Method for producing doped cathode active material

By preparing fluoride-doped cathode active material with olivine crystal structure, the problem of insufficient stability and cycle stability of cathode materials for lithium-ion batteries is solved, lower capacity attenuation and higher cycle stability are achieved, and the Overall performance of electrochemical cells.

CN118946529APending Publication Date: 2024-11-12BASF SE
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380029795.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-25
Filing Date
2023-03-20
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The existing lithium-ion battery cathode materials have instability in charging and discharging behavior, resulting in insufficient capacity attenuation and cycle stability. Especially the low conductivity of lithium iron phosphate materials, requiring a large amount of conductive carbon to improve performance, but conductive carbon is No significant contribution to energy density and efficiency.

Method used

A method is used to prepare fluoride doped cathode active materials with olivine crystal structure, combining lithium sources and carbon by combining specific phosphate and transition metal sources, including iron and other metals such as vanadium, titanium, nickel, cobalt, etc. The LiFe(1-x)M1x(PO4)1-yF3y structure is formed by high temperature treatment to ensure uniform distribution of fluoride and a carbon layer is coated on the surface of the particles.

Benefits of technology

It significantly improves the stability and cycle stability of the cathode material, reduces capacity attenuation, and improves the performance of electrochemical cells under constant product quality, especially in high temperature conditions, showing good low-temperature performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005056385790000161
    Figure BDA0005056385790000161
  • Figure BDA0005056385790000171
    Figure BDA0005056385790000171
  • Figure BDA0005056385790000201
    Figure BDA0005056385790000201
Patent Text Reader

Abstract

A process for manufacturing a fluoride-doped cathode active material having an olivine crystal structure wherein the process comprises the steps of: (a) providing a source of phosphate, a source of a metal selected from iron other than lithium, and optionally a source of at least one further element M1 selected from titanium, vanadium, nickel, yttrium, copper, magnesium, zinc, aluminum, cobalt and manganese, wherein at least 55 mol-% of the metal other than lithium is iron, and wherein the source may be formed from one or more compounds, (b) providing a lithium source containing 0.01% to 2.5% by weight of fluoride homogeneously dispersed in the lithium source wherein the lithium source is selected from the group consisting of lithium hydroxide and lithium carbonate, (c) mixing the phosphate source, a transition metal source with the fluoride-containing lithium source, and with an additional lithium source containing less fluoride, and optionally with a hydrocarbon, (d) optionally reacting between at least two components in the mixture from step (c), thereby obtaining an adduct, (e) treating the mixture obtained from step (c) or the adduct from step (d) at a temperature in the range of 400 DEG C to 1000 DEG C under a reducing or inert atmosphere.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] The present invention relates to a method for producing a fluoride-doped cathode active material having an olivine crystal structure, wherein the method comprises the following steps:

[0002] (a) providing a phosphate source, a source of a metal other than lithium and selected from iron, and optionally at least one further element M 1 a source of an element selected from vanadium, titanium, nickel, cobalt, copper, zinc, magnesium, aluminium, yttrium and manganese, wherein at least 55 mol-% of the metal other than lithium is iron, and wherein the source can be formed from one or more compounds,

[0003] (b) providing a lithium source, the lithium source containing 0.01% to 2.5% by weight of fluoride uniformly dispersed in the lithium source, wherein the lithium source is selected from lithium hydroxide and lithium carbonate,

[0004] (c) mixing the phosphate source, the transition metal source with the fluoride-containing lithium source, and with an additional lithium source containing less fluoride, and optionally with a hydrocarbon,

[0005] (d) optionally, reacting at least two components of the mixture from step (c) to obtain an adduct,

[0006] (e) treating the mixture obtained from step (c) or the adduct from step (d) at a temperature ranging from 400°C to 1000°C under a reducing or inert atmosphere.

[0007] Lithium-ion secondary batteries are modern devices for storing energy. Many applications have been and are being considered, from small devices such as mobile phones and laptops to automotive batteries and other electric vehicle batteries. The various components of the battery, such as electrolytes, electrode materials, and separators, play a decisive role in the performance of the battery. Special attention has been paid to cathode materials. Several materials have been proposed, such as lithium iron phosphate ("LFP"), lithium cobalt oxide ("LCO"), and lithium nickel cobalt manganese oxide ("NCM"). Despite extensive research, the solutions found so far still leave room for improvement.

[0008] In particular, in many cases, the charging and discharging behavior is not good enough. Although lithium iron phosphate does not contain environmentally harmful transition metals, it still has disadvantages such as low electrical conductivity. For high-performance electrochemical cells, relatively large amounts of conductive carbon need to be added. However, conductive carbon does not make a positive contribution to volumetric energy density or higher energy transport efficiency. In particular, conductive carbon does not contribute to the properties of electrochemical cells (such as capacity, cycle stability, energy, etc.).

[0009] Various publications indicate that doping LFP with fluoride may help low temperature performance, B. Wu et al., J. New Mat. Electrochem. Synth. 2011, 14, 147, produced by reacting iron (+II) oxalate with lithium hydroxide, lithium fluoride and NH4H2PO4. M. Pan et al., J. Solid State Electrochem. 2012, 16, 1615 disclosed a method of making doped LFP using NH4F as a fluoride source. The authors associated the signals in the X-ray diffraction spectrum with phases such as Li3FeF6.

[0010] However, it has been found that the above materials vary greatly between different samples.

[0011] Therefore, the object of the present invention is to provide a cathode active material having improved stability such as lower capacity fade and improved cycle stability at a constant product quality. Another object is to provide a method for making a cathode active material having improved stability such as lower capacity fade and improved cycle stability at a constant product quality.

[0012] Accordingly, the method defined at the outset has been found, hereinafter also referred to as "the method of the invention" or as "the method according to the (present) invention". The method of the invention comprises a series of steps as defined at the outset, hereinafter also referred to as step (a), step (b), step (c), etc. The method of the invention will be described in more detail below.

[0013] The method of the present invention is a method for making a fluoride-doped cathode active material having an olivine crystal structure. The olivine crystal structure is found in materials such as LFP, LiFePO4. In the olivine crystal structure, the iron can be selected from vanadium, titanium, nickel, cobalt, copper, zinc, magnesium, aluminum, yttrium and manganese, and a metal M selected from a combination of at least two of the above-mentioned 1 Partial replacement.

[0014] In one embodiment of the present invention, the cathode active material prepared according to the method of the present invention is characterized by the general formula:

[0015] LiFe (1-x) M 1 x (PO4) 1-y F 3y

[0016] x is in the range of 0 to 0.45, and wherein y is in the range of 0.0002 to 0.03,

[0017] M 1 Selected from Y, Cu, Zn, Mg, Al, Ni, Ti, V, Co and Mn, and selected from a combination of at least two of the above mentioned, preferably selected from Ni, Co, Mn and V.

[0018] In one embodiment of the present invention, the above general formula refers to the electrically neutral state of the cathode active material prepared according to the method of the present invention.

[0019] This cathode active material is in the form of primary particle agglomerates, the average diameter (d50) of such agglomerates is in the range of 1 μm to 16 μm, preferably 2 to 10 μm, more preferably 2 to 5 μm, even more preferably 4 to 5 μm. Although strictly speaking the D50 value is a median value, it is often also referred to as the average particle size (D50).

[0020] In one embodiment of the present invention, the cathode active material prepared according to the method of the present invention is coated with a carbon layer between primary crystallites (primary particles) and on the surface of secondary particles. In the context of the present invention, the average particle size (D50) refers to the median of the volume-based particle size as can be determined, for example, by light scattering, especially by laser (LASER) scattering technology, for example at a pressure in the range of 0.5 to 3 bar.

[0021] In one embodiment of the present invention, the average diameter of the primary particles of the cathode active material prepared according to the method of the present invention is in the range of 1 to 2000 nm, preferably 10 to 1000 nm, particularly preferably 50 to 500 nm, and even more preferably 80 to 270 nm. The average primary particle size can be determined, for example, by SEM or TEM, or by an XRD method. This XRD method preferably uses the Scherrer Equation, in which the peak width is inversely proportional to the crystallite size.

[0022] Many elements are ubiquitous. For example, sodium, copper and chloride can be detected in very small proportions in almost all inorganic materials. In the context of the present invention, cations or anions with a proportion of less than 0.01% by weight are ignored. Therefore, in the context of the present invention, a doped cathode active material having an olivine crystal structure containing less than 0.01% by weight of sodium is considered to be sodium-free.

[0023] Step (a) comprises a phosphate source, a source of a metal other than lithium and selected from iron, and optionally at least one further element M as defined above. 1 A source of, wherein at least 55 mol-% of the metal other than lithium is iron, the percentage being relative to the transition metal content, and wherein the source may be formed from one or more compounds. Preferably, 70 to 99 mol-% or 100 mol-% of the transition metal is iron.

[0024] The source of transition metals may contain transition metals in the "correct" oxidation state. In other embodiments, at least one of the transition metals is in too high an oxidation state, for example, iron may be in a +III oxidation state. In such embodiments, a reducing agent may need to be applied, for example in step (e) or in step (d), or at least one of the other components selected from the phosphate source is a reducing agent.

[0025] Suitable phosphate sources are phosphoric acid H3PO4, phosphorous acid H3PO3 / P(OH)3, either as free acid or partially neutralized with ammonia, ammonium hydrogen phosphate NH4H2PO4, (NH4)2HPO4, and phosphates. Phosphorous acid can be used as a reducing agent and then react to form phosphates.

[0026] In one embodiment of the invention, a reducing agent of a non-phosphate source is also provided in step (a), such as ascorbic acid or lactic acid or hydrazine or a sugar compound such as glucose. Some polymers, such as polypropylene, may also be used as reducing agents. Ascorbic acid or lactic acid or polymers may then be at least partially converted into carbon and deposited as a coating of the cathode active material.

[0027] The cathode active material having an olivine crystal structure can be produced according to various methods, for example by a solid-state method or by a precipitation method, and the sources of transition metal and phosphorus are then selected accordingly.

[0028] For example, step (a) may be performed as follows

[0029] (a1) combining an aqueous solution of an iron (+III) salt, ammonium (hydrogen) phosphate and a reducing agent, or

[0030] (a2) combining an aqueous slurry of an iron compound selected from Fe2O3, Fe3O4, FeOOH and Fe(OH)3 with a reducing agent and a phosphate source, or

[0031] (a3) combining an aqueous solution of an iron (+III) salt, a phosphate source, and optionally at least one reducing agent and polyethylene glycol, or

[0032] (a4) providing a solution of a Fe(+II) compound in an organic solvent and a solution of H3PO4 in a water-miscible solvent such as NMP (N-methylpyrrolidone), or

[0033] (a5) mixing Fe(+II) oxalate and ammonium dihydrogen phosphate in the presence of a C1-C6-alkanol or polyethylene glycol,

[0034] (a6) Synthesize FePO4 with an average particle size ranging from 1 to 16 μm.

[0035] The embodiments will be described in more detail herein.

[0036] In one embodiment, a cathode active material having an olivine crystal structure can be prepared by a gelation method. The gelation method can control the material structure at the nanoscale from the initial stage of synthesis. In such an embodiment, the aqueous solution containing a water-soluble iron (III) salt (such as Fe(NO3)3 or Fe2(SO4)3), a phosphate source (such as NH4H2PO4) and a reducing agent (such as ascorbic acid) in step (a1), and optionally at least one M 1 A water-soluble compound (such as Co(NO3)2, Mn(NO3)2, Ni(NO3)2, VO(NO3)2, VOCl2, VOCl3, ZnCl2, Zn(NO3)2, Mg(NO3)2, Cu(NO3)2, etc.) is combined with a lithium source according to step (c) (see above) and then gelled by evaporating water. A dry gel is obtained, which is then dried at a temperature of 300°C to 400°C, then mechanically treated, such as grinding, and dried again at 450°C to 550°C, followed by calcination at 700°C to 825°C, preferably under a hydrogen atmosphere. The reducing agent is preferably ascorbic acid, which can also be used as a carbon source.

[0037] In the context of the present invention, the term "water-soluble" refers to compounds whose solubility in water at 20° C. is at least 50 g / l. The term "water-insoluble" refers to compounds whose solubility in water at 20° C. is less than 0.1 g / l. Compounds with solubility between the two are called "partially water-soluble" or "moderately water-soluble".

[0038] In another embodiment, the cathode active material having an olivine crystal structure can be synthesized from a water-insoluble iron compound (as an iron source) under hydrothermal conditions. In this embodiment, an aqueous slurry of a water-insoluble iron (III) compound (such as Fe2O3, Fe3O4, FeOOH or Fe(OH)3) is mixed with at least one reducing agent (such as hydrazine, hydrazine hydrate, hydrazine sulfate, hydroxylamine, a carbon-based reducing agent (primary or secondary alcohol), a reducing sugar, or ascorbic acid, or a reducing phosphorus compound (such as H3PO3 or its ammonium salt)) in step (a2) for preparation. A carbon source such as graphite, soot or activated carbon can be added. In the case where the reducing agent does not carry any phosphorus atoms, a phosphate source such as phosphoric acid, ammonium phosphate or (di) ammonium hydrogen phosphate is added, especially (NH4)2HPO4 or NH4H2PO4. A combination of H3PO3 or its ammonium salt and a phosphate source is also feasible. The slurry thus obtained is mixed with a lithium source (step (c)) and then reacted at a temperature ranging from 100° C. to 350° C., preferably for a period ranging from 1 to 24 hours. The reaction can be carried out at a pressure ranging from 1 to 100 bar. The water is then removed, followed by calcination, for example at 700° C. to 900° C., preferably under a hydrogen atmosphere.

[0039] In another embodiment, the cathode active material having an olivine crystal structure can be synthesized starting from a water-soluble iron compound (as an iron source) under hydrothermal conditions as in step (a3). In this embodiment, in step (a3), an aqueous solution of a water-soluble iron (II) compound (such as FeSO4.7H2O) or an aqueous solution of a water-soluble iron (III) compound (such as Fe2(SO4)3.7H2O) is mixed with the lithium source obtained from step (c) and with a phosphorus compound (such as H3PO4, (NH4)3PO4.3H2O, NH4H2PO4 or (NH4)2HPO4), with or without the addition of a reducing agent (such as ascorbic acid), and / or with or without the addition of polyethylene glycol (PEG). The solution thus obtained is then subjected to a hydrothermal treatment at 120°C to 190°C, preferably above 175°C, thereby producing the adduct. After the hydrothermal treatment, in most cases, the powder thus obtained will be treated at a higher temperature (for example in the range of 600°C to 800°C).

[0040] In another embodiment, a cathode active material having an olivine crystal structure can be synthesized by a sol-gel method. In such an embodiment, a solution of a water-soluble iron (II) compound such as ferrous acetate (Fe(acetate)2) and H3PO4 in at least one organic solvent such as DMF (N,N-dimethylformamide) is prepared in step (a4) and combined with a lithium source (step (c)). The one or more organic solvents are then removed, preferably by evaporation. The residue is then gradually heated to 700°C and then calcined at a temperature in the range of 750°C to 850°C under a reducing atmosphere (e.g., under hydrogen).

[0041] In another embodiment, the cathode active material having an olivine crystal structure can be synthesized from an oxalate such as ferric oxalate. Ferric oxalate can be provided by a solid state method in step (a5), by preparing a stoichiometric mixture of FeC2O4·2H2O and NH4H2PO4, and a lithium source (step (c)) in the presence of an alcohol, by ball milling or by using a high shear mixer. A carbon source such as polyvinyl alcohol (PVA) or glucose is added, and the resulting material is sintered, for example, at 600° C. to 800° C. in a reducing atmosphere.

[0042] In another embodiment, ferric oxalate can be used in a soft chemical-rheological phase reaction method, wherein in step (a5), FeC2O4·2H2O is combined with a phosphorus compound (such as NH4H2PO4) and a lithium source (step (c)) by sufficient grinding, with the addition of a polymer (such as polyethylene glycol) as a carbon source. The precursor thus obtained is then heated to 400°C to 800°C under an inert atmosphere.

[0043] In another embodiment, the cathode active material having an olivine crystal structure can be synthesized by a solid-state reaction in the range of 650° C. to 800° C. from the iron phosphate blend provided in (a6) without or preferably with crystal water, mixed according to step (c). The heat treatment is carried out under carbothermal conditions, for example using sugar as a reducing agent, and under a reducing or inert atmosphere.

[0044] In each of the above embodiments, in step (c), a relative amount of iron or iron and M may be applied. 1 The total molar excess of the lithium source.

[0045] In the formulas of the above compounds, water of crystallization may be omitted.

[0046] In step (b) a lithium source is provided, wherein the source contains 0.01% to 2.5% by weight of fluoride, uniformly dispersed in the lithium source. Preferably 0.05% to 0.5% by weight. The percentages are relative to the corresponding lithium source. The fluoride is preferably lithium fluoride, but may have counterions other than lithium and derived from impurities. Preferably, the majority of the fluoride is lithium fluoride. Even more preferably, the fluoride is lithium fluoride.

[0047] The lithium source is selected from lithium carbonate, lithium oxide (Li2O) and lithium hydroxide (LiOH), and includes lithium hydroxide hydrates such as but not limited to LiOH.H2O. Lithium oxide (Li2O) and lithium hydroxide (LiOH) are preferred.

[0048] In the lithium source, the fluoride is uniformly dispersed, preferably lithium fluoride. The term "uniformly dispersed" means that, for example, by X-ray diffraction, particle size distribution, optical microscopy and SEM / EDX (scanning electron microscopy / energy dispersive X-ray spectroscopy), no individual crystals or agglomerates of fluoride or even LiF may be detected. Particle size distribution and X-ray diffraction and SEM / EDX are preferred.

[0049] Preferably, the fluoride-containing lithium source is produced by recycling spent batteries, for example by a recovery process of lithium carbonate or lithium hydroxide from a lithium salt solution containing fluoride (e.g. derived from an electrolyte such as LiPF6 or from a decomposed fluoropolymer binder).

[0050] In one embodiment of the present invention, the recovery method comprises the following steps:

[0051] (i) producing black powder, sometimes referred to as black matter or active matter, from spent lithium-ion batteries by mechanical destruction of the batteries followed by thermal treatment,

[0052] (ii) treating the black powder with at least one of Ca(OH)2 or Mg(OH)2 in the presence of water or a polar solvent other than water at a temperature of at least 70°C, preferably 70°C to 120°C,

[0053] (iii) separating the solid from the liquid, preferably by filtration, optionally followed by washing the solid residue with a polar solvent such as water, thereby obtaining a solution of lithium hydroxide containing fluoride, and

[0054] (iv) optionally after purification of the solution, removing water from the solution of lithium hydroxide by one or more steps, for example by evaporation, to produce solid LiOH.

[0055] In another embodiment, steps (i) to (iii) are performed after step (v),

[0056] (v) adding CO2 or any water-soluble carbonate, such as Na2CO3, to precipitate Li2CO3,

[0057] (vi) separating the solid from the liquid by a solid-liquid separation method, such as filtration, optionally followed by washing the solid residue with a polar solvent such as water, thereby obtaining solid lithium carbonate containing fluoride.

[0058] The lithium hydroxide produced according to the above recovery method generally contains 0.01% to 1.3% by weight of fluoride relative to the monohydrate of LiOH, preferably 0.05% to 0.5% by weight. Depending on the drying conditions, anhydrous LiOH is obtained instead of the monohydrate. In this case, the characteristic amounts of the above-mentioned impurities related to the monohydrate are respectively higher in concentration, about 1.75 times higher for 100% anhydrous LiOH (corresponding to the molar amount of the monohydrate divided by the molar amount of the anhydrate).

[0059] The lithium carbonate produced according to the above recovery method generally contains 0.01 to 1.5% by weight of fluoride, preferably 0.05 to 0.5% by weight.

[0060] Step (c) comprises mixing the oxide or (oxy)hydroxide of TM with the fluoride-containing lithium source, and with an additional lithium source containing less fluoride, and optionally with one or more dopants based on at least one metal other than lithium. By carrying out step (c), a mixture is obtained. The expression "the fluoride-containing lithium source" is the lithium source provided in step (b). The expression "containing less fluoride" refers to a lithium source compared to the lithium source provided in step (b).

[0061] The combined amounts of precursors and total lithium source will correspond to the desired stoichiometry of the target cathode active material. Typically a stoichiometric amount or even a slight excess of lithium relative to the metal other than lithium is selected.

[0062] Step (c) may comprise mixing with an additional lithium source which contains less fluoride than the lithium source provided in step (b), for example 1 to 150 ppm, or even below detection levels.

[0063] The dopant is selected from oxides, hydroxides and oxyhydroxides of Mg, Y, Ti, Zr, W, Nb, Ta and especially Al. Lithium titanate is a possible titanium source. Examples of dopants are MgO, Mg(OH)2, TiO2 (selected from rutile and anatase, preferably anatase), and basic titanium oxides such as TiO(OH)2, and Li4Ti5O 12, ZrO2, Zr(OH)4, Li2ZrO3, Nb2O3, Ta2O5, Li2WO4, WO3, MoO3, Li2MoO4, yttrium oxide, Al(OH)3, Al2O3, Al2O3 hydrate and AlOOH. Preferred Al compounds are Al(OH)3, α-Al2O3, γ-Al2O3, Al2O3 hydrate and AlOOH, as well as TiO2 and Zr(OH)4. Even more preferred dopants are Al2O3 selected from α-Al2O3, γ-Al2O3, and most preferably γ-Al2O3.

[0064] In a preferred embodiment, relative to iron and M 1 One or more dopants are applied in an amount of up to 2.5 mol %, preferably 0.1 up to 1.5 mol %.

[0065] In one embodiment of the invention, a carbon source is also added in step (c). Suitable carbon sources are organic compounds that decompose to form carbon during the heat treatment process of step (e). Suitable carbon sources are organic polymers, such as but not limited to polyethylene glycol, polypropylene, starch, cellulose. Other examples of carbon sources include low molecular weight organic compounds, such as lactic acid, monosaccharides or disaccharides, such as glucose, fructose, mannose, lactose and maltose, ascorbic acid (which can be used as both a reducing agent and a carbon source), stearic acid, citric acid, and ammonium salts thereof. It is preferred to avoid using alkali metal salts other than lithium salts as carbon sources.

[0066] Examples of suitable equipment for carrying out step (c) are high shear mixers, drum mixers, ploughshare mixers and free fall mixers.

[0067] In one embodiment of the present invention, step (c) is carried out at a temperature ranging from ambient temperature to 200°C, preferably from 20°C to 50°C.

[0068] In one embodiment of the present invention, the duration of step (c) is 10 minutes to 2 hours. Depending on whether additional mixing is performed in step (d), sufficient mixing must be completed in step (c).

[0069] The mixing of the precursor, the lithium source from step (b) and - optionally - a further lithium source and / or one or more dopants and, if applicable, a carbon source can all be carried out in one step or in sub-steps, for example by first mixing the lithium source containing fluoride with the one or more dopants and adding this mixture to the precursor, or by first mixing the precursor with the lithium source containing fluoride and then adding the dopant and further lithium source, or by first mixing the dopant with the precursor and then adding the lithium source containing lithium fluoride and further lithium source. It is preferred to first mix the precursor with both lithium sources and then add the dopant or carbon source, as the case may be.

[0070] In one embodiment of the present invention, step (c) comprises two sub-steps:

[0071] (c1) mixing a fluoride-containing lithium source with a fluoride-free lithium source, and optionally the one or more dopants,

[0072] (c2) mixing the mixture obtained from step (c1) with the oxide or (oxy)hydroxide of said TM and - if applicable - with said one or more dopants or carbon source.

[0073] In one embodiment of the present invention, the weight ratio of the fluoride-containing lithium source to the fluoride-free lithium source as provided in step (b) is in the range of 20:1 to 1:20, preferably 1:1 to 1:20.

[0074] Although an organic solvent, such as glycerol or ethylene glycol, or water may be added in step (c), it is preferred to carry out step (c) in a dry state without adding water or an organic solvent.

[0075] A mixture was obtained.

[0076] In the optional step (d), at least two components of the mixture from step (c) are reacted to obtain an adduct. During the formation of the adduct, some reaction occurs between the iron source, the phosphate source and the lithium source or with some reducing agent, but the composition of the adduct is different from the composition of the target cathode active material having an olivine structure. In most cases, the carbon source has not yet decomposed when the adduct is formed. However, in most cases, some iron (III) reduction has occurred, at least to a significant extent.

[0077] In one embodiment of step (d), the chemical reaction is carried out in the presence of a solvent, such as water or a water-miscible solvent, such as a C2-C4-alkanol or NMP or N-ethylpyrrolidone ("NEP"). At the end of step (d), the solvent or water may be at least partially removed, for example by a spray drying process. Although a slurry or paste may be fed in step (e), it is preferred that a powder or wet powder is fed in step (e).

[0078] Step (e) comprises heat treating the mixture from step (c) or the adduct from step (d) (if applicable), for example at a temperature in the range of 400 to 1000°C, preferably 600 to 900°C.

[0079] In one embodiment of the present invention, the mixture from step (c) or the adduct from step (d) is heated to 400°C to 1000°C at a heating rate of 0.1 to 10°C / min.

[0080] In one embodiment of the invention, the temperature is ramped up before reaching the desired temperature of 400° C. to 1000° C., preferably 600° C. to 900° C. In a preferred example, the mixture from step (c) is first heated to a temperature of 300° C. to 400° C. and then kept constant for a period of 10 minutes to 4 hours, and then it is increased to 650° C. up to 900° C.

[0081] In embodiments where at least one solvent is used in step (c) or (d) (if applicable), the one or more solvents are removed as part of step (e), or separately and prior to starting step (e), for example by filtering, evaporating or distilling the one or more solvents. Evaporation and distillation are preferred.

[0082] In one embodiment of the invention, step (e) is carried out in a roller hearth kiln, a pusher kiln or a rotary kiln or a combination of at least two of the foregoing. The advantage of a rotary kiln is that the homogeneity of the material produced therein is very good. In roller hearth kilns and pusher kilns, different reaction conditions for the different steps can be easily set. In laboratory scale tests, box furnaces and tube furnaces as well as split tube furnaces are also feasible.

[0083] In one embodiment of the present invention, step (e) is performed in an inert atmosphere (such as nitrogen or a noble gas), or in a reducing atmosphere (for example under hydrogen).

[0084] By implementing the method of the present invention, a cathode active material showing excellent stability, such as low capacity fade and high cycle stability, and a constant composition is produced.

[0085] Another aspect of the present invention is a cathode active material, also referred to hereinafter as the cathode active material of the present invention. The cathode active material of the present invention can be represented by the general formula LiFe (1-x) M 1 x (PO4) 1-y F 3y and its average particle size (D50) is in the range of 1 to 16 μm, preferably 2 to 10 μm and more preferably 3 to 5 μm, wherein M 1 Selected from Ni, Ti, V, Y, Al, Mg, Zn, Cu, Co and Mn, and wherein x is in the range of 0 to 0.45, and wherein y is in the range of 0.0002 to 0.03, and F is uniformly distributed in this cathode active material.

[0086] M 1 Preferred examples of x are Ni, Ti, V, Co and Mn. More preferably, x is 0.

[0087] F is uniformly distributed in the cathode active material of the present invention in the form of fluoride. This means that F is not accumulated on the outer surface of the secondary particles, but inside the secondary particles. Some fluoride may accumulate at the grain boundaries of the primary particles, but preferably there is no accumulation. In addition, there are few or even no secondary particles that do not contain fluoride.

[0088] The cathode active material of the present invention is in granular form. In one embodiment of the present invention, the average particle size (D50) of the cathode active material of the present invention is in the range of 1 to 16 μm, preferably 2 to 10 μm, and more preferably 3 to 5 μm. The average particle size (D50) in the context of the present invention refers to the median of the volume-based particle size as can be determined, for example, by light scattering. In one embodiment, the precursor has a unimodal particle size distribution. In other embodiments, the particle distribution of the precursor can be bimodal, for example, having a maximum value in the range of 1 to 5 μm, and having another maximum value in the range of 7 to 16 μm.

[0089] The particle shape of the secondary particles of the cathode active material of the present invention is preferably spherical, which are particles with a spherical shape. Spherical spheres should include not only those particles that are completely spherical, but also those particles in which at least 90% (number average) of the representative samples have a maximum and minimum diameter that differ by no more than 10%.

[0090] In one embodiment of the present invention, the cathode active material of the present invention is composed of secondary particles, which are agglomerates of primary particles. Preferably, the precursor is composed of spherical secondary particles, which are agglomerates of primary particles. Even more preferably, the precursor is composed of spherical secondary particles, which are agglomerates of spherical primary particles or flakes.

[0091] In one embodiment of the present invention, the cathode active material of the present invention has a particle size distribution span in the range of 0.5 to 0.9, which is defined as [(D90)-(D10)] divided by (D50), all of which are determined by laser analysis. In another embodiment of the present invention, the precursor may have a particle size distribution span in the range of 1.1 to 1.8.

[0092] In one embodiment of the present invention, the cathode active material of the present invention further contains conductive modified carbon, also referred to as C. C can be selected from soot, activated carbon, carbon nanotubes, graphene and graphite. C can be added in its own form during the preparation of the electrode material according to the present invention, or can be prepared in situ with the cathode active material having an olivine crystal structure by decomposing a carbon source during step (e).

[0093] In one embodiment of the present invention, the amount of C is in the range of 1 to 8% by weight, preferably at least 2% by weight, relative to the cathode active material having an olivine crystal structure.

[0094] In one embodiment of the present invention, the surface (BET) of the cathode active material of the present invention is between 5 and 35 m 2 / g, preferably 7 to 15m 2 / g range.

[0095] In one embodiment of the present invention, the cathode active material of the present invention is in the form of primary particle agglomerates having an average diameter (d50) ranging from 1 μm to 10 μm, preferably from 2 to 5 μm, even more preferably from 4 to 5 μm.

[0096] In one embodiment of the present invention, the cathode active material having an olivine crystal structure of the present invention is coated with a C layer between primary crystallites (primary particles) and on the surface of secondary particles. The layer may be incomplete or complete.

[0097] In one embodiment of the present invention, the average primary particle size of C is in the range of 1 to 500 nm, preferably in the range of 2 to 100 nm, particularly preferably in the range of 2 to 50 nm, very particularly preferably in the range of 2 to 4 nm or less.

[0098] A further aspect of the invention relates to an electrode comprising at least one particulate cathode active material according to the invention. They are particularly useful for lithium ion batteries. A lithium ion battery comprising at least one electrode according to the invention exhibits good cycling behavior / stability. An electrode comprising at least one particulate cathode active material according to the invention is also referred to hereinafter as a cathode according to the invention or a cathode according to the invention.

[0099] Specifically, the cathode of the present invention contains

[0100] (A) at least one cathode active material according to the present invention,

[0101] (B) carbon in a conductive form, added after the manufacture of the cathode material (A) or produced in situ,

[0102] (C) an adhesive material, also referred to as an adhesive or adhesive (C), and preferably,

[0103] (D) Current collector.

[0104] In a preferred embodiment, the cathode of the present invention comprises

[0105] (A) 80 to 98% by weight of the particulate cathode active material of the present invention,

[0106] (B) 1 to 17% by weight of carbon,

[0107] (C) 1 to 15% by weight of a binder,

[0108] Percentages are relative to the sum of (A), (B), and (C).

[0109] The cathodes according to the present invention may comprise additional components. They may include a current collector such as, but not limited to, aluminum foil. They may further comprise conductive carbon and a binder.

[0110] The cathode according to the present invention contains conductive modified carbon, also referred to as carbon (B) for short. Carbon (B) may be selected from soot, activated carbon, carbon nanotubes, graphene and graphite, and a combination of at least two of the foregoing.

[0111] Suitable binders (C) are preferably selected from organic (co)polymers. Suitable (co)polymers, i.e. homopolymers or copolymers, can be selected from (co)polymers obtainable, for example, by anionic, catalytic or free radical (co)polymerization, in particular from polyethylene, polyacrylonitrile, polybutadiene, polystyrene, and copolymers of at least two comonomers selected from ethylene, propylene, styrene, (meth)acrylonitrile and 1,3-butadiene. Polypropylene is also suitable. In addition, polyisoprene and polyacrylates are also suitable. Polyacrylonitrile is particularly preferred.

[0112] In the context of the present invention, polyacrylonitrile is understood to mean not only polyacrylonitrile homopolymers but also copolymers of acrylonitrile with 1,3-butadiene or styrene. Polyacrylonitrile homopolymers are preferred.

[0113] In the context of the present invention, polyethylene is understood to mean not only homopolyethylene but also copolymers of ethylene which comprise at least 50 mol % of copolymerized ethylene and up to 50 mol % of at least one further comonomer, for example α-olefins such as propylene, butene (1-butene), 1-hexene, 1-octene, 1-decene, 1-dodecene, 1-pentene and also isobutene, vinylaromatic compounds such as styrene and also (meth)acrylic acid, vinyl acetate, vinyl propionate, C1-C12-hydroxyethyl esters of (meth)acrylic acid. 10 - Alkyl esters, especially methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, n-butyl acrylate, 2-ethylhexyl acrylate, n-butyl methacrylate, 2-ethylhexyl methacrylate, and also maleic acid, maleic anhydride and itaconic anhydride. The polyethylene may be HDPE or LDPE.

[0114] In the context of the present invention, polypropylene is understood to mean not only homopolypropylene, but also copolymers of propylene, which contain at least 50 mol-% copolymerized polypropylene and up to 50 mol-% of at least one further comonomer, for example ethylene and α-olefins such as butene, 1-hexene, 1-octene, 1-decene, 1-dodecene and 1-pentene. The polypropylene is preferably isotactic or substantially isotactic.

[0115] In the context of the present invention, polystyrene is understood to mean not only homopolymers of styrene but also C1-C12 copolymers with acrylonitrile, 1,3-butadiene, (meth)acrylic acid, (meth)acrylic acid, and the like. 10 - copolymers of alkyl esters, divinylbenzene, especially 1,3-divinylbenzene, 1,2-diphenylethylene and α-methylstyrene.

[0116] Another preferred binder (C) is polybutadiene.

[0117] Other suitable binders (C) are selected from polyethylene oxide (PEO), cellulose, carboxymethylcellulose, polyimide and polyvinyl alcohol.

[0118] In one embodiment of the present invention, the binder (C) is selected from a group consisting of binders having an average molecular weight M in the range of 50,000 to 1,000,000 g / mol, preferably to 500,000 g / mol. w Those (co)polymers.

[0119] The binder (C) may be a cross-linked or non-cross-linked (co)polymer.

[0120] In a particularly preferred embodiment of the present invention, binder (C) is selected from halogenated (co) polymers, especially fluorinated (co) polymers. Halogenated or fluorinated (co) polymers are understood to mean those (co) polymers comprising at least one (co) polymerized (co) monomer having at least one halogen atom or at least one fluorine atom per molecule, more preferably at least two halogen atoms or at least two fluorine atoms per molecule. Examples are polyvinyl chloride, polyvinylidene chloride, polytetrafluoroethylene, polyvinylidene fluoride (PVdF), tetrafluoroethylene-hexafluoropropylene copolymer, vinylidene fluoride-hexafluoropropylene copolymer (PVdF-HFP), vinylidene fluoride-tetrafluoroethylene copolymer, perfluoroalkyl vinyl ether copolymer, ethylene-tetrafluoroethylene copolymer, vinylidene fluoride-chlorotrifluoroethylene copolymer and ethylene-chlorofluoroethylene copolymer.

[0121] Suitable binders (C) are, in particular, polyvinyl alcohols and halogenated (co)polymers, for example polyvinyl chloride or polyvinylidene chloride, and in particular fluorinated (co)polymers, such as polyvinyl fluoride and in particular polyvinylidene fluoride and polytetrafluoroethylene.

[0122] The cathode of the present invention may contain 1% to 15% by weight of one or more binders relative to the cathode active material of the present invention. In other embodiments, the cathode of the present invention may contain 0.1% to less than 1% by weight of one or more binders.

[0123] Another aspect of the invention is a battery comprising at least one cathode comprising the cathode active material of the invention, carbon, and a binder, at least one anode, and at least one electrolyte.

[0124] The embodiments of the cathode of the present invention have been described above in detail.

[0125] The anode may contain at least one anode active material, such as carbon (graphite), TiO2, lithium titanium oxide, silicon or tin. The anode may additionally contain a current collector, such as a metal foil such as copper foil.

[0126] The electrolyte may include at least one non-aqueous solvent, at least one electrolyte salt, and optionally additives.

[0127] The nonaqueous solvent of the electrolyte may be liquid or solid at room temperature and is preferably selected from polymers, cyclic or acyclic ethers, cyclic or acyclic acetals, and cyclic or acyclic organic carbonates.

[0128] Examples of suitable polymers are in particular polyalkylene glycols, preferably poly-C1-C4-alkylene glycols, and in particular polyethylene glycol. Polyethylene glycol may account for up to 20 mol% of one or more C1-C4-alkylene glycols. Polyalkylene glycols are preferably polyalkylene glycols with two methyl or ethyl end caps.

[0129] The molecular weight M of suitable polyalkylene glycols and in particular suitable polyethylene glycols is w It may be at least 400 g / mol.

[0130] The molecular weight M of suitable polyalkylene glycols and in particular suitable polyethylene glycols is w It may be up to 5,000,000 g / mol, preferably up to 2,000,000 g / mol.

[0131] Examples of suitable acyclic ethers are, for example, diisopropyl ether, di-n-butyl ether, 1,2-dimethoxyethane, 1,2-diethoxyethane, of which 1,2-dimethoxyethane is preferred.

[0132] Examples of suitable cyclic ethers are tetrahydrofuran and 1,4-dioxane.

[0133] Examples of suitable acyclic acetals are, for example, dimethoxymethane, diethoxymethane, 1,1-dimethoxyethane and 1,1-diethoxyethane.

[0134] Examples of suitable cyclic acetals are 1,3-dioxane and in particular 1,3-dioxolane.

[0135] Examples of suitable acyclic organic carbonates are dimethyl carbonate, ethyl methyl carbonate and diethyl carbonate.

[0136] Examples of suitable cyclic organic carbonates are compounds according to the general formula (II) and (III)

[0137]

[0138] Where R 1 , R 2 and R 3 may be identical or different and are selected from hydrogen and C1-C4-alkyl, for example methyl, ethyl, n-propyl, isopropyl, n-butyl, isobutyl, sec-butyl and tert-butyl, wherein R 2 and R 3 Preferably, not all of them are tert-butyl. In another embodiment, R in formula (II) 1 is fluorine and R 2 and R 3 It's hydrogen.

[0139] In a particularly preferred embodiment, R 1 is methyl and R 2 and R 3 Each is hydrogen, or R 1 , R 2 and R 3 Each is hydrogen.

[0140] Another preferred cyclic organic carbonate is vinylene carbonate, formula (IV).

[0141]

[0142] The solvent or solvents are preferably used in anhydrous state, ie with a water content in the range from 1 ppm to 0.1% by weight, which can be determined, for example, by Karl-Fischer titration.

[0143] The electrolyte (C) further comprises at least one electrolyte salt. Suitable electrolyte salts are in particular lithium salts. Examples of suitable lithium salts are LiPF6, LiBF4, LiClO4, LiAsF6, LiCF3SO3, LiC(C n F 2n+1 SO2)3, lithium imide such as LiN(C n F 2n+1SO2)2, wherein n is an integer in the range of 1 to 20, LiN(SO2F)2, Li2SiF6, LiSbF6, LiAlCl4 and compounds having the general formula (C n F 2n+1 SO2) t Salts of YLi, wherein m is defined as follows:

[0144] When Y is selected from oxygen and sulfur, t=1,

[0145] When Y is selected from nitrogen and phosphorus, t=2, and

[0146] When Y is selected from carbon and silicon, t=3.

[0147] Preferred electrolyte salts are selected from LiC(CF3SO2)3, LiN(CF3SO2)2, LiPF6, LiBF4, LiClO4, among which LiPF6 and LiN(CF3SO2)2 are particularly preferred.

[0148] In an embodiment of the invention, the battery according to the invention comprises one or more separators, by means of which the electrodes are mechanically separated. Suitable separators are polymer films, in particular porous polymer films, which are non-reactive to metallic lithium. Particularly suitable materials for separators are polyolefins, in particular film-forming porous polyethylene and film-forming porous polypropylene.

[0149] The membrane composed of polyolefin, in particular polyethylene or polypropylene, can have a porosity in the range of 35% to 45%. Suitable pore diameters are, for example, in the range of 30 to 500 nm.

[0150] In another embodiment of the present invention, the separator can be selected from a PET nonwoven material filled with inorganic particles. Such a separator can have a porosity in the range of 40% to 55%. Suitable pore sizes are, for example, in the range of 80 to 750 nm.

[0151] The battery according to the invention further comprises a housing, which may have any shape, for example a cubic or cylindrical disc or cylindrical can shape. In a variant, a metal foil configured as a pouch is used as housing.

[0152] The battery according to the present invention shows good cycling stability and low capacity fade.

[0153] The battery according to the invention may comprise two or more electrochemical cells combined with one another, which may be connected in series or in parallel, for example. Preferably they are connected in series. In the battery according to the invention, at least one of the electrochemical cells comprises at least one cathode according to the invention. Preferably, in the electrochemical cells according to the invention, the majority of the electrochemical cells comprise a cathode according to the invention. Even more preferably, in the battery according to the invention, all electrochemical cells comprise a cathode according to the invention.

[0154] The invention further provides for the use of a battery according to the invention in an apparatus, in particular in a mobile device. Examples of mobile devices are vehicles, such as cars, bicycles, aircraft or water vehicles (such as ships or vessels). Other examples of mobile devices are those that are moved manually, such as computers, in particular laptops, telephones or electric hand tools, such as in the construction industry, in particular drills, battery-powered screwdrivers or battery-powered staplers.

[0155] The present invention is further illustrated by the following working examples.

[0156] Description of the method

[0157] Li in aqueous solution was determined by optical emission spectroscopy using inductively coupled plasma (ICP-OES). Instrument: ICP-OES Agilent 5100SVDV; Wavelength: Li 670.783 nm; Internal standard: Sc 361.383 nm; Dilution factor: Li; Calibration: external.

[0158] Elemental analysis of fluorine and fluoride was performed according to the standardized methods: DIN EN 14582:2016-12 on sample preparation for determination of bulk fluorine content (waste sample); detection method is ion-selective electrode measurement. DIN 38405-D4-2:1985-07 (water samples; digestion of inorganic solids, followed by acid-loaded distillation and fluoride determination using an ion-selective electrode).

[0159] Starting Materials:

[0160] "Battery grade" LiOH.H2O, hereinafter also referred to as "LiOH bg", is commercially available from Livent and has a fluoride content of less than 5 ppm

[0161] LiF was commercially available from Sigma Aldrich.

[0162] I. Providing starting materials for calcination

[0163] I.1 Synthesis of LiOH containing LiF, step (b.1)

[0164] According to the method described in Jia Li et al., Journal of Hazardous Materials 2016, 302, 97-104, about 1 t of mechanically treated battery waste is treated to obtain reduced material, the battery waste containing spent cathode active material (containing nickel, cobalt and manganese), organic carbon in the form of graphite and soot, and residual electrolyte, and other impurities (including fluorine compounds, phosphorus and calcium in particular). The atmosphere in the roasting system is air, the oxygen in which reacts with the carbon in the battery waste to form carbon monoxide, and the treatment temperature is 800°C.

[0165] After reaction and cooling to ambient temperature, the heat treated material was recovered from the furnace, mechanically treated to obtain granular material and analyzed by X-ray powder diffraction, elemental analysis and particle size distribution.

[0166] The Li content was 3.6 wt.-%, providing a reference for the following leaching procedure (see below). Fluorine (2.6 wt.-%) was mainly present as inorganic fluorides (2.3 wt.-%). The particle size was well below 1 mm; D50 was determined to be 17.36 μm.

[0167] The obtained XRD pattern was compared with the calculated reference pattern of Ni (which is the same as the pattern of one of the following: Co x Ni 1-x , x = 0 to 0.6, Co, Li2CO3 and LiAlO2), the following conclusions can be drawn: Ni is completely present in the form of a metallic phase, pure Ni or an alloy combined with Co. When in contact with permanent magnetic materials, the entire sample shows typical ferromagnetic behavior. As lithium salts, Li2CO3 and LiAlO2 can be clearly identified by their characteristic diffraction patterns.

[0168] Leaching of heat-treated black material with Ca(OH)2:

[0169] A PFA flask was charged with 30 g of the above heat treated battery waste material and 9 g of solid Ca(OH)2. The solids were mixed. Then, 200 g of water was added under stirring and the whole mixture was refluxed for 6 hours. After 6 hours, the solid content was filtered off and the filtrate sample was taken and analyzed for Li (c(Li)=0.49 wt.-%) and F (c(F)=0.015 wt.-%).

[0170] Solid LiOH from leached LiOH filtrate

[0171] The filtrate obtained from the above experiment was then dried to produce solid LiOH as a monohydrate containing fluoride. Two different procedures were applied to adjust the fluoride content:

[0172] (A) Water is completely evaporated from 150 mL of a filtrate containing 0.49 wt.-% lithium and 0.015 wt.-% fluoride (40° C., 42 mbar). LiOH·LiF.1 is obtained. The XRD of LiOH·LiF.1 shows a small amount of Li2CO3 impurity. The latter is due to contact with air during most of the process steps. In addition to carbon-based impurities, elemental analysis shows fluoride as one of the main impurities (c(F)=0.5 wt.-%).

[0173] (B) Another 150 mL portion of the filtrate from another LiOH leaching experiment (containing 0.49 wt.-% lithium and 0.015 wt.-% fluoride) was concentrated 6-fold by evaporation (40° C., 42 mbar) (c(Li)=2.94 wt.-%), filtered and finally dried at 40° C. under a constant nitrogen flow for 24 h. XRD of LiOH·LiF.2 shows a small amount of Li2CO3 impurity. The latter is due to contact with air during most of the process steps. In addition to carbon-based impurities, elemental analysis shows fluoride as one of the main impurities (c(F)=0.25 wt.-%).

[0174] I.2 Synthesis of Li2CO3 containing fluoride, step (b.2)

[0175] CO2 was introduced into a LiOH solution containing 2.6 wt.-% lithium and 0.017 wt.-% fluoride for seven hours (ambient conditions, about 5 L / h). A white solid immediately emerged. After 7 hours, the solid was filtered off, dried and analyzed by XRD and by elemental analysis: Li2CO3·LiF.2 (Li=19.0 wt.-%, F=0.22 wt.-%). No separate LiF was detected.

[0176] II. Preparation of cathode active materials

[0177] II.1 Step (a.1), mixing step, step (c.1), and calcination, step (d.1)

[0178] “Battery grade” LiOH.H 2 O (hereinafter also referred to as “LiOH bg”, commercially available from Levent Corporation, having a fluoride content of less than 5 ppm) was used for mixing with LiOH.LiF.1.

[0179] Providing an iron source and a phosphate source, step (a.1)

[0180] Provides the following ingredients:

[0181]

[0182]

[0183] Step (b.1): LiOH bg and LiOH·LiF.1 were mixed in a MICROTRON laboratory mixer from Kinematica in a molar ratio of LiOH bg to LiOH·LiF.1 of 1:1. A mixture was obtained.

[0184] Step (c.1):

[0185] 4,600 g of H2O was charged into a 6-1 reactor equipped with a mixer and a heater. The water was heated to a temperature of 76°C. Then the addition of the individual ingredients was started. First, 75.7 g of the mixture from step (b.1) (corresponding to 3.16 mol of Li) was added and dissolved within 20 min. Due to the exothermic reaction, the solution temperature rose to 80.5°C. Then, α-FeOOH was added and stirred for another 20 min. Then, H3PO4 and H3PO3 were added. After 20 minutes, starch and lactose were added in powder form.

[0186] Step (d.1): The temperature of the yellow slurry thus obtained was 87°C. Then, 500 g of H2O was added. The slurry thus obtained was stirred at 85°C for 21 hours. The solid was then isolated by spray drying. N2 (25 Nm 3 / h) as drying gas, and applying the following spray drying parameters, the slurry prepared in the above step is spray dried:

[0187] T 进 295℃-298℃

[0188] T 出 135℃-143℃

[0189] Slurry feed: 724.1g / h

[0190] After spray drying, 125 g of yellow spray powder, Adduct 1, was obtained.

[0191] Step (e.1): 60 g of the spray powder obtained as above were calcined in a rotating quartz bulb. The rotating bulb rotated at a speed of 10 rpm. The spray powder sample was heated from ambient temperature to a temperature of 700° C. at a heating rate of 11.33° C. / min. Finally, the material was calcined at a temperature of 700° C. for 1 hour under a stream of N2 (16 NL / h). The CAM.1 according to the invention thus obtained as a black powder was then cooled to ambient temperature and sieved, (D50): 5 μm.

[0192] Electrochemical testing was performed in a coin-type half-cell, showing excellent first cycle discharge capacity and cycling stability.

[0193] II.2 Preparation of comparative cathode active material (C-CAM.2)

[0194] Repeat step (a.1) and step (a.2).

[0195] Step (b.1) is not performed.

[0196] In step C-(c.2), pure LiOH·H2O bg was added. Steps C-(d.2) and C-(e.2) were carried out similarly. A comparative material, C-CAM.2, was obtained.

[0197] II.3 Preparation of comparative cathode active material (C-CAM.3)

[0198] Repeat step (a.1) and step (a.3).

[0199] Compare step C-(b.3):

[0200] LiOH·H2O bg and LiF were mixed in a MICROTRON laboratory mixer from Cainmetall in a weight ratio of 99.66:0.34. A premix was obtained. As can be seen from the crystals, LiF crystals were still present in the premix.

[0201] Steps C-(d.3) and C-(e.3): Step (d.1) was repeated, but using the mixture from step C-(c.3). After cooling to ambient temperature, the resulting powder was deagglomerated and sieved through a 50 μm sieve. C-CAM.3 was obtained. Several samples of C-CAM.3 showed different and inconsistent behavior compared to CAM.1 and C-CAM.2.

[0202] III. Testing of cathode active materials

[0203] III.1 Cathode fabrication, general procedure

[0204] Positive electrode: PVDF binder ( 5130) was dissolved in NMP (Merck) to produce a 7.5 wt.% solution. For the preparation of the electrodes, the binder solution (3 wt.%) and carbon black (Super C65, 3 wt.-%) were suspended in NMP. After mixing using a planetary centrifugal mixer (ARE-250, Thinky Corp.; Japan), the CAM of the present invention (or comparative CAM) (94 wt.%) was added and the suspension was mixed again to obtain a lump-free slurry. The solid content of the slurry was adjusted to 61%. The slurry was coated on Al foil using a KTF-S roll-to-roll coater (Mathis AG). All electrodes were calendered before use. The thickness of the cathode material was 100 μm, corresponding to 6.5 mg / cm 2 Before cell assembly, all electrodes were dried at 105 °C for 7 h.

[0205] III.2 Electrolyte Preparation

[0206] A substrate electrolyte composition (EL substrate 1) was prepared containing 1 M LiPF6 in 3:7 by weight ethylene carbonate and ethyl methyl carbonate.

[0207] III.3 Fabrication of test cells

[0208] The following ingredients were blended with each other to produce the cathode (A.1):

[0209] 93g CAM.1

[0210] 3 g of polyvinylidene fluoride, (c.1) ("PVdF"), available from Arkema Group as Kynar 2801 Commercial,

[0211] 2.5 g of carbon black, (b.1), BET surface area 62 m 2 / g, commercially available from Timcal as "SuperC 65L",

[0212] 1.5 g of graphite, (b.2), commercially available from Temeco as KS6.

[0213] A sufficient amount of N-methylpyrrolidone (NMP) was added while stirring and the mixture was stirred with an Ultraturrax until a firm, lump-free paste was obtained.

[0214] The cathode was prepared as follows: the paste was applied to a 30 μm thick aluminum foil using a 15 μm doctor blade. The loading after drying was 2.0 mAh / cm 2The loaded foil was dried in a vacuum oven at 105 °C for 16 h. After cooling to room temperature in a fume hood, a disc-shaped cathode was punched out on the foil. The cathode disc was then weighed and introduced into an argon glove box, where it was vacuum dried again. The prepared disc was then used to assemble the battery cell.

[0215] The electrochemical tests were carried out in "TC2" button cell cells. The electrolyte used (C.1) was a 1 M solution of LiPF6 in ethyl methyl carbonate / ethylene carbonate (1:1 by volume).

[0216] Separator (D.1): Glass fiber. Anode (B.1): Graphite. Potential range of battery cell: 2.50V to 4.0V.

[0217] An electrochemical cell according to the invention (BAT.1) was obtained.

[0218] III.4 Production of cathodes and electrochemical cells according to the invention and production of comparative cathodes and electrochemical cells

[0219] For comparative purposes, the above experiment was repeated, but with an equal amount of C-CAM.2 replacing (CAM.1) of the invention. A comparative electrochemical cell C-(BAT.2) was obtained.

[0220] IV. Battery Testing

[0221] The electrochemical cell according to the invention and the comparative electrochemical cell were each subjected to the following cycle schedule: Cell potential range: 2.50 V to 4.0 V, 0.1 C (1st cycle), 0.2 C (2nd to 7th cycles). 1 C = 160 mA / g. Temperature: 45°C, ambient temperature and -25°C.

[0222] Compared to comparative electrochemical cells, the electrochemical cells according to the invention showed overall very good or better performance.

[0223] The electrical conductivity can be determined as follows:

[0224] Disc-shaped pellets were formed from (CAM. 1) with a diameter of 0.8 cm and a height between 7 mm (at 100 bar) and 1 to 2 mm (at 500 bar). The electrical conductivity was measured according to BJ Ingram et al., J. Electrochem. Soc. 2003, 150, E396.

[0225] As a comparison, disc-shaped pellets having a diameter of 1.4 cm and a height of 6 mm were formed from C-(CAM.2) and tested under the same conditions.

[0226] The battery based on the cathode active material of the present invention is more excellent. In particular, Bat.1 based on CAM.1 shows higher cycle stability and lower resistance growth compared to C-Bat.2 based on C-CAM.2 and C-Bat.3 based on C-CAM.3. In particular, several samples of C-CAM.3 show completely different electrochemical behaviors. Without wishing to be bound by any theory, we assume that some samples of C-CAM.3 contain fluoride, while others do not.

Claims

1. A method for producing a fluoride-doped cathode active material having an olivine crystal structure, wherein the method comprises the following steps: (a) providing a phosphate source, a source of a metal other than lithium and selected from iron, and optionally at least one further element M 1 a source of an element selected from vanadium, titanium, nickel, cobalt, copper, zinc, magnesium, aluminium, yttrium and manganese, wherein at least 55 mol-% of the metal other than lithium is iron, and wherein the source can be formed from one or more compounds, (b) providing a lithium source, the lithium source containing 0.01% to 2.5% by weight of fluoride uniformly dispersed in the lithium source, wherein the lithium source is selected from lithium hydroxide and lithium carbonate, (c) mixing said phosphate source and source of a metal other than lithium with said fluoride-containing lithium source, and with an additional lithium source containing less fluoride, and optionally with a hydrocarbon, (d) optionally, reacting at least two components of the mixture from step (c) to obtain an adduct, (e) treating the mixture obtained from step (c) or the adduct from step (d) at a temperature ranging from 400°C to 1000°C under a reducing or inert atmosphere.

2. The method according to claim 1, wherein: The sources of phosphate and transition metal are provided by the following steps: (a1) combining an aqueous solution of an iron (+III) salt, ammonium (hydrogen) phosphate and a reducing agent, or (a2) combining an aqueous slurry of an iron compound selected from Fe2O3, Fe3O4, FeOOH and Fe(OH)3 with a reducing agent and a phosphate source, or (a3) combining an aqueous solution of an iron (+III) salt, a phosphate source, and optionally at least one reducing agent and polyethylene glycol, or (a4) providing a solution of a Fe(+II) compound in an organic solvent and a solution of H3PO4 in a water-miscible solvent, or (a5) mixing Fe(+II) oxalate and ammonium dihydrogen phosphate in the presence of a C1-C6-alkanol or polyethylene glycol, (a6) synthesizing FePO4 with an average particle size in the range of 1 to 16 μm, In each case this was done in the absence or presence of cobalt or manganese compounds.

3. The method according to claim 1 or 2, wherein: The lithium source is lithium hydroxide.

4. A method according to any one of the preceding claims, wherein: Step (e) is performed at a temperature ranging from 850°C to 1000°C.

5. A method according to any one of the preceding claims, wherein: In step (a), a reducing agent is also provided.

6. A method according to any one of the preceding claims, wherein: The weight ratio of the fluoride-containing lithium source to the fluoride-free lithium source is in the range of 1:1 to 1:

20.

7. A method according to any one of the preceding claims, wherein: The mixing step (c) is carried out in at least two sub-steps. (c1) mixing a fluoride-containing lithium source with a fluoride-free lithium source and optionally a hydrocarbon, (c2) mixing the mixture obtained in step (c1) with sources of the phosphate and transition metal.

8. A method according to any one of the preceding claims, wherein: Step (a1), (a2), (a3) ​​or (a4) is combined with step (d), which is carried out at a temperature in the range of 20°C to 150°C.

9. A method according to any one of the preceding claims, wherein: The lithium source in which the fluoride is uniformly dispersed is obtained by a method of recycling waste batteries.

10. A method according to any one of the preceding claims, wherein: The fluoride is lithium fluoride.

11. A method according to any one of the preceding claims, wherein: In the lithium source provided in step (b), individual crystals or agglomerates of fluoride may not be detected by particle size distribution and X-ray diffraction and SEM / EDX.

12. A LiFe (1-x) M 1 x (PO4) 1-y F 3yThe particulate cathode active material has an average particle size (D50) in the range of 1 to 16 μm, wherein M 1 Selected from Ni, V, Ti, Co, Y, Al, Mg, Cu, Zn and Mn, and wherein x is in the range of 0 to 0.45, and wherein y is in the range of 0.0002 to 0.03, and wherein F is uniformly distributed in this cathode active material and does not accumulate on the surface of the secondary particles of this cathode active material.

13. The particulate cathode active material according to claim 12, wherein x is 0.

14. The particulate cathode active material according to claim 12 or 132, additionally comprising carbon as a coating.

15. A cathode comprising (A) at least one particulate cathode active material according to any one of claims 12 to 14, (B) carbon in an electrically conductive form, (C) Adhesive material.

16. A battery comprising (1) at least one cathode according to claim 15, (2) at least one anode, and (3) At least one electrolyte.