting the intermediate particles from step (b) or (d) with a carbon-containing precursor (preferably a hydrocarbon) at a temperature effective to cause deposition of the pyrolytic carbon material in the pores of the intermediate particles.

[0301] Suitable hydrocarbons include polycyclic hydrocarbons containing 10 to 25 carbon atoms and optionally 1 to 3 heteroatoms, optionally wherein the polyaromatic hydrocarbon is selected from naphthalene, substituted naphthalenes (such as dihydroxynaphthalene), anthracene, tetracene, pentacene, fluorene, acenapthene, phenanthrene, fluoranthene, pyrene, , perylene, coronene, fluorenone, anthraquinone, anthrone and their alkyl substituted derivatives. Suitable pyrolytic carbon precursors also include bicyclic monoterpenes, optionally wherein the bicyclic monoterpenes are selected from camphor, borneol, eucalyptol, camphene, careen, sabinene, limonene and pinene. Other suitable pyrolytic carbon precursors include C 2 -C 10A hydrocarbon, optionally wherein the hydrocarbon is selected from alkanes, alkenes, alkynes, cycloalkanes, cycloalkenes and aromatic hydrocarbons, such as methane, ethylene, propylene, limonene, styrene, cyclohexane, cyclohexene, α-terpinene and acetylene. Other suitable pyrolytic carbon precursors include phthalocyanine, sucrose, starch, graphene oxide, reduced graphene oxide, pyrene, perhydropyrene, 9,10-triphenylene, tetracene, benzopyrene, perylene, coronene and A preferred carbon precursor is acetylene.

[0302] Temperatures suitable for deposition of pyrolytic carbon materials are in the range of 300 to 800°C, or 400 to 700°C. For example, the temperature may be no more than 680°C, or no more than 660°C, or no more than 640°C, or no more than 620°C, or no more than 600°C, or no more than 580°C, or no more than 560°C, or no more than 540°C, or no more than 520°C, or no more than 500°C. The minimum temperature will depend on the type of carbon precursor used. Preferably, the temperature is at least 300°C, or at least 350°C, or at least 400°C, or at least 450°C, or at least 500°C.

[0303] The carbon-containing precursor used can be used in pure form or as a mixture diluted with an inert carrier gas such as nitrogen or argon. For example, the carbon-containing precursor can be used in an amount ranging from 0.1% to 100% by volume, or from 0.5% to 20% by volume, or from 1% to 10% by volume, or from 1% to 5% by volume, based on the total volume of the precursor and the inert carrier gas. The presence of oxygen should be minimized to prevent undesired oxidation of the deposited electroactive material. Preferably, the oxygen content is less than 0.01% by volume, more preferably less than 0.001% by volume, based on the total volume of the gas.

[0304] In the case of depositing pyrolytic carbon material, the same compound can act as a passivator and a pyrolytic carbon precursor at the same time. For example, if styrene is selected as the pyrolytic carbon precursor, styrene will also act as a passivator if the intermediate particles from step (b) are not exposed to oxygen before contacting with styrene. In this case, the passivation in the step and the deposition of the conductive carbon material can be carried out simultaneously, for example, at a temperature in the range of 300-700°C. Alternatively, the deposition of the passivation and conductive carbon material can be carried out in sequence, and the same material is used as the passivator and the pyrolytic carbon precursor, but wherein the deposition of the pyrolytic carbon precursor is carried out at a temperature higher than the passivation. For example, the passivation can be carried out at a temperature in the range of 25°C to less than 300°C, and the deposition of pyrolytic carbon can be carried out at a temperature in the range of 300-700°C. These two steps can be suitably carried out in sequence by raising the temperature while maintaining contact with the compound that acts as the passivator and the pyrolytic carbon precursor at the same time. At lower temperatures (for example, in the range of 25°C to <300°C), passivation will be the main process. As the temperature increases (eg, to 300-700° C.), deposition of pyrolytic carbon will ensue.

[0305] A range of different silicon loadings in composite particles can be obtained using the method of the present invention. For example, based on the total mass of the composite particles, the amount of silicon in the composite particles can be in the range of 5 to 85 wt %. Preferably, based on the total mass of the composite particles, the amount of silicon in the composite particles is 10 to 85 wt %, or 15 to 85 wt %, or 20 to 80 wt %, or 25 to 80 wt %, or 30 to 75 wt %, or 35 to 75 wt %, or 40 to 70 wt %, or 45 to 65 wt %. The total silicon loading in the composite particles is the sum of the silicon deposited in steps (b) and (d) (including repetitions of step (d)).

[0306] The amount of silicon in the composite particles is preferably selected so that at least 20% to 90% of the internal pore volume of the porous particles is occupied by silicon. For example, silicon can occupy 20% to 80%, or 25% to 75%, or 30% to 70%, or 35 to 65%, or 40 to 60%, or 45% to 55% of the internal pore volume of the porous particles. Within these preferred ranges, the remaining pore volume of the porous particles effectively accommodates the expansion of silicon during charge and discharge without large excess pore volume, which is detrimental to the volumetric capacity of the granular particles. However, the amount of silicon is not too high, not so high as to hinder effective lithiation due to insufficient metal ion diffusion rate or mechanical resistance to lithiation due to insufficient expansion volume.

[0307] By requiring the mass ratio of silicon to porous particles to be [0.5×P 1 To 1.9×P 1]:1, the amount of silicon in the composite particles can be related to the available pore volume in the porous particles, where P 1 is the total pore volume of micropores and mesopores in porous particles (in cm 3 / g) (for example, if the total volume of the micropores and mesopores of a porous particle is 1.2 cm 3 / g, then P 1 = 1.2). This relationship takes into account the density of silicon and the pore volume of the porous particles to define a weight ratio of silicon at which the occupied pore volume is approximately 20% to 82%.

[0308] The amount of silicon in the composite particles may be determined by elemental analysis.Preferably, elemental analysis is used to determine the elemental composition of the individual porous particles and the composition of the composite particles.

[0309] The silicon content is preferably determined by ICP-OES (Inductively Coupled Plasma - Optical Emission Spectroscopy). A variety of ICP-OES instruments are commercially available, such as The carbon content (and, if desired, the hydrogen content, nitrogen content and oxygen content) of the composite particles and the porous carbon particles themselves is preferably determined by IR absorption. A suitable instrument for determining the carbon content, hydrogen content, nitrogen content and oxygen content is Micro Elemental Analyzer (available from Leco Corporation).

[0310] Preferably at least 90 wt%, more preferably at least 95 wt%, even more preferably at least 98 wt% of the silicon in the composite particles is located within the internal pore volume of the porous particles, so that no or very little silicon is located on the outer surface of the composite particles. As discussed above, deposition of silicon in the CVI process occurs on the surface of the porous particles.

[0311] The method of the present invention may further comprise the following steps:

[0312] (e) forming a plurality of modified material domains in the pores and / or on the outer surface of the composite particles from step (b) or (d).

[0313] Step (e) is performed immediately after the last silicon deposition step (i.e., step (b), or step (d), or the last repetition of step (d) in the case of repeated steps (c) and (d). The formation of the modified material domain is similar to the steps described above, except that step (e) is performed after the last silicon deposition step, while the previous step can be performed between consecutive electroactive material deposition steps.

[0314] Any of the modifying materials and deposition conditions disclosed herein are suitable for both steps.

[0315] The modifying material domain formed in step (e) may comprise the same or different modifying material as the modifying material domain formed in the previous step.

[0316] Optionally, step (e) comprises contacting the composite particles from step (b) or (d) with a passivating agent.Preferred passivating agents and passivating conditions are as set out above.

[0317] Optionally, step (e) comprises depositing a lithium ion permeable material into the pores and / or on the outer surface of the composite particles from step (b) or (d). This provides a further improvement in the performance of the composite particles when used as electroactive materials in lithium ion batteries by reducing the surface area of ​​the composite particles and by sealing the electroactive material domains away from electrolyte access.

[0318] The lithium ion permeable material may be deposited immediately after the last electroactive material deposition step. Alternatively, the lithium ion permeable material may be deposited after a first passivation step as in step (e) discussed above.

[0319] One suitable lithium ion permeable material is a pyrolytic carbon material. The pyrolytic carbon material can be obtained by chemical vapor infiltration (CVI), that is, by thermally decomposing a volatile carbon-containing gas (such as ethylene) onto the surface of the composite particles.

[0320] A suitable process for depositing the pyrolytic carbon material comprises: combining the composite particles from step (b) or (d) with a pyrolytic carbon precursor; and heating the pyrolytic carbon precursor to a temperature effective to cause deposition of the pyrolytic conductive carbon material into the pores and / or external surfaces of the composite particles.

[0321] Preferred pyrolytic carbon precursors and pyrolysis conditions are as described above.

[0322] In the case where the lithium ion permeable material is a pyrolytic carbon material, in step (e), the same compound can act as both a passivating agent and a pyrolytic carbon precursor. Suitable conditions for passivating and forming a pyrolytic carbon material using the same compound as a passivating agent and a pyrolytic carbon precursor in step (e) are as described above.

[0323] Alternatively, different compounds may be used as the passivating agent and the pyrolytic carbon precursor in step (e). For example, the passivating agent may be styrene and the pyrolytic carbon precursor may be a compound such as cyclohexane that is capable of forming a pyrolytic carbon material but is unable to passivate the silicon surface.

[0324] The composite particles obtained by the process of the invention can be characterized by their performance under thermogravimetric analysis (TGA) in air. This analytical method relies on the principle that a weight increase is observed when silicon is oxidized in air and at elevated temperatures.

[0325] As defined herein, "surface silicon" is calculated from the initial mass increase in the TGA trace from the minimum value at 150°C to 500°C to the maximum mass measured in the temperature range of 550°C to 650°C, wherein the TGA is performed in air at a heating rate of 10°C / min. This mass increase is believed to be due to oxidation of the surface silicon, thus enabling the percentage of surface silicon to be determined as a proportion of the total amount of silicon according to the following formula:

[0326] Y=1.875×[(M max –M min ) / M f ]×100%

[0327] Where Y is the percentage of surface silicon (as a proportion of the total silicon in the sample), M max is the maximum mass of the sample measured in the temperature range of 550°C to 650°C, M min is the minimum mass of the sample above 150°C and below 500°C, and M f is the mass of the sample at 1400°C when oxidation is complete. For completeness, it should be understood that 1.875 is SiO 2 With O 2 The molar mass ratio (i.e. the SiO 2 Typically, TGA analysis is performed using a sample amount of 10 mg ± 2 mg.

[0328] It has been found that when the surface silicon measured by the above TGA method is at least 20% by weight of the total amount of silicon in the material, the reversible capacity retention over multiple charge / discharge cycles is significantly improved. Preferably, at least 22% by weight, or at least 25% by weight, at least 30% by weight of silicon, or at least 35% by weight of silicon, or at least 40% by weight of silicon, or at least 45% by weight of silicon is surface silicon as measured by thermogravimetric analysis (TGA).

[0329] In addition to the surface silicon content, the silicon-containing composite particles obtained by the process of the present invention preferably have a low coarse bulk silicon content as determined by TGA. Coarse bulk silicon is defined herein as silicon oxidized above 800° C. as determined by TGA, wherein TGA is performed in air at a heating rate of 10° C. / min. Therefore, the coarse bulk silicon content is determined according to the following formula:

[0330] Z=1.875×[(M f -M 800 ) / M f ]×100%

[0331] Where Z is the percentage of silicon that is not oxidized at 800°C, M 800 is the mass of the sample at 800 °C, and M f is the mass of ash at 1400°C when oxidation is complete. For the purposes of this analysis, it is assumed that any mass increase above 800°C corresponds to oxidation of silicon to SiO 2 , and the total mass when oxidation is complete is SiO 2 .

[0332] Silicon that oxidizes above 800° C. is less desirable. Preferably, no more than 10 wt%, or no more than 8 wt%, or no more than 6 wt%, or no more than 5 wt%, or no more than 4 wt%, or no more than 3 wt%, or no more than 2 wt%, or no more than 1.5 wt% of the silicon is macrophase silicon as determined by TGA.

[0333] Preferably, at least 20 wt% of the silicon is surface silicon and no more than 10 wt% of the silicon is rough phase silicon, both of which are determined by TGA. More preferably, at least 25 wt% of the silicon is surface silicon and no more than 10 wt% of the silicon is rough phase silicon, both of which are determined by TGA. More preferably, at least 30 wt% of the silicon is surface silicon and no more than 10 wt% of the silicon is rough phase silicon, both of which are determined by TGA. More preferably, at least 35 wt% of the silicon is surface silicon and no more than 8 wt% of the silicon is rough phase silicon, both of which are determined by TGA. More preferably, at least 40 wt% of the silicon is surface silicon and no more than 5 wt% of the silicon is rough phase silicon, both of which are determined by TGA. More preferably, at least 45 wt% of the silicon is surface silicon and no more than 2 wt% of the silicon is rough phase silicon, both of which are determined by TGA.

[0334] The BET surface area of ​​the composite particles obtained according to the process of the invention is preferably not more than 300 m 2 / g, or not more than 250m 2 / g, or not more than 200m 2 / g, or not more than 150m 2 / g. More preferably, no more than 100m 2 / g, or not more than 80m 2 / g, or not more than 60m 2 / g, or not more than 40m 2 / g, or not more than 30m 2 / g, or not more than 25m 2 / g, or not more than 20m 2 / g, or not more than 15m 2 / g, or not more than 10m 2 / g, or not more than 5m 2 / g. Generally, a low BET surface area is preferred to minimize the formation of a solid electrolyte interface (SEI) layer at the surface of the composite particles during the first charge-discharge cycle of the anode. However, too low a BET surface area leads to unacceptably low charge rates and capacities due to the inaccessibility of the silicon bulk to the metal ions in the surrounding electrolyte. The BET surface area is preferably at least 0.1 m 2 / g, or at least 1m 2 / g, or at least 2m 2 / g, or at least 5m 2 For example, the BET surface area of ​​the composite particles can be in the range of 0.1 to 100 m 2 / g, or 0.1 to 80m 2 / g, or 0.5 to 60m 2 / g, or 0.5 to 40m 2 / g, or 1 to 30m 2 / g, or 1 to 25m 2 / g, or 2 to 20m 2 / g range.

[0335] In a third aspect, the present invention provides a composite particle, which is obtainable by the method according to the first aspect of the present invention.

[0336] In a fourth aspect of the invention, a composition is provided, comprising the composite particles according to the third aspect of the invention and at least one other component. In particular, a composition is provided, comprising the composite particles according to the third aspect of the invention and at least one other component, the at least one other component being selected from: (i) a binder; (ii) a conductive additive; and (iii) an additional particulate electroactive material. The composition according to the fourth aspect of the invention can be used as an electrode composition and can therefore be used to form an active layer of an electrode.

[0337] In a fifth aspect, the invention provides an electrode comprising a composite particle according to the third aspect of the invention in electrical contact with a current collector. The particulate material used to prepare the electrode of the fifth aspect of the invention may be in the form of a composition according to the fourth aspect of the invention.

[0338] As used herein, the term current collector refers to any conductive substrate capable of carrying an electric current to the electroactive particles in the composition and carrying an electric current out of the electroactive particles in the composition. Examples of materials that can be used as current collectors include copper, aluminum, stainless steel, nickel, titanium and sintered carbon. Copper is a preferred material. The current collector is typically in the form of a foil or mesh having a thickness of 3 to 500 μm. The granular material of the present invention can be applied to one or both surfaces of the current collector to a thickness preferably in the range of 10 μm to 1 mm, for example 20 to 500 μm, or 50 to 200 μm.

[0339] The electrode of the fifth aspect of the invention can be used as an anode of a metal ion battery. Therefore, in a sixth aspect, the invention provides a rechargeable metal ion battery comprising: an anode comprising an electrode as described above; a cathode comprising a cathode active material capable of releasing and reabsorbing metal ions; and an electrolyte between the anode and the cathode.

[0340] The metal ion is preferably a lithium ion. More preferably, the rechargeable metal ion battery of the present invention is a lithium ion battery, and the cathode active material is capable of releasing and accepting lithium ions.

[0341] Example

[0342] Example 1

[0343] Silicon-carbon composite particles are prepared by placing porous carbon particles in a stainless steel autoclave with an agitator and gas inlet and outlet lines. The autoclave is purged with nitrogen and the furnace temperature is then set to 500°C. Before the temperature of the particle bed reaches 500°C, the gas supply is switched from nitrogen to pure monosilane. After one hour, the furnace is closed and the autoclave is slowly depressurized. The autoclave is then refilled with monosilane and heated again to 500°C and maintained for another hour. The furnace is closed, refilled, and heated, each repeated multiple times as needed for the target silicon content. After the feeding is complete, the autoclave is purged with nitrogen and exposed to increasing concentrations of oxygen to passivate the composite particles before cooling to room temperature.

[0344] Figure 1 Representative temperatures of the inner surface of the reaction zone and temperatures within a plurality of particles in this example are shown.

[0345] Figure 2 Representative temperatures of the interior surface of the reaction zone and temperatures within a plurality of particles during one silicon deposition cycle in this example are shown.

[0346] It was observed that during contact of the gas containing the silicon-containing precursor with the porous particles, the representative temperature of the inner surface of the reaction zone significantly exceeded the temperature within the plurality of particles most of the time. Under these conditions, significant contamination of the reaction zone occurred, and large flakes of silicon-rich composite material were formed. It is expected that the reaction zone will need to be shut down and cleaned after the process, rendering the process inoperable.

[0347] Example 2

[0348] Silicon-carbon composite particles are prepared by placing porous carbon particles in a stainless steel autoclave with an agitator and gas inlet and outlet lines. The autoclave is purged with nitrogen and the furnace temperature is then set to 430°C. Monosilane is added to the autoclave before the temperature of the particle bed reaches 370°C. After one hour, the furnace is closed and the autoclave is slowly depressurized. The autoclave is then refilled with monosilane and heated again to 430°C and maintained for another hour. The furnace closing, refilling and heating are each repeated multiple times as needed for the target silicon content. After the feeding is completed, the autoclave is purged with nitrogen and exposed to increasing concentrations of oxygen to passivate the composite particles before cooling to room temperature.

[0349] Figure 3 Representative temperatures of the inner surface of the reaction zone and temperatures within a plurality of particles in this example are shown.

[0350] Figure 4 Representative temperatures of the interior surface of the reaction zone and temperatures within a plurality of particles during one silicon deposition cycle in this example are shown.

[0351] It is observed that during contact of the gas containing the silicon-containing precursor with the porous particles, the representative temperature of the inner surface of the reaction zone exceeds the temperature within the plurality of particles at most times. Figure 1 The temperature difference between the inner surface of the reaction zone and the temperature within the plurality of particles at any given time was smaller than that of the deposition conditions shown in . Under these conditions, significant contamination of the reaction zone occurred, and large flakes of silicon-rich composite material were formed. It is expected that the reaction zone would need to be shut down and cleaned after the process, making the process inoperable.

[0352] Example 3

[0353] Silicon-carbon composite particles are prepared by placing porous carbon particles in a stainless steel autoclave with an agitator and gas inlet and outlet lines. The autoclave is purged with nitrogen and the furnace temperature is then set to 400°C. After the temperature of the particle bed reaches 350°C, monosilane is added to the autoclave. After one hour, the autoclave is slowly depressurized. The autoclave is then refilled with monosilane and kept for another hour. The decompression and refilling are each repeated multiple times as required for the target silicon content. After the feeding is completed, the autoclave is purged with nitrogen and exposed to increasing concentrations of oxygen to passivate the composite particles before cooling to room temperature.

[0354] Figure 5 Representative temperatures of the inner surface of the reaction zone and temperatures within a plurality of particles in this example are shown.

[0355] Figure 6 Representative temperatures of the interior surface of the reaction zone and temperatures within a plurality of particles during one silicon deposition cycle in this example are shown.

[0356] and Figure 1-4 Compared with the deposition conditions shown in Figure 5 and 6 When the temperature of the inner surface of the reaction zone exceeds the temperature within the plurality of particles, the difference between the temperature of the inner surface of the reaction zone and the temperature within the plurality of particles at any given time is smaller. Under these conditions, contamination of the reaction zone occurs; however, the flakes of the silicon-rich composite material are smaller than in Examples 1 and 2 and are within the tolerance range. It is expected that the process can be operated, but the reaction zone needs to be shut down and cleaned.

[0357] Example 4

[0358] Silicon-carbon composite particles are prepared by placing porous carbon particles in a stainless steel autoclave with an agitator and gas inlet and outlet lines. The autoclave is purged with nitrogen and the furnace temperature is then set to 350°C. After the temperature of the particle bed reaches 350°C, monosilane is added to the autoclave. After one hour, the autoclave is slowly depressurized. The autoclave is then refilled with monosilane and kept for another hour. The decompression and refilling are each repeated multiple times as required for the target silicon content. After the feeding is completed, the autoclave is purged with nitrogen and exposed to increasing concentrations of oxygen to passivate the composite particles before cooling to room temperature.

[0359] Figure 7 Representative temperatures of the inner surface of the reaction zone and temperatures within a plurality of particles in this example are shown.

[0360] Figure 8 Representative temperatures of the interior surface of the reaction zone and temperatures within a plurality of particles during one silicon deposition cycle in this example are shown.

[0361] It is observed that during the period when the gas containing the silicon-containing precursor is in contact with the porous particles, the temperature within the plurality of particles exceeds the temperature of the inner surface of the reaction zone at most times. Figure 1-6 Compared with the deposition conditions shown in Figure 7 and 8 When the temperature of the inner surface of the reaction zone exceeds the temperature within the plurality of particles, the difference between the temperature of the inner surface of the reaction zone and the temperature within the plurality of particles at any given time is much smaller. Under these conditions, the reaction zone is not fouled. Such a process may be able to extend the run time without requiring shutdown and cleaning of the reaction zone.

[0362] Example 5

[0363] Silicon-carbon composite particles are prepared by placing porous carbon particles in a stainless steel autoclave with an agitator and gas inlet and outlet lines. The autoclave is purged with nitrogen and the furnace temperature is then set to 350°C. After the temperature of the particle bed reaches 350°C, monosilane is added to the autoclave. After one hour, the autoclave is slowly decompressed. The autoclave is then refilled with monosilane and kept for another hour. The decompression and refilling are repeated. After 25 hours, the furnace is turned off and placed under an inert nitrogen atmosphere. After about 8 hours, the furnace temperature is set to 350°C. After the temperature of the particle bed reaches 350°C, monosilane is added to the autoclave, and the steps of pressurization and refilling are each repeated as many times as needed for the target silicon content. After the feeding is completed, the autoclave is purged with nitrogen and exposed to increasing concentrations of oxygen to passivate the composite particles before cooling to room temperature.

[0364] Fig. 9 Representative temperatures of the inner surface of the reaction zone and temperatures within a plurality of particles in this example are shown.

[0365] Fig.10 Representative temperatures of the heat source of the reaction zone and the temperatures within a plurality of particles during one silicon deposition cycle in this example are shown.

[0366] It is observed that during the period when the gas containing the silicon-containing precursor is in contact with the porous particles, the temperature within the plurality of particles exceeds the temperature of the inner surface of the reaction zone at most times. Figure 1-6 Compared with the deposition conditions shown in Fig. 9 and 10 When the temperature of the inner surface of the reaction zone exceeds the temperature within the plurality of particles, the difference between the temperature of the inner surface of the reaction zone and the temperature within the plurality of particles at any given time is much smaller. Under these conditions, the reaction zone is not fouled. This process may be able to extend the run time without requiring shutdown and cleaning of the reaction zone.

[0367] Example 6

[0368] Silicon-carbon composite particles were prepared by placing porous carbon particles in a stainless steel autoclave with an agitator and gas inlet and outlet lines. The autoclave was purged with nitrogen and the furnace temperature was then set to 395°C. After the temperature of the particle bed reached 395°C, monosilane was continuously added to the autoclave. After the feeds were complete, the autoclave was purged with nitrogen and exposed to increasing concentrations of oxygen to passivate the composite particles before cooling to room temperature.

[0369] Fig.11 Shown are representative temperatures of the inner surface of the reaction zone and the temperatures within the plurality of particles during the period in which monosilane was continuously added to the autoclave in this example.

[0370] It was observed that during contact of the gas containing the silicon-containing precursor with the porous particles, the temperature within the plurality of particles exceeded the temperature of the inner surface of the reaction zone. Under these conditions, the reaction zone was not contaminated. This process may be able to extend the run time without requiring shutdown and cleaning of the reaction zone.

[0371] The following table summarizes the maximum values ​​(the maximum temperature of the inner surface of the reaction zone at a given time minus the minimum temperature within the particles at the same time) for each of the above examples throughout the reaction. The table also indicates the extent to which the reactor was contaminated.

[0372] Example Maximum ΔT Is the reactor contaminated? Example 1 +154.27 Yes, out of tolerance Example 2 +100.98 Yes, out of tolerance Example 3 +79.59 Yes, but within tolerance Example 4 +5.019 no Example 5 +4.758 no Example 6 -17 no

Claims

1. A method for preparing composite particles, the method comprising the following steps: (a) providing a plurality of porous particles in a reaction zone, the reaction zone having an inner surface; as well as (b) contacting the plurality of particles in the reaction zone with a gas comprising at least 25% by volume of a silicon-containing precursor at a temperature effective to cause deposition of silicon in the pores of the porous particles; During step (b), ΔT≤+90°C is maintained, wherein ΔT represents the temperature difference between the maximum temperature of the inner surface of the reaction zone and the minimum temperature within the multiple porous particles during the same period, and a positive value of ΔT indicates that the maximum temperature of the inner surface of the reaction zone is higher than the minimum temperature within the multiple particles.

2. The method according to claim 1, wherein during step (b) ΔT≤+85°C, or ΔT≤+80°C, or ΔT≤+75°C, or ΔT≤+70°C, or ΔT≤+65°C, or ΔT≤+60°C, or ΔT≤+55°C, or ΔT≤+50°C, or ΔT≤+45°C, or ΔT≤+40°C, or ΔT≤+35°C, or ΔT≤+30°C, or ΔT≤+25°C, or ΔT≤+20°C, or ΔT≤+15°C, or ΔT≤+10°C, or ΔT≤+5°C, or ΔT≤0°C, or ΔT≤-5°C, or ΔT≤-10°C is maintained.

3. The method according to claim 1 or 2, wherein the ΔT maintained during step (b) is between +90°C and -110°C, or +85°C and -110°C, or +80°C and -110°C, or +75°C and -110°C, or +70°C and -110°C, or +65°C and -110°C, or +60°C and -110°C, or +55°C and -110°C, or +50°C and -110°C, or +45°C and -110°C, or +40°C and -110°C, or +35°C and -110°C, or +30°C and -110°C, or +25°C and -110°C, or +20°C and -110°C, or +15°C and -110°C, or +10°C and -110°C, or in the range of +5°C to -110°C, or 0°C to -110°C, or -5°C to -110°C, or -5°C to -105°C, or -5°C to -100°C, or -5°C to -95°C, or -5°C to -90°C, or -5°C to -85°C, or -5°C to -80°C, or -5°C to -75°C, or -5°C to -70°C, or -5°C to -65°C, or -5°C to -60°C, or -5°C to -55°C, or -5°C to -50°C, or -5°C to -45°C, or -5°C to -40°C, or -5°C to -35°C, or -5°C to -30°C, or -5°C to -25°C, or -5°C to -20°C, or -5°C to -15°C, or -5°C to -10°C.

4. The method of any one of the preceding claims, wherein during the contacting, the minimum temperature within the plurality of porous particles is between 340 and 400°C, or 340 and 395°C, or 340 and 390°C, or 345 and 400°C, or 345 and 395°C, or 345 and 390°C, or 350 and 400°C, or 350 and 395°C, or 350 and 390°C, or 350 and 385°C, or 350 and 380°C, or 355 and 400°C, or 355 and 395°C, or 355 and 390°C. or 370 to 400°C, or 370 to 395°C, or 370 to 390°C, or 370 to 385°C, or 370 to 380°C, or 370 to 385°C, or 370 to 380°C.

5. A method according to any one of the preceding claims, wherein step (a) comprises: The plurality of porous particles are preheated prior to providing the plurality of porous particles in the reaction zone.

6. The method of claim 5, wherein the plurality of porous particles are preheated to a temperature of 300 to 480°C, or 320 to 450°C, or 330 to 400°C, or 340 to 390°C, or 345 to 390°C, or 350 to 400°C, or 350 to 390°C, or 350 to 385°C, or 350 to 380°C, or 355 to 390°C, or 355 to 385°C, or 355 to 380°C, or 360 to 390°C, or 360 to 385°C, or 360 to 380°C.

7. The method of any one of the preceding claims, wherein the reaction zone comprises a heat source, and step (a) comprises operating the heat source to heat the plurality of porous particles to 340 to 400°C, or 340 to 395°C, or 340 to 390°C, or 345 to 400°C, or 345 to 395°C, or 345 to 390°C, or 350 to 400°C, or 350 to 395°C, or 350 to 390°C, or 350 to 385°C, or 350 to 380°C, or 355 to 400°C, or 355 to 39 5°C, or 355 to 390°C, or 355 to 385°C, or 355 to 380°C, or 360 to 400°C, or 360 to 395°C, or 360 to 390°C, or 360 to 385°C, or 360 to 380°C, or 365 to 400°C, or 365 to 395°C, or 365 to 390°C, or 365 to 385°C, or 365 to 380°C, or 370 to 400°C, or 370 to 395°C, or 370 to 390°C, or 370 to 385°C, or 370 to 380°C.

8. The method of claim 7, wherein the heat source is a convective or conductive heat source.

9. The method according to any one of the preceding claims, wherein step (b) comprises preheating the gas to a temperature of 100 to 350°C, or 110 to 340°C, or 120 to 330°C, or 130 to 320°C, or 140 to 310°C, or 150 to 300°C prior to the contacting.

10. The process of any one of the preceding claims, wherein during the contacting, the maximum temperature of the inner surface of the reaction zone is from 150 to 480°C, or from 150 to 460°C, or from 150 to 440°C, or from 150 to 420°C, or from 150 to 400°C, or from 150 to 390°C, or from 200 to 390°C, or from 250 to 390°C, or from 300 to 390°C, or from 340 to 375°C, or from 340 to 370°C, or from 345 to 370°C, or from 345 to 365°C, or from 350 to 400°C, or from 350 to 390°C, or from 350 to 380°C, or from 350 to 370°C, or from 350 to 365°C.

11. A method according to any one of the preceding claims, wherein step (a) comprises providing a batch of the plurality of porous particles in the reaction zone.

12. The method according to any one of the preceding claims, further comprising: (c) interrupting the deposition of silicon to form intermediate particles, and optionally separating by-products from the intermediate particles; as well as (d) contacting the intermediate particles from step (c) with a gas comprising a silicon-containing precursor in a reaction zone at a temperature effective to cause further deposition of the silicon in the pores of the intermediate particles; wherein during step (d) ΔT≤+90°C, or ΔT≤+85°C, or ΔT≤+80°C, or ΔT≤+75°C, or ΔT≤+70°C, or ΔT≤+65°C, or ΔT≤+60°C, or ΔT≤+55°C, or ΔT≤+50°C, or ΔT≤+45°C, or ΔT≤+40°C, or ΔT≤+35°C, or ΔT≤+30°C, or ΔT≤+25°C, or ΔT≤+20°C, or ΔT≤+15°C, or ΔT≤+10°C, or ΔT≤+5°C, or ΔT≤0°C, or ΔT≤-5°C, or ΔT≤-10°C is maintained, wherein ΔT represents the temperature difference between the highest temperature of the inner surface of the reaction zone and the lowest temperature within the plurality of porous particles, wherein a positive value of ΔT indicates that the highest temperature of the inner surface of the reaction zone is higher than the lowest temperature within the plurality of particles.

13. The process of claim 12, wherein during the contacting in steps (b) and / or (d), the maximum temperature of the inner surface of the reaction zone is from 150 to 480°C, or from 150 to 460°C, or from 150 to 440°C, or from 150 to 420°C, or from 150 to 400°C, or from 150 to 390°C, or from 200 to 390°C, or from 250 to 390°C, or from 300 to 390°C, or from 340 to 375°C, or from 340 to 370°C, or from 345 to 370°C, or from 345 to 365°C, or from 350 to 400°C, or from 350 to 390°C, or from 350 to 380°C, or from 350 to 370°C, or from 350 to 365°C.

14. The method of claim 12 or 13, wherein during steps (b), (c) and (d), the minimum temperature within the plurality of porous particles is maintained at 340 to 400°C, or 340 to 395°C, or 340 to 390°C, or 345 to 400°C, or 345 to 395°C, or 345 to 390°C, or 350 to 400°C, or 350 to 395°C, or 350 to 390°C, or 350 to 385°C, or 350 to 380°C, or 355 to 400°C, or 355 to 395°C, or 355 to 390°C. or a temperature in the range of 355 to 390°C, or 355 to 385°C, or 355 to 380°C, or 360 to 400°C, or 360 to 395°C, or 360 to 390°C, or 360 to 385°C, or 360 to 380°C, or 365 to 400°C, or 365 to 395°C, or 365 to 390°C, or 365 to 385°C, or 365 to 380°C, or 370 to 400°C, or 370 to 395°C, or 370 to 390°C, or 370 to 385°C, or 370 to 380°C.

15. The method according to any one of claims 12 to 14, wherein step (d) comprises preheating the gas to a temperature of 100 to 350°C, or 110 to 340°C, or 120 to 330°C, or 130 to 320°C, or 140 to 310°C, or 150 to 300°C prior to the contacting.

16. The method of any one of claims 1 to 11, wherein step (b) comprises continuously introducing the gas comprising the silicon-containing precursor into the reaction zone.

17. A method according to any one of the preceding claims, wherein step (b) or step (d) comprises interrupting the deposition of the silicon to form the composite particles and removing the composite particles from the reaction zone.

18. The method according to any one of claims 1 to 10, wherein step (a) comprises: providing a chemical vapor permeation unit including the reaction zone; providing a raw material comprising the porous particles; and continuously introducing the porous particles into the reaction zone; And step (b) comprises: continuously introducing the gas comprising the silicon-containing precursor into the reaction zone; providing conditions in the reaction zone effective to cause deposition of silicon in the pores of the porous particles; continuously removing composite particles from the reaction zone, the composite particles comprising a porous particle skeleton and elemental silicon within pores of the porous particle skeleton; and Exhaust gas is continuously withdrawn from the reaction zone.

19. A process according to any one of the preceding claims, wherein during the contacting in steps (b) and / or (d), the maximum temperature of the inner surface of the reaction zone does not exceed 480°C, or does not exceed 460°C, or does not exceed 440°C, or does not exceed 420°C, or does not exceed 400°C, or does not exceed 395°C, or does not exceed 390°C, or does not exceed 385°C, or does not exceed 380°C.

20. A method according to any one of the preceding claims, wherein step (b) and / or step (d) comprises continuously stirring the porous particles during the contacting, preferably continuously stirring the porous particles mechanically during the contacting, preferably wherein the reaction zone comprises an agitator for continuously stirring the porous particles during the contacting, preferably wherein the agitation is performed by a high shear mixer.

21. The method of any one of the preceding claims, wherein in step (a) the volume of the plurality of porous particles in the reaction zone is at least 100 cm 3 Reaction area per liter (cm 3 / L RV ), or at least 150cm 3 / L RV , or at least 200cm 3 / L RV , or at least 250cm 3 / L RV , or at least 300cm 3 / L RV , or at least 400cm 3 / L RV , or at least 500cm 3 / L RV , or at least 600cm 3 / L RV , or at least 700cm 3 / L RV , or at least 800cm 3 / L RV , or at least 900cm 3 / L RV .

22. A method according to any one of the preceding claims, wherein in step (a) the ratio of the internal surface area of ​​the reaction zone to the mass of the porous particles in the reaction zone is no more than 1 m 2 / kg, or not more than 0.9m 2 / kg, or not more than 0.8m 2 / kg, or not more than 0.7m 2 / kg, or not more than 0.6m 2 / kg, or not more than 0.5m 2 / kg, or not more than 0.4m 2 / kg, or not more than 0.3m 2 / kg, or not more than 0.2m 2 / kg, or not more than 0.1m 2 / kg.

23. A method according to any one of the preceding claims, wherein the ratio of the internal surface area of ​​the reaction zone to the mass of porous particles in the reaction zone is at least 0.001 m 2 / kg, or at least 0.002m 2 / kg, or at least 0.003m 2 / kg, or at least 0.004m 2 / kg, or at least 0.006m 2 / kg, or at least 0.008m 2 / kg, or at least 0.01m 2 / kg.

24. The process of any one of the preceding claims, wherein the bed depth of the porous particles in the reaction zone is at least 11 cm, or at least 15 cm, or at least 20 cm, or at least 25 cm, or at least 30 cm.

25. The method according to any one of the preceding claims, wherein the silicon-containing precursor is selected from the group consisting of monosilane (SiH4), disilane (Si2H6), trisilane (Si3H8), tetrasilane (Si4H 10 ), methylsilane, dimethylsilane and chlorosilane, and various mixtures thereof.

26. The process according to any one of the preceding claims, wherein the pressure in steps (b) and / or (d) is from 10 to 10000 kPa, or from 100 to 5000 kPa, or from 100 to 4000 kPa, or from 100 to 3000 kPa, or from 100 to 2000 kPa, or from 100 to 1000 kPa, or from 100 to 500 kPa.

27. The process according to any one of the preceding claims, wherein the pressure of steps (b) and / or (d) is from 10 to 15000 kPa, or from 50 to 10000 kPa, or from 120 to 5000 kPa, or from 150 to 2000 kPa, or from 200 to 1800 kPa, or from 200 to 1600 kPa, or from 250 to 1500 kPa, or from 300 to 1200 kPa, or from 400 to 1000 kPa, or from 500 to 900 kPa, or from 600 to 800 kPa.

28. A method according to any of the preceding claims, wherein the gas containing a silicon-containing precursor contains at least 30 volume % of a silicon-containing precursor based on the total volume of the gas, or at least 40 volume %, or at least 50 volume %, or at least 60 volume %, or at least 70 volume %, or at least 80 volume %, or at least 90 volume %, or at least 95 volume %, or at least 97 volume %, or at least 99 volume % of a silicon-containing precursor based on the total volume of the gas.

29. A method according to any one of the preceding claims, wherein the porous particles have a BET surface area of ​​100 m 2 / g to 4,000m 2 / g, or 500m 2 / g to 4,000m 2 / g, or 750m 2 / g to 3,500m 2 / g, or 1,000m 2 / g to 3,250m 2 / g, or 1,000m 2 / g to 3,000m 2 / g, or 1,000m 2 / g to 2,500m 2 / g, or 1,000m 2 / g to 2,000m 2 / g range.

30. The method of any preceding claim, wherein the porous particles comprise micropores and / or mesopores.

31. The method according to any one of the preceding claims, wherein the porous particles comprise micropores and / or mesopores and the total pore volume of the micropores and mesopores measured by nitrogen adsorption is between 0.4 and 2.2 cm 3 / g, or 0.45 to 2.2 cm 3 / g, or 0.5 to 2cm 3 / g, or 0.55 to 2cm 3 / g, or 0.6 to 1.8 cm 3 / g, or 0.65 to 1.8 cm 3 / g, or 0.7 to 1.6 cm 3 / g, or 0.7 to 1.5 cm 3 / g, or 0.7 to 1.4 cm 3 / g range.

32. A method according to any one of the preceding claims, wherein the PD of the porous particles 50The pore diameter is no more than 30nm, or no more than 25nm, or no more than 20nm, or no more than 15nm, or no more than 12nm, or no more than 10nm, or no more than 8nm, or no more than 6nm, or no more than 5nm, or no more than 4nm, or no more than 3nm, or no more than 2.5nm, or no more than 2nm, or no more than 1.5nm.

33. A method according to any one of the preceding claims, wherein the PD of the porous particles 30 The pore diameter is no more than 25nm, or no more than 20nm, or no more than 15nm, or no more than 12nm, or no more than 10nm, or no more than 8nm, or no more than 6nm, or no more than 5nm, or no more than 4nm, or no more than 3nm, or no more than 2.5nm, or no more than 2nm, or no more than 1nm.

34. The method according to any one of the preceding claims, wherein the porous particles have a D 50 The particle size ranges from 0.5 to 30 μm, or 1 to 25 μm, or 1 to 20 μm, or 2 to 25 μm, or 2 to 20 μm, or 2 to 18 μm, or 2 to 15 μm, or 2 to 12 μm, or 2.5 to 15 μm, or 2.5 to 12 μm, or 2 to 10 μm.

35. A method according to any one of the preceding claims, wherein at least 20 wt. % of the silicon in the composite particles is surface silicon (Y) and no more than 10 wt. % of the silicon is macrophase silicon (Z), wherein the content of surface silicon and macrophase silicon is determined by TGA according to the method described in the specification.

36. A system for preparing composite particles, the system comprising: (a) a reaction zone, the reaction zone being configured to accommodate a plurality of porous particles, the reaction zone having: (i) at least one heat source configured to heat the plurality of porous particles; (ii) at least one gas inlet for receiving a gas comprising at least 25% by volume of a silicon-containing precursor; (iii) at least one gas outlet for removing exhaust gas from said reaction zone; (b) at least one sensor configured to acquire temperature data within the plurality of porous particles; (c) at least one sensor configured to acquire temperature data of an inner surface of the reaction zone; as well as (d) processor; Wherein, at least one sensor configured to obtain temperature data within the multiple porous particles and at least one sensor configured to obtain temperature data of the inner surface of the reaction zone are configured to send corresponding temperature data to the processor, and the processor is configured to control the heat source so as to maintain ΔT≤+90°C, wherein ΔT represents the temperature difference between the highest temperature of the inner surface of the reaction zone and the lowest temperature within the multiple porous particles during the same period, wherein a positive value of ΔT indicates that the highest temperature of the inner surface of the reaction zone is higher than the lowest temperature within the multiple particles.

37. The system of claim 36, wherein the reaction zone comprises a high shear mixer for continuously agitating the plurality of porous particles.