Multifunctional vinyl aromatic copolymer
By adjusting the meta-substance ratio of divinyl aromatic compounds and adding alkyl styrene structural units, the problem of multiple pores and insufficient interlayer peel strength in the prepreg is solved, and the problem of multifunctional vinyl aromatic copolymers is achieved. Laminated plate with excellent dielectric characteristics and heat resistance.
Patent Information
- Application Number
- CN202380028494.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-28
- Filing Date
- 2023-03-22
- Publication Date
- 2024-11-12
AI Technical Summary
The existing multifunctional vinyl aromatic copolymers produce a large number of pores during the production of prepregs, the laminated plate has poor appearance and insufficient interlayer peel strength.
By adjusting the metastas ratio of divinyl aromatic compounds to more than 60 mol%, the molecular weight distribution of the multifunctional vinyl aromatic copolymer is controlled so that it contains almost no crosslinking structure, thereby reducing pore generation and improving interlayer peeling Strength, while increasing heat resistance by adding an appropriate amount of alkyl styrene structural unit.
Prepregs and laminated plates with excellent dielectric characteristics and heat resistance are achieved, with good appearance and high interlayer peel strength, while reducing dielectric loss tangent.
Smart Images

Figure BDA0005048783230000061 
Figure BDA0005048783230000062 
Figure BDA0005048783230000063
Abstract
Description
Technical Field
[0001] The present disclosure relates to, among other things, multifunctional vinyl aromatic copolymers. Background Art
[0002] In recent years, with the remarkable progress of information network technology or the expansion of services using information networks, electronic devices are required to achieve large-capacity information and high-speed processing speed. In order to cope with these requirements, for printed wiring boards mounted in electronic devices, low dielectric constant and low dielectric loss tangent are strongly required on the basis of the insulation reliability, heat resistance, rigidity, flame retardancy and other characteristics that have always been required. Therefore, for resin compositions that are the main insulating materials constituting printed wiring boards, further improvements in dielectric loss tangent have been studied in particular, and a scheme for using cured resins of vinyl compounds with various chemical structures has been proposed.
[0003] As such a curable resin, for example, Patent Document 1 discloses a soluble multifunctional vinyl aromatic copolymer obtained by polymerizing a divinyl aromatic compound and a monovinyl aromatic compound in the presence of a Lewis acid catalyst.
[0004] Patent Document 2 proposes a polyfunctional vinyl aromatic copolymer obtained by polymerizing a divinyl aromatic compound with not only a vinyl aromatic compound but also a cycloolefin compound.
[0005] Prior art literature
[0006] Patent Literature
[0007] Patent Document 1: International Publication No. 2017 / 115813
[0008] Patent Document 2: International Publication No. 2018 / 181842
[0009] Non-patent literature
[0010] Non-patent document 1: Akifumi Noujima, et al., "Gold Nanoparticle-CatalyzedEnvironmentally Benign Deoxygenation of Epoxides to Alkenes", Molecules, (2011), 16(10), pp.8209-8227
[0011] Non-patent document 2: Gerrit Wienhoefer, et al., "Selective Iron-catalyzedTransfer Hydrogenation of Terminal Alkynes", Chemical Communications (Cambridge, United Kingdom), (2012), 48(40), pp.4827-4829 Summary of the invention
[0012] Problems to be solved by the invention
[0013] However, the existing multifunctional vinyl aromatic copolymers described in Patent Documents 1 and 2 have excellent dielectric properties and heat resistance, but have the problem of generating a large number of pores during the preparation of prepregs, poor appearance of laminated boards, and poor interlayer peeling strength. Therefore, one of the objects of the present disclosure is to provide a multifunctional vinyl aromatic copolymer and a curable resin composition containing the multifunctional vinyl aromatic copolymer, which can provide a prepreg with excellent dielectric properties and heat resistance and few pores, and a laminated board with good appearance and high interlayer peeling strength.
[0014] Means for solving problems
[0015] Examples of embodiments of the present disclosure are listed in the following items [1] to
[20] . [1]
[0017] A multifunctional vinyl aromatic copolymer having structural units derived from a divinyl aromatic compound and structural units derived from a monovinyl aromatic compound, wherein the proportion of the meta-isomer of the divinyl aromatic compound is greater than 60 mol %, and the dispersity (Mw / Mn) of the molecular weight distribution of the multifunctional vinyl aromatic copolymer represented by the ratio of the weight average molecular weight to the number average molecular weight is greater than 1 and less than 2.5. [2]
[0019] The multifunctional vinyl aromatic copolymer as described in item 1, wherein the proportion of the meta-isomer of the divinyl aromatic compound is less than 100 mol%. [3]
[0021] The multifunctional vinyl aromatic copolymer according to item 2, wherein the ratio of the meta-form of the divinyl aromatic compound is 96 mol % or less. [4]
[0023] The multifunctional vinyl aromatic copolymer according to any one of items 1 to 3, wherein the number average molecular weight is 300 to 7,000. [5]
[0025] The multifunctional vinyl aromatic copolymer according to any one of items 1 to 4, wherein in the molecular weight distribution, the area value occupied by the component having a molecular weight of 10,000 or more is 60% or less of the whole. [6]
[0027] The multifunctional vinyl aromatic copolymer according to any one of items 1 to 5, wherein the molecular weight distribution is unimodal. [7]
[0029] The polyfunctional vinyl aromatic copolymer according to any one of items 1 to 6, comprising 1 mol% to 99 mol% of structural units derived from an alkylstyrene having an alkyl group having 3 to 20 carbon atoms, based on 100 mol% of the total of all structural units. [8]
[0031] The multifunctional vinyl aromatic copolymer according to item 7, wherein the alkylstyrene is an alkylstyrene having an alkyl group having 6 to 10 carbon atoms. [9]
[0033] The multifunctional vinyl aromatic copolymer as described in item 8, wherein the alkylstyrene is 4-n-octylstyrene.
[10]
[0035] A curable resin composition comprising:
[0036] The multifunctional vinyl aromatic copolymer according to any one of items 1 to 9; and
[0037] One or more selected from the group consisting of a curable reaction type compound, a curable reaction type resin, a thermoplastic resin and a radical polymerization initiator.
[11]
[0039] The curable resin composition according to item 10 comprises a curable reactive compound, wherein the curable reactive compound is a trialenyl isocyanurate and / or a trialenyl cyanurate.
[12]
[0041] The curable resin composition according to item 10 or 11, comprising a curable reactive resin, wherein the curable reactive resin is polyphenylene ether.
[13]
[0043] The curable resin composition according to any one of Items 10 to 12, further comprising a flame retardant and / or a filler.
[14]
[0045] A cured product obtained by curing the curable resin composition according to any one of items 10 to 13.
[15]
[0047] A curable composite material comprising the curable resin composition according to any one of items 10 to 13 and a substrate, wherein the substrate constitutes 1% to 99% by mass based on the total mass of the curable composite material.
[16]
[0049] A cured composite material obtained by curing the curable composite material according to item 15.
[17]
[0051] A laminate comprising a plurality of layers of the cured composite material according to item 16.
[18]
[0053] A metal-clad laminate comprising a layer of the curable composite material according to item 15 and a metal foil layer.
[19]
[0055] A metal foil with resin, comprising:
[0056] Metal foil, and
[0057] A film obtained by curing the curable resin composition according to any one of items 10 to 13 on one surface of the metal foil.
[20]
[0059] A resin composition varnish comprising:
[0060] Organic solvents, and
[0061] The curable resin composition according to any one of items 10 to 13 dissolved in the organic solvent.
[0062] Effects of the Invention
[0063] According to the present disclosure, a multifunctional vinyl aromatic copolymer and a curable resin composition containing the multifunctional vinyl aromatic copolymer can be provided, which can provide a prepreg with excellent dielectric properties and heat resistance and few voids, and a laminate with good appearance and high interlayer peel strength. DETAILED DESCRIPTION
[0064] The specific embodiment of the present invention (hereinafter referred to as "the present embodiment") is described below. The following embodiment is one mode of the present invention, and therefore the present invention is not limited to the following embodiment. Therefore, the following embodiment can be implemented by appropriately deforming within the scope of the gist of the present invention. In addition, unless otherwise stated, "to" in the present disclosure refers to the numerical values including both ends as the upper limit and the lower limit. In the present disclosure, the upper limit and the lower limit of the numerical range can be arbitrarily combined.
[0065] [Multifunctional vinyl aromatic copolymer]
[0066] The multifunctional vinyl aromatic copolymer disclosed in the present invention has a structural unit (a) derived from a divinyl aromatic compound and a structural unit (b) derived from a monovinyl aromatic compound. Among the structural units (a) derived from the divinyl aromatic compound, more than 60 mol% are meta-forms. "Meta-forms" refer to structural units derived from divinyl aromatic compounds in which two vinyl groups are coordinated to each other at meta positions. In the multifunctional vinyl aromatic copolymer, the dispersity (Mw / Mn) of the molecular weight distribution represented by the ratio of the weight average molecular weight (Mw) to the number average molecular weight (Mn) is less than 2.5.
[0067] Although not limited by theory, it is believed that the molecular weight distribution of existing multifunctional vinyl aromatic copolymers is broad and multimodal in the high molecular weight region, that is, it contains a large amount of high molecular weight components formed by crosslinking during polymerization. The high molecular weight components formed by crosslinking during polymerization are difficult to dissolve in the varnish solvent, so the undissolved high molecular weight components will become the main cause of pores. In contrast, in the soluble multifunctional vinyl aromatic copolymer disclosed in the present invention, by making the ratio of the meta-body of the structural unit (a) derived from the above-mentioned divinyl aromatic compound to be 60 mol% or more, the side reaction of the growing end reacting with the vinyl of the structural unit (a) derived from the divinyl aromatic compound during polymerization to form a crosslinked structure is suppressed, and a multifunctional vinyl copolymer with a narrow molecular weight distribution without a crosslinked structure can be obtained. Since the obtained multifunctional vinyl copolymer contains almost no crosslinking structure, the amount of pores generated during the production of prepregs is reduced, and when a laminate is produced, the appearance and interlayer peeling strength are improved. In addition, by making the proportion of the meta-body in the structural unit (a) from the divinyl aromatic compound be 60 mol% or more, one vinyl group of the divinyl aromatic compound will not be used for crosslinking during polymerization and can remain until curing. As a result, when the amount of free radical polymerization initiator added is the same, three-dimensional crosslinking will be carried out during curing, so the glass transition temperature is improved and the solder heat resistance is improved. In addition, since the vinyl group remains until curing, the amount of free radical polymerization initiator added can be reduced, thereby reducing the dielectric loss tangent. Therefore, it can be considered that the multifunctional vinyl aromatic copolymer disclosed in the present invention can provide a prepreg with excellent dielectric properties and heat resistance and few pores, as well as a laminate with good appearance and high interlayer peeling strength.
[0068] The structure of the structural unit (a) is not particularly limited as long as it is a structure derived from a divinyl aromatic compound, but preferably includes a structure represented by the following chemical formula (1).
[0069] [Chemistry 1]
[0070]
[0071] (In the formula, R1 represents an aromatic hydrocarbon group having 6 to 30 carbon atoms, and n represents an integer greater than 1.)
[0072] The structure of the structural unit (a) may include a structure in which both of the two vinyl groups derived from the divinyl aromatic compound react, for example, a structure represented by the following chemical formula (1′).
[0073] [Chemistry 2]
[0074]
[0075] (In the formula, R1 represents an aromatic hydrocarbon group having 6 to 30 carbon atoms, and n represents an integer greater than 1.)
[0076] In the general formulae (1) and (1'), R1 is preferably independently a divalent aromatic hydrocarbon group having 6 to 30 carbon atoms, such as phenylene, naphthylene, divalent biphenylene, structural isomers thereof, and combinations thereof, and preferably phenylene from the viewpoint of solubility. n is independently an integer greater than 1, and the upper limit of n is not limited, and may be, for example, 100 or less.
[0077] The structure of the structural unit (b) is not particularly limited as long as it is derived from a monovinyl aromatic compound (but excluding substances corresponding to the "alkylstyrene having an alkyl group having 3 to 20 carbon atoms" of the structural unit (c)), but preferably includes a structure represented by the following chemical formula (2).
[0078] [Chemistry 3]
[0079]
[0080] (In the formula, R2 represents an aromatic hydrocarbon group having 6 to 30 carbon atoms, and n represents an integer greater than 1.)
[0081] In the general formula (2), R2 preferably includes a monovalent aromatic hydrocarbon group having 6 to 30 carbon atoms, such as phenyl, naphthyl, monovalent biphenyl, their structural isomers and combinations thereof, and phenyl is preferred from the perspective of solubility. n is an integer greater than 1, and the upper limit of n is not limited, for example, it can be less than 100. In the multifunctional vinyl aromatic copolymer, the structural units (a) and the structural units (b) can be arranged in an alternating, random, block or grafted manner, or in a combination thereof.
[0082] In the multifunctional vinyl aromatic copolymer disclosed in the present invention, relative to the total of 100 mol% of all structural units, it is preferred to contain 1 mol% to 99 mol% of structural units (c) derived from alkylstyrene having an alkyl group with 3 to 20 carbon atoms. The alkyl group with 3 to 20 carbon atoms may be a linear or branched alkyl group, preferably a linear alkyl group. From the perspective of both improving heat resistance and strength and easiness of handling, the number of carbon atoms is preferably 6 to 10, and more preferably 6 to 8. As the alkyl group, more specifically, propyl, butyl, pentyl, hexyl, heptyl, octyl, nonyl, decyl and their structural isomers can be cited. From the perspective of ease of acquisition, 4-n-octylstyrene having 8 carbon atoms is particularly preferred. By having structural units derived from these alkylstyrenes, the multifunctional vinyl aromatic copolymer can provide laminated plates having higher heat resistance and strength.
[0083] The content of the structural unit derived from alkylstyrene is preferably 1 mol% to 99 mol%, more preferably 5 mol% to 99 mol%, and further preferably 10 mol% to 99 mol%, relative to 100 mol% of the total of all structural units. The polyfunctional vinyl aromatic copolymer can provide a laminate having higher heat resistance and strength by having the structural unit derived from alkylstyrene in such a content range.
[0084] The vinyl group of the structural unit (a) derived from the divinyl aromatic compound functions as a crosslinking component and contributes to improving the heat resistance of the multifunctional vinyl aromatic copolymer. On the other hand, the structural unit derived from the monovinyl aromatic compound (b) does not have a vinyl group and therefore does not function as a crosslinking component, but helps to improve the compatibility with curable resins such as modified PPE, improve the solubility in varnish solvents, and improve the moldability of prepregs and laminates.
[0085] In the structural unit (a) derived from a divinyl aromatic compound, "meta-isomer" refers to a structural unit derived from a divinyl aromatic compound in which two vinyl groups are in meta position (meta position) relative to each other. That is, in the general formula (1), it refers to a structural isomer in which the bond of the R1 group to the main chain and the vinyl groups are in meta position relative to each other, and in the general formula (1'), it refers to a structural isomer in which the bond of the R1 group to the main chain and the ethylene group derived from the vinyl groups are in meta position relative to each other. In the structural unit (a), the proportion of the structural isomer of the meta-isomer (hereinafter referred to as the meta-isomer ratio) is 60 mol% or more, i.e., 60 mol% or more and 100 mol% or less, preferably 65 mol% or more and 100 mol% or less, and more preferably 70 mol% or more and 100 mol% or less. This can further improve the dielectric properties, heat resistance, appearance and interlayer peeling strength. It should be noted that the vicinity of the structural unit from the divinyl aromatic is in an environment surrounded by aromatic rings, but when the meta-body ratio is 100mol%, there will be double bonds only near the main chain, and the reactivity during solidification tends to decrease compared with the double bonds from the para-body. Therefore, by including a small amount of double bonds from the para-body as the reaction starting point, there is a tendency of good reactivity, and dielectric properties, appearance and interlayer peeling strength, and solder heat resistance can be taken into account, so the meta-body ratio is preferably less than 100mol%, more preferably less than 99mol%, and more preferably less than 96mol%. In this case, the meta-body ratio is, for example, more than 60mol% and less than 100mol%, preferably more than 65mol% and less than 99%, more preferably more than 70mol% and less than 96mol%. The meta-body ratio in the structural unit (a) from the divinyl aromatic compound is caused by the ratio of the meta-body contained in the divinyl aromatic compound used as a monomer during polymerization. That is, in order to synthesize a multifunctional vinyl copolymer having a structural unit (a) derived from a divinyl aromatic compound with the above-mentioned meta-isomer ratio, a monomer of a divinyl aromatic compound having an meta-isomer ratio of preferably 60 mol% to 100 mol%, more preferably 65 mol% to 100 mol%, further preferably 70 mol% to 100 mol%, or preferably 60 mol% to less than 100 mol%, more preferably 65 mol% to 99 mol%, further preferably 70 mol% to 96 mol%.
[0086] The structural unit (a) from the divinyl aromatic compound can be a structure in which only one vinyl group represented by the general formula (1) reacts, a structure in which two vinyl groups represented by the general formula (1') react, and the like. Among these, the amount of the repeating unit in which only one vinyl group represented by the general formula (1) reacts is preferably 1 mol% to 95 mol%, more preferably 5 mol% to 50 mol%, further preferably 5 mol% to 40 mol%, and further preferably 5 mol% to 35 mol% relative to the sum of the structural units (a), (b) and (c). By making the amount of the repeating unit within this range, the side reaction in which the growing end reacts with the vinyl group of the structural unit (a) from the divinyl aromatic compound to form a crosslinked structure during polymerization is suppressed, and a multifunctional vinyl copolymer with a small number of crosslinked structures and a narrow molecular weight distribution can be obtained. In addition, the vinyl group remaining without being used for crosslinking during curing can be reduced, so that the dielectric loss tangent can be further reduced.
[0087] The amount of the structural unit (b) derived from the monovinyl aromatic compound is preferably 5 mol% to 99 mol%, more preferably 50 mol% to 95 mol%, further preferably 60 mol% to 95 mol%, and further preferably 65 mol% to 95 mol%, relative to the total amount of the structural units (a), (b) and (c). By making the amount of the unit within this range, a multifunctional vinyl aromatic copolymer having excellent compatibility with a curable resin such as modified PPE, solubility in a varnish solvent, and moldability of a prepreg or a laminate can be formed.
[0088] The structural unit (a) from the divinyl aromatic compound and the structural unit (b) from the monovinyl aromatic compound may contain one kind each, or may contain a combination of more than two kinds. As an example of a divinyl aromatic compound, as long as it is an aromatic having two vinyl groups, it is not limited. Preferably, divinylbenzene, divinylnaphthalene, divinylbiphenyl, their structural isomers, and their mixtures are used. From the aspect of solubility, divinylbenzene is more preferred. As an example of a monovinyl aromatic compound, as long as it is an aromatic having one vinyl group, it is not limited. For example, vinyl aromatic compounds such as styrene, vinylnaphthalene, and vinylbiphenyl can be cited; alkyl-substituted vinyl aromatic compounds such as o-methylstyrene, m-methylstyrene, p-methylstyrene, o-, p-dimethylstyrene, o-ethylvinylbenzene, m-ethylvinylbenzene, and p-ethylvinylbenzene are mentioned. In order to prevent the gelation of the multifunctional vinyl aromatic copolymer; the effect of improving solvent solubility and processability is increased; the cost is low; and the reason for easy acquisition, styrene and ethylvinylbenzene (including each positional isomer or a mixture thereof) are preferred. The monovinyl aromatic compound may not contain styrene.
[0089] The polyfunctional vinyl aromatic copolymer may have structural units derived from other monomer components such as trivinyl aromatic compounds, trivinyl aliphatic compounds, divinyl aliphatic compounds, monovinyl aliphatic compounds, etc., in addition to structural units derived from divinyl aromatic compounds and monovinyl aromatic compounds, within the range not impairing the effects of the present disclosure.
[0090] The number average molecular weight (Mn: the number average molecular weight measured by gel permeation chromatography in terms of standard polystyrene) of the multifunctional vinyl aromatic copolymer is preferably 300 to 7,000, more preferably 350 to 6,000, and further preferably 400 to 4,000. By making Mn 300 or more, there is a tendency that the molecular weight is sufficiently high and the strength of the cured product can be improved, and by making Mn 7,000 or less, there is a tendency that the molding processability can be improved. In addition, the dispersion degree (Mw / Mn) of the molecular weight distribution represented by the ratio of the weight average molecular weight (Mw: the weight average molecular weight measured by gel permeation chromatography in terms of standard polystyrene) to Mn is 3.0 or less, preferably 2.5 or less, and more preferably 1 to 2.3. If Mw / Mn is greater than 2.5, there is a tendency that the molecular weight distribution shows multimodality of two or more peaks, and the molecular weight distribution becomes broad on the high molecular weight side. This indicates the generation of crosslinking and insoluble components in the polymerization, and thus there is a tendency to produce pores in the prepreg and significantly reduce the peel strength of the laminate. In addition, since the two vinyl groups of the divinyl aromatic compound are used in the polymerization, the content of the vinyl group to be used during curing is reduced, and the glass transition temperature after curing tends to decrease. Among these preferred molecular weights and molecular weight distributions, there is a tendency to contain almost no metamers of the general formula (1') in which both vinyl groups have reacted. In this case, in the determination of the metamer ratio, the amount of the metamer of the general formula (1') can be ignored as a numerical value compared to the amount of the metamer of the general formula (1). By making the metamer ratio and the dispersity values of the multifunctional vinyl aromatic copolymer within the above-mentioned specific range, there is a tendency to exert a synergistic effect, especially from the aspects of heat resistance and interlayer peel strength. As the reason, although not limited to theory, the present disclosure discloses that the curing reactivity of the double bonds of the inter-phase body is mild. Therefore, by making the ratio of the inter-phase body more than 60%, when manufacturing a metal-clad laminate or a metal foil with a resin, the resin layer has appropriate reactivity during curing, and the rate of increase in the viscosity of the resin layer can be slowed down. And by making Mw / Mn more than 1 and less than 2.5, the rate of increase in the viscosity of the resin layer can be further slowed down. Through the synergistic effect of the two, the resin penetrates into the interior of the roughened surface of the copper foil while having moderate fluidity until the middle stage of the curing reaction, and has a tendency to cure uniformly. In addition, it can be considered that since the curing ends after the penetration, the anchoring effect is improved, resulting in good heat resistance and improved interlayer peeling strength.
[0091] The molecular weight distribution more preferably shows a unimodal differential molecular weight distribution. In addition, in the integrated molecular weight distribution, the polymer with a molecular weight of 10,000 or more preferably accounts for less than 60% of the whole. The unimodal molecular weight distribution and the polymer with a molecular weight of 10,000 or more within the above range mean that high molecular weight components cross-linked during polymerization are hardly included, solubility in varnish solvents is improved, and a prepreg with few pores and a laminate with good appearance and high interlayer peeling strength can be provided.
[0092] [Method for producing polyfunctional vinyl aromatic copolymer]
[0093] The method for producing the soluble multifunctional vinyl aromatic copolymer disclosed in the present invention can include a method for producing the multifunctional vinyl aromatic copolymer by polymerizing monomers such as divinyl aromatic compounds and monovinyl aromatic compounds in the presence of a catalyst and a catalyst promoter. In more detail, the following method is preferred: relative to the total amount of monomers, 1 mol% or more and less than 95 mol% of divinyl aromatic compounds and 5 mol% or more and less than 99 mol% of monovinyl aromatic compounds are used, and the polymerization is carried out at a temperature of -78°C to 120°C. Here, as a catalyst, a Lewis acid catalyst can be preferably used, and as an added base of a catalyst promoter, a Lewis base compound can be preferably used. In addition, with regard to the apparatus used in the polymerization, it is preferred to use an apparatus that is dried at 200°C for more than 2 hours immediately before use, and immediately cooled in a nitrogen atmosphere after being taken out from a dryer, etc., to remove moisture from the surface.
[0094] As a catalyst, an initiator commonly used in cationic polymerization and living cationic polymerization is selected. From the perspective of ease of polymerization control, a Lewis acid catalyst is preferably selected. A Lewis acid catalyst is a compound composed of a metal ion (acid) and a ligand (base), and can be used without particular restrictions as long as it can accept an electron pair. Among them, from the perspective of the heat decomposition resistance of the obtained multifunctional vinyl aromatic copolymer, a metal fluoride or its complex is preferred, and a 2-6 valent metal fluoride or its complex of B, Al, Ga, In, Si, Ge, Sn, Pb, Sb, Bi, Ti, W, Zn, Fe and V is particularly preferred. These catalysts can be used alone or in combination of two or more. From the perspective of the molecular weight and molecular weight distribution control of the obtained multifunctional vinyl aromatic copolymer and the polymerization activity, it is most preferred to use an ether complex of boron trifluoride. Here, as the ether of the ether complex, there are diethyl ether, dimethyl ether, dibutyl ether, etc. For reasons of easy availability and low cost, boron trifluoride diethyl ether complex is particularly preferred.
[0095] The catalyst can be used in a range of 0.0001 to 10 molar ratios relative to the total amount of monomers, more preferably 0.001 to 1, and further preferably 0.001 to 0.1. If the molar ratio is 10 or less, the polymerization rate will not become too large, and polymerization control such as molecular weight distribution becomes easy. In addition, when the molar ratio is 0.0001 or more, sufficient polymerization rate can be ensured, the time spent on polymerization can be reduced, cost reduction can be achieved, and industrial implementation is beneficial.
[0096] In the manufacturing method of the multifunctional vinyl aromatic copolymer disclosed in the present invention, various reagents can be added as catalyst co-agents. For example, as an added base, one or more Lewis base compounds are used. As Lewis base compounds, monoester compounds, diester compounds, thioester compounds, thioether compounds, ketone compounds, ether compounds, and phosphine compounds can be cited. The Lewis base compound is selected appropriately according to the initiator (catalyst) used in the polymerization. For example, when a boron trifluoride diethyl ether complex is used as the catalyst, a monoester compound and a diester compound are preferably used. As a specific example, acetic acid esters such as butyl acetate, diesters such as dimethyl adipate, and diethyl malonate. One Lewis base compound can be used or two or more can be used in combination.
[0097] The Lewis base compound controls the interaction between the carbon cation as an active species and the counter anion by coordinating to the Lewis acid catalyst as a counter anion during the polymerization reaction, thereby adjusting the relative reaction frequency with the monomer that also acts as a chain transfer agent. Generally, by adding a Lewis base compound, the carbon cation terminal as an active species interacts with the Lewis base compound, thereby suppressing side reactions such as the carbon cation terminal acting on other molecular chains, and controlling the molecular weight distribution.
[0098] The Lewis base compound is preferably added at a molar ratio of 0.1 to 100, more preferably 1 to 100, and particularly preferably 5 to 50 relative to the amount of the catalyst. Within the above range, the polymerization rate can be appropriately maintained, the above-mentioned side reactions can be suppressed, and a polyfunctional vinyl aromatic copolymer having a unimodal molecular weight distribution can be obtained.
[0099] A solvent may be added as needed during the polymerization. As a solvent, a compound that does not hinder polymerization and is a substance that dissolves the catalyst, catalyst promoter, and monomer components to form a uniform solution. Specifically, from the perspective of the balance of polymerization activity and solubility, toluene, xylene, n-hexane, cyclohexane, methylcyclohexane or ethylcyclohexane, and acetonitrile are particularly preferred. In addition, regarding the amount of solvent used, considering the viscosity of the resulting polymerization solution or the ease of heat removal, it is preferably determined in a manner that the monomer components in the polymerization solution are 1vol% to 90vol%, preferably 1vol% to 80vol%, and particularly preferably 1vol% to 60vol%. If the concentration is 1vol% or more, sufficient polymerization efficiency can be ensured, resulting in cost reduction. If it is less than 90vol%, the molecular weight and molecular weight distribution of the generated multifunctional vinyl aromatic copolymer can be reduced, the pores of the prepreg can be suppressed, and the interlayer peeling strength and molding processability of the laminate can be improved.
[0100] When producing a multifunctional vinyl aromatic copolymer, it is necessary to polymerize the polymerization solution at a temperature of -78°C to 120°C. The polymerization temperature is selected according to the catalyst or solvent used, and is preferably -20°C to 120°C, more preferably 30°C to 120°C, and particularly preferably 40°C to 120°C for the sake of industrial feasibility. If the polymerization temperature is 120°C or less, the selectivity of the reaction is improved, thereby obtaining a narrower molecular weight distribution and suppressing the generation of gel. If it is -78°C or more, sufficient catalyst activity can be ensured and the polymerization efficiency can be improved.
[0101] The method for recovering the polyfunctional vinyl aromatic copolymer after the polymerization reaction is stopped is not particularly limited, and may be, for example, a commonly used method such as a heating concentration method, a steam stripping method, or precipitation using a poor solvent. From the perspective of being able to remove the compounds used for polymerization or recovery such as a catalyst, a catalyst promoter, and a solvent from the copolymer and reducing the residual amount, a method of precipitation using a poor solvent is preferably repeated two or more times.
[0102] [Curable resin composition]
[0103] The curable resin composition disclosed herein contains a multifunctional vinyl aromatic copolymer and contains at least one selected from the group consisting of a curable reactive compound, a curable reactive resin, a thermoplastic resin, and a free radical polymerization initiator. It may further contain an initiator such as a free radical polymerization initiator, a flame retardant, a silica filler, and a solvent as needed. The elements that can constitute the curable resin composition are described below.
[0104] In the present disclosure, "curable reaction type compound" refers to a low molecular weight compound that functions as a crosslinking agent when curing a curable resin composition, specifically, a compound having a molecular weight of less than 300. As a curable reaction type compound, isocyanuric acid trialenyl ester and / or cyanuric acid trialenyl ester (hereinafter referred to as "isocyanuric acid / cyanuric acid trialenyl ester") are liquid at room temperature, so they are preferred from the perspective of ease of handling. In order to further improve the compatibility of the multifunctional vinyl aromatic copolymer with any of the curable reaction resin and the thermoplastic resin, and to further improve the heat resistance and interlayer peeling strength of the laminate, as the isocyanuric acid trialenyl ester compound, isocyanuric acid triallyl ester (TAIC) and the like are more preferred, and as the cyanuric acid trialenyl ester compound, triallyl cyanurate (TAC) and the like are more preferred.
[0105] The amount of isocyanuric acid / trienyl cyanurate in the curable resin composition is preferably 2% to 20% by mass relative to the total weight of the components other than the solvent. From the perspective of compatibility with other components, or the reduction of dielectric loss tangent of a molded body of the resin composition, a prepreg containing the resin composition, a laminate of a plurality of prepregs, a laminate of a prepreg and a substrate, and a good appearance, the amount of isocyanuric acid / trienyl cyanurate is more preferably 2% to 15% by mass, and further preferably 3% to 10% by mass.
[0106] In addition to isocyanuric acid trialenyl ester / cyanurate, common crosslinking agents may be added to the curable reactive compound within a range that does not impair the properties. Examples thereof include polyfunctional methacrylate compounds having two or more methacryloyl groups in the molecule, polyfunctional acrylate compounds having two or more acryloyl groups in the molecule, polyfunctional vinyl compounds having two or more vinyl groups in the molecule such as polybutadiene, vinylbenzyl compounds such as divinylbenzene having a vinylbenzyl group in the molecule (excluding the one added as a copolymerizable monomer in the above-mentioned component (b)), and polyfunctional maleimide compounds having two or more maleimide groups in the molecule such as 4,4'-bismaleimidodiphenylmethane.
[0107] In the present disclosure, "curable reactive resin" refers to a polymer material other than a multifunctional vinyl aromatic copolymer that can function as a cross-linking agent when curing a curable resin composition, specifically, a compound with a molecular weight of 300 or more. As a curable reactive resin, polyphenylene ether (hereinafter referred to as "PPE") is preferred from the aspects of low dielectric properties and heat resistance. PPE contains phenylene ether units as repeating structural units. The phenylene group in the phenylene ether unit may or may not have a substituent. In the present disclosure, PPE as a curable reactive resin includes dimers, trimers, oligomers and polymers. The curable reactive resin can be mixed as the main material of the curable resin composition, thereby obtaining a cured product with excellent strength. "Mixing as the main material" means that it occupies the largest mass % among the components contained in the curable resin composition.
[0108] PPE may also contain other structural units in addition to the phenylene ether unit. The amount of other structural units relative to the number of all unit structures is typically 30 mol% or less, 25 mol% or less, 20 mol% or less, 15 mol% or less, 10 mol% or less, or 5 mol% or less. However, as long as it does not hinder the effects of the present disclosure, the amount of other structural units relative to the number of all unit structures may exceed 30 mol%.
[0109] Specific examples of PPE include poly(2,6-dimethyl-1,4-phenylene ether), poly(2-methyl-6-ethyl-1,4-phenylene ether), poly(2-methyl-6-phenyl-1,4-phenylene ether), poly(2,6-dichloro-1,4-phenylene ether), copolymers of 2,6-dimethylphenol and other phenols (e.g., 2,3,6-trimethylphenol, 2-methyl-6-butylphenol, etc.), PPE copolymers obtained by coupling 2,6-dimethylphenol with biphenols or bisphenols, and PPE having a linear or branched structure obtained by heating poly(2,6-dimethyl-1,4-phenylene ether) in the presence of a phenolic compound such as bisphenols or triphenols and a radical polymerization initiator in a toluene solvent to perform a redistribution reaction. Further examples include PPE in which the terminal hydroxyl groups of these PPEs are substituted with functional groups containing carbon-carbon double bonds. Specific examples of the functional group having a carbon-carbon double bond include vinyl, allyl, isopropenyl, 1-butenyl, 1-pentenyl, p-vinylphenyl, p-isopropenylphenyl, m-vinylphenyl, m-isopropenylphenyl, o-vinylphenyl, o-isopropenylphenyl, p-vinylbenzyl, p-isopropenylbenzyl, m-vinylbenzyl, m-isopropenylbenzyl, o-vinylbenzyl, o-isopropenylbenzyl, p-vinylphenylvinyl, p-vinylphenylpropenyl, p-vinylphenylbutenyl, m-vinylphenylvinyl, m-vinylphenylpropenyl, m-vinylphenylbutenyl, o-vinylphenylvinyl, o-vinylphenylpropenyl, o-vinylphenylbutenyl, methacryloyl, acryloyl, 2-ethylacryloyl, and 2-hydroxymethylacryloyl.
[0110] The number average molecular weight of PPE is preferably 1,000 to 5,000. By making the resin composition contain such a low molecular weight PPE, the viscosity increase of the resin composition varnish can be suppressed, so that the coating property of the resin composition varnish on the substrate can be improved. By achieving the improvement of the coating property, it is also possible to achieve the improvement of various properties required for the resin composition or its cured product. The number average molecular weight of the low molecular weight PPE is preferably 1,000 to 4,000, or 1,500 to 3,000.
[0111] The PPE contained in the curable reaction type resin may be one kind or a combination of two or more kinds of PPE having a number average molecular weight of 1,000 to 5,000.
[0112] The amount of PPE in the curable resin composition is 50% to 90% by weight relative to the total weight of the components other than the solvent. From the perspective of compatibility with other components, or the reduction of dielectric loss tangent of a cured product of the curable resin composition, a prepreg, a laminate of a plurality of prepregs, a laminate of a prepreg and a substrate, and a good appearance, the amount of PPE is preferably 50% to 80% by weight, more preferably 50% to 70% by weight.
[0113] Examples of the radical polymerization initiator include peroxides such as benzoyl peroxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, di-tert-butyl peroxide, tert-butylcumyl peroxide, di(2-tert-butylperoxyisopropyl)benzene, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, dicumyl peroxide, di-tert-butyl peroxyisophthalate, tert-butyl peroxybenzoate, 2,2-bis(tert-butylperoxy)butane, 2,2-bis(tert-butylperoxy)octane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, bis(trimethylsilyl)peroxide, and trimethylsilyltriphenylsilyl peroxide. It should be noted that free radical initiators such as 2,3-dimethyl-2,3-diphenylbutane can also be used as reaction initiators for resin compositions. Among them, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexyne-3, di(2-tert-butylperoxyisopropyl)benzene and 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane are preferred from the perspective of being able to provide a cured product having excellent heat resistance and mechanical properties and having a low dielectric constant and a low dielectric loss tangent.
[0114] The 1-minute half-life temperature of the radical polymerization initiator is preferably 155°C to 185°C, or 160°C to 180°C, or 165°C to 175°C. In the present disclosure, the 1-minute half-life temperature is a temperature at which the radical polymerization initiator decomposes and the amount of active oxygen thereof becomes half in 1 minute. The 1-minute half-life temperature is a value confirmed by the following method, that is, the radical polymerization initiator is dissolved in a solvent inert to free radicals, such as benzene, so as to have a concentration of 0.05 mol / L to 0.1 mol / L, and the radical polymerization initiator solution is thermally decomposed under a nitrogen atmosphere.
[0115] By setting the 1-minute half-life temperature of the radical polymerization initiator to 155°C or higher, when the resin composition is subjected to heat and pressure molding, the reaction with the crosslinking agent can be started after the PPE is fully melted, so there is a tendency for excellent moldability. On the other hand, by setting the 1-minute half-life temperature of the radical polymerization initiator to 185°C or lower, the decomposition rate of the radical polymerization initiator under normal heat and pressure molding conditions (for example, a maximum reaching temperature of 200°C) can be sufficient, so the crosslinking reaction with the crosslinking agent can be effectively and slowly carried out, so that a cured product with good electrical properties (especially dielectric loss tangent) can be formed.
[0116] Examples of the radical polymerization initiator having a 1-minute half-life temperature in the range of 155° C. to 185° C. include tert-hexyl peroxyisopropyl monocarbonate (155.0° C.) (the term in parentheses is the 1-minute half-life temperature, the same below), tert-butyl peroxy-3,5,5-trimethylhexanoate (166.0° C.), tert-butyl peroxylaurate (159.4° C.), tert-butyl peroxyisopropyl monocarbonate (158.8° C.), tert-butyl peroxy-2-ethylhexyl monocarbonate (161.4° C.), tert-hexyl peroxybenzoate (160.3° C.), 2,5-dimethyl-2,5-di(benzoyl peroxy)hexanoate (161.4° C.), tert-butyl peroxy-2,5-di(benzoyl peroxy)hexanoate (162.0° C.), tert-butyl peroxy-3,5,5-trimethylhexanoate (166.0° C.), tert-butyl peroxylaurate (159.4° C.), tert-butyl peroxyisopropyl monocarbonate (158.8° C.), tert-butyl peroxy-2-ethylhexyl monocarbonate (161.4° C.), tert-hexyl peroxybenzoate (162.0° C.), tert-butyl peroxy-2,5-di(benzoyl peroxy)hexanoate (162.0° C.), tert-butyl peroxy-3,5,5-trimethylhexanoate (166.0° C.), tert-butyl peroxy-3,5,5-trimethylhexanoate (166.0° C.), tert-butyl peroxylaurate (159.4° C.), tert-butyl peroxy-2,5 The following samples were analyzed by X-ray diffraction analysis: 1) hexane (158.2°C), tert-butyl peroxyacetate (159.9°C), 2,2-di(tert-butylperoxy)butane (159.9°C), tert-butyl peroxybenzoate (166.8°C), n-butyl 4,4-di(tert-butylperoxy)valerate (172.5°C), di(2-tert-butylperoxyisopropyl)benzene (175.4°C), dicumyl peroxide (175.2°C), di-tert-hexyl peroxide (176.7°C), 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (179.8°C) and tert-butylcumyl peroxide (173.3°C), etc.
[0117] The content of the radical polymerization initiator is preferably 0.05% by mass or more, more preferably 0.1% by mass or more, further preferably 0.3% by mass or more, further preferably 0.5% by mass or more, based on 100% by mass of the total mass of the curable resin composition, from the viewpoint of improving the reaction rate, and is preferably 3% by mass or less, more preferably 2% by mass or less, further preferably 1% by mass or less, from the viewpoint of suppressing the dielectric constant and dielectric loss tangent of the obtained cured product to a low level.
[0118] The curable resin composition preferably contains a flame retardant. As flame retardants, for example, inorganic flame retardants such as antimony trioxide, aluminum hydroxide, magnesium hydroxide, and zinc borate; aromatic bromine compounds such as hexabromobenzene, decabromodiphenylethane, 4,4-dibromobiphenyl, and ethylenebistetrabromophthalimide; phosphorus-based flame retardants such as resorcinol bis-diphenyl phosphate and resorcinol bis (dimethylphenyl) phosphate, etc. These flame retardants can be used alone or in combination of two or more. Among these, the flame retardant is preferably decabromodiphenylethane from the perspective of having a low dielectric constant and a low dielectric loss tangent when the curable resin composition is cured.
[0119] The content of the flame retardant is not particularly limited, but is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and further preferably 15 parts by mass or more relative to a total of 100 parts by mass of the curable resin composition from the perspective of maintaining the flame retardancy of the UL standard 94V-0 grade. In addition, from the perspective of being able to maintain the dielectric constant and dielectric loss tangent of the obtained cured product at a low level, the content of the flame retardant is preferably 50 parts by mass or less, more preferably 45 parts by mass or less, and further preferably 40 parts by mass or less.
[0120] The curable resin composition may contain a filler. As a filler, a silica filler may be contained. As the silica filler, both natural silica and synthetic silica may be used, for example, fused silica, amorphous silica, AEROSIL and hollow silica may be mentioned. The content of the silica filler may be 10 to 100 parts by mass relative to 100 parts by mass of all components that can be used as a crosslinking agent. In addition, the silica filler may be a material whose surface has been surface treated using a silane coupling agent or the like.
[0121] The curable resin composition may further contain additives such as a heat stabilizer, an antioxidant, a UV absorber, a surfactant, and a lubricant in addition to the above-mentioned components.
[0122] [Resin composition varnish]
[0123] The resin composition varnish disclosed in the present invention contains an organic solvent and a curable resin composition disclosed in the present invention dissolved in the organic solvent. The resin composition varnish may have suitable fluidity when impregnated in glass cloth. In the manufacturing process of the prepreg, it is preferred to dry and remove the solvent using a hot air dryer or the like after impregnating the resin composition varnish in the glass cloth. The solid components in the resin composition varnish may be dissolved or dispersed in the varnish. Regarding the amount of solvent, it can be appropriately adjusted in such a way that the fluidity of the resin composition varnish is within a suitable range. For example, the amount of solvent in the resin composition varnish may be 20% to 80% by mass, or 30% to 70% by mass, or 40% to 60% by mass.
[0124] As the solvent, aromatic compounds such as toluene and xylene, methyl ethyl ketone, cyclopentanone, cyclohexanone, and chloroform are preferred from the viewpoint of solubility of the components in the resin composition. These solvents may be used alone or in combination of two or more.
[0125] From the perspective of ensuring suitable fluidity of the resin composition varnish even at room temperature, aromatic compounds such as toluene are preferred as solvents, for example, toluene-methyl ethyl ketone mixed solvents, toluene-cyclohexanone mixed solvents, and toluene-cyclopentanone mixed solvents are preferred. In addition, in the case of the resin composition of the present disclosure, even if it is a solvent of toluene alone, it can be appropriately dissolved in the solvent, and further, in order to make it excellent in the impregnation property into the substrate, a solvent of toluene alone is also preferred as a solvent.
[0126] [Uncured material]
[0127] (Curing composite material)
[0128] The curable composite material (also referred to as "prepreg") disclosed herein comprises a curable resin composition and a substrate, and the substrate constitutes 1% to 99% by mass based on the total mass of the curable composite material. As the substrate, glass cloth formed by E glass fiber, L glass fiber, S glass fiber, etc., and organic fiber cloth formed by aramid resin fiber, etc. can be cited. As a method for manufacturing a curable composite material, for example, a method of impregnating the substrate into the above-mentioned resin composition varnish disclosed herein and drying to remove the solvent can be cited.
[0129] (Metal-clad laminate)
[0130] The metal-clad laminate of the present invention has a layer of the curable composite material of the present invention (uncured) and a metal foil layer. The metal-clad laminate of the present invention can be manufactured by laminating the layer of the curable composite material of the present invention with the metal foil layer. The curable composite material combined with the metal foil can be one sheet or multiple sheets, and the metal foil can be stacked on one side or both sides of the curable composite material according to the application and processed into a metal-clad laminate.
[0131] [cured material]
[0132] According to the present disclosure, there is also provided a cured product obtained by curing the curable resin composition of the present disclosure. The cured product of the present disclosure has excellent dielectric properties and heat resistance, few pores, and good appearance.
[0133] (Curing composite materials)
[0134] Examples of the cured product include a cured composite material obtained by curing the curable composite material (prepreg) of the present disclosure. Curing can be performed by heating the resin composition at a curing temperature for a predetermined time.
[0135] (laminated body)
[0136] For a curable composite material (prepreg), a laminate (laminate) can be provided by laminating and curing a plurality of sheets. More specifically, a plurality of sheets of a curable composite material (prepreg) can be laminated and cured to provide a laminate having a plurality of layers of the cured composite material disclosed herein.
[0137] (Curing Metal-Clad Laminates)
[0138] The curable composite material (prepreg) can be laminated with other layers as needed and cured. More specifically, the layer of the curable composite material disclosed in the present invention is laminated with the metal foil layer and the obtained metal-clad laminate is cured, thereby providing a cured metal-clad laminate having a layer of the cured composite material disclosed in the present invention and a metal foil layer. Regarding the dielectric loss tangent of the cured metal-clad laminate, when measured at 10 GHz by the method described in the embodiment, it is preferably less than 0.0033, more preferably less than 0.0031. The cured metal-clad laminate preferably has a layer of a cured product (cured composite material) of a curable composite material (prepreg) and a metal foil layer that are laminated and closely fitted, and can be appropriately used as a material for electronic circuit substrates. As metal foil, for example, aluminum foil and copper foil can be cited, among which copper foil is preferred due to its low resistance. One of the particularly preferred uses of the cured metal-clad laminate is a printed wiring board. In the printed wiring board, it is preferred to remove at least a portion of the metal foil from the cured metal-clad laminate.
[0139] (Printed Wiring Board)
[0140] A printed wiring board is formed by removing a portion of the metal foil from a metal-clad laminate. The printed wiring board can be typically formed by a method of pressurized heating molding using the curable composite material (prepreg) disclosed above. The printed wiring board is manufactured from the curable composite material (prepreg) disclosed herein, thereby having excellent heat resistance and electrical properties (low dielectric constant and low dielectric loss tangent), thereby being able to suppress changes in electrical properties associated with environmental changes, and thus having excellent insulation reliability and mechanical properties.
[0141] (Metal foil with resin)
[0142] Another example of a cured product is a metal foil with resin. The metal foil with resin has a metal foil and a film formed by curing the curable resin composition of the present disclosure on at least one side or both sides of the metal foil. As the metal foil, for example, aluminum foil and copper foil can be cited, among which copper foil is preferred due to its low resistance. The film before curing can be overlapped with the metal foil and vacuum pressed to produce it.
[0143] Example
[0144] Examples of the present disclosure are given below, but the present disclosure is not limited to the examples.
[0145] [Method for synthesizing divinylbenzene]
[0146] The meta-type divinylbenzene was synthesized with reference to Non-Patent Document 1, and the para-type divinylbenzene was synthesized with reference to Non-Patent Document 2.
[0147] [Synthesis of multifunctional vinyl aromatic copolymers]
[0148] (Example 1)
[0149] 0.9 mol (111 g) of divinylbenzene having a structural isomer ratio of 60%, 7.7 mol of styrene (manufactured by Tokyo Chemical Industry Co., Ltd., 797 g), and 7.8 mol of n-propyl acetate (manufactured by Tokyo Chemical Industry Co., Ltd., 799 g) were placed in a 3 L flask, and 0.3 mol of a diethyl ether complex of boron trifluoride (manufactured by Tokyo Chemical Industry Co., Ltd.) was added at 70°C, and the mixture was reacted for 3 hours. After the reaction of the polymerization solution was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed 5 times with pure water, and reprecipitated twice with methanol (manufactured by Kanto Chemical Co., Ltd.) and propyl acetate, and then the solid was recovered by vacuum filtration, air-dried in a ventilation room overnight, and vacuum-dried at 80°C for 3 hours using a vacuum dryer. The obtained solid was weighed, and it was confirmed that 223 g of copolymer A was obtained.
[0150] The obtained copolymer A was subjected to GPC analysis, and the results showed that Mn was 3,800, Mw was 8200, and Mw / Mn was 2.2. 13 C-NMR and 1 The structural units of the copolymer A were calculated by H-NMR analysis as follows.
[0151] Structural unit (a) derived from a divinyl aromatic compound: 24 mol%
[0152] Structural unit (b) derived from a monovinyl aromatic compound: 76 mol%
[0153] Meta-form ratio in the structural unit (a) derived from the divinyl aromatic compound: 67 mol%
[0154] (Examples 2 to 8)
[0155] A copolymer was synthesized in the same manner as in Example 1 except that divinylbenzene having a different ratio of the meta-isomer was used as a monomer.
[0156] (Example 9)
[0157] 8.3 mol of n-propyl acetate (manufactured by Tokyo Chemical Industry Co., Ltd., 850 g), 7.2 mol of styrene (manufactured by Tokyo Chemical Industry Co., Ltd., 750 g), 0.9 mol of 4-n-octylstyrene (manufactured by Tokyo Chemical Industry Co., Ltd., 195 g), and 0.9 mol (111 g) of divinylbenzene having a structural isomer ratio of 60 mol% were placed in a 3 L flask. 0.3 mol of a diethyl ether complex of boron trifluoride (manufactured by Tokyo Chemical Industry Co., Ltd.) was added at 70° C. and reacted for 3 hours. In the preparation of the polymerization solution, a catalyst co-agent (n-propyl acetate), a monovinyl aromatic compound, an alkylstyrene, a divinyl aromatic compound, and a catalyst (diethyl ether complex of boron trifluoride) were mixed in this order. After the reaction of the polymerization solution was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed with pure water 5 times, and reprecipitated twice with methanol (manufactured by Kanto Chemical Co., Ltd.) and propyl acetate, and then the solid was recovered by vacuum filtration, air-dried overnight in a ventilation room, and vacuum-dried at 80° C. for 3 hours using a vacuum dryer. The obtained solid was weighed to confirm that 317 g of a copolymer was obtained.
[0158] GPC analysis of the obtained copolymer revealed Mn 3,800, Mw 8,400, and Mw / Mn 2.2. The structural unit of the copolymer was calculated as follows by GC analysis of the reaction solution.
[0159] Structural unit (a) derived from divinyl aromatic compound: 19 mol%
[0160] Structural unit (b) derived from a monovinyl aromatic compound: 72 mol%
[0161] Structural unit derived from alkylstyrene (c): 9 mol%
[0162] (Examples 10 to 14)
[0163] A copolymer was synthesized in the same manner as in Example 1 except that the monomer ratio of styrene, 4-n-octylstyrene and divinylbenzene was changed.
[0164] (Examples 15 to 21)
[0165] A copolymer was synthesized in the same manner as in Example 1 except that the type of 4-n-alkylstyrene used as a comonomer was different. 4-n-alkylstyrene synthesized by our company was used.
[0166] (Example 22)
[0167] A copolymer was synthesized in the same manner as in Example 9 except that the alkylstyrene used as the comonomer was tert-butylstyrene (manufactured by Tokyo Chemical Industry Co., Ltd.).
[0168] Tables 1 to 3 show the synthesis results of the examples and the evaluation results of the following evaluation methods.
[0169]
[0170]
[0171]
[0172] (Comparative Examples 1 to 7)
[0173] A copolymer was synthesized in the same manner as in Example 1 except that divinylbenzene having a different ratio of the meta-isomer was used as a monomer.
[0174] (Comparative Example 8)
[0175] A copolymer was synthesized in the same manner as in Comparative Example 2 except that the amount of the sodium bicarbonate aqueous solution added was increased, the ratio of the base to the catalyst was adjusted to that shown in Table 4, and the polymerization reaction time was adjusted to 1 hour.
[0176] Table 4 shows the synthesis results of the comparative examples and the evaluation results of the following evaluation methods.
[0177]
[0178] [Manufacture of curable resin composition]
[0179] The following materials were mixed to produce a curable resin composition.
[0180] (Curing Reactive Compound)
[0181] TAIC (Made by Mitsubishi Chemical Corporation, molecular weight: 249.7, number of unsaturated double bonds per molecule: 3)
[0182] (Curing Reactive Resin)
[0183] ·Terminal methacryloyl-modified PPE (product name "SA9000", manufactured by Sabic Innovative Plastics, Mn: 2756, number of terminal functional groups per molecule: 2)
[0184] (Free Radical Polymerization Initiator)
[0185] ·Bis(1-tert-butylperoxy-1-methylethyl)benzene (product name "Perbutyl P", manufactured by NOF Corporation)
[0186] [Preparation of resin composition varnish]
[0187] The curable reaction type resin, the multifunctional vinyl aromatic copolymer and the curable reaction type compound were weighed in a weight ratio of 50:40:10, and a free radical polymerization initiator was weighed in an amount of 1% by mass relative to the solid content and put into a container. A toluene / methyl ethyl ketone mixed solvent was added in a ratio of 50:50 and in a manner of 50% by mass of the solid content, and stirred for more than 5 hours to prepare a resin composition varnish.
[0188] [Preparation of prepreg]
[0189] The low dielectric constant glass cloth L2116 (weight 94g / m 2 , thickness 91 μm, width 50 mm) was impregnated with a resin composition varnish, scraped off using a slit, and dried at 120° C. for 60 minutes to prepare a prepreg.
[0190] [Production of Laminated Body]
[0191] Eight prepregs were stacked and heated from room temperature at a rate of 3°C / min while being pressurized at 5 kg / cm 2 After reaching 130°C, the temperature was raised at a rate of 3°C / min and the pressure was 40kg / cm 2 After that, the temperature reached 200°C and the pressure was 40 kg / cm 2 The laminate was produced by vacuum pressing under the conditions of 60 minutes.
[0192] [Evaluation method]
[0193] (Analysis method for the ratio of meta-form in the structural unit derived from the divinyl aromatic compound of the multifunctional vinyl aromatic copolymer)
[0194] Using a nuclear magnetic resonance spectrometer manufactured by JEOL (model name: JNM-ECZ500R / S1), 13 The measurement was performed by C-NMR analysis. Chloroform-d1 was used as the solvent, and the resonance line of tetramethylsilane was used as the internal standard. The ratio of the area value of the peak at 125 ppm to the area values of the peaks at 113 ppm, 135 ppm, and 137 ppm was taken as the ratio of the meta-form in the structural unit derived from the divinyl aromatic compound.
[0195] (Analysis method for ratio of each structural unit of a polyfunctional vinyl aromatic copolymer)
[0196] Using a nuclear magnetic resonance spectrometer manufactured by JEOL (model name: JNM-ECZ500R / S1), 13 C-NMR and 1 H-NMR analysis was performed. Chloroform-d1 was used as a solvent, and the resonance line of tetramethylsilane was used as an internal standard. The ratio of the area value of the peaks at 5.2ppm and 5.7ppm to the area value of the peaks at 5.8ppm to 7.7ppm was taken as the ratio of the structural unit (a) derived from the divinyl aromatic compound, and the value obtained by subtracting the ratio of the structural unit (a) derived from the divinyl aromatic compound from 1 was taken as the ratio of the structural unit (b) derived from the monovinyl aromatic compound.
[0197] (Measurement method of molecular weight distribution)
[0198] The number average molecular weight (Mn) of the styrene elastomer was determined by comparing the elution time with that of a standard polystyrene with a known molecular weight using gel permeation chromatography (GPC). Specifically, a measurement sample having a sample concentration of 1.0 mass % (solvent: chloroform) was prepared, and the measurement was performed using HLC-8320GPC (manufactured by Tosoh Corporation) as the measurement device under the following conditions.
[0199] Column: 3 Shodex K-806L connected in series
[0200] Eluent: Chloroform
[0201] Injection volume: 100 μL
[0202] Flow rate: 1.0mL / min
[0203] Column temperature: 40°C
[0204] Detector: RI
[0205] (Evaluation method of voids in prepreg)
[0206] Three sample pieces of 10 mm long and 10 mm wide were cut from the prepreg, and after grinding the cross-section, the presence of voids was observed using an optical microscope with a 50x lens so that the upper and lower surfaces fell within the field of view. The same operation was performed at three locations for each sample, for a total of nine locations, and the degree of void generation was evaluated according to the following evaluation criteria.
[0207] A: 0 pores
[0208] B: more than 1 pore and less than 5 pores
[0209] C: More than 5 pores
[0210] (Method for measuring interlayer peel strength)
[0211] Two prepreg sheets were stacked, and copper foil (thickness 12 μm, surface roughness Rz 2.0 μm, FV-WS foil, manufactured by Furukawa Electric Co., Ltd.) was stacked on top of each other. The prepreg was heated at a temperature increase rate of 3°C / min from room temperature and at a pressure of 5 kg / cm 2 After reaching 130°C, the temperature was raised at a rate of 3°C / min and the pressure was 30kg / cm 2 After that, the temperature reached 200°C and the pressure was 30 kg / cm 2 The double-sided copper-clad laminate was made by vacuum pressing for 60 minutes under the conditions of . The test sample was cut into a size of 15 mm in width × 150 mm in length. The copper foil was peeled off at an angle of 90° and a speed of 50 mm / min relative to the laminate surface using Autograph (AG-5000D, manufactured by Shimadzu Corporation), and the average value of the load at this time was measured, and the average value of 5 measurements was obtained.
[0212] (Method for determining whether laminated boards have thin spots (white spots))
[0213] The appearance of the laminated board representing the resin-unimpregnated portion of the glass wiring bundle was visually evaluated for the presence of thin spots in the laminated board of 50 mm x 80 mm. Specifically, the laminated board was illuminated with a penlight at an angle of 30° and visually observed at an angle of 45° to confirm the presence of thin spots.
[0214] (Method for measuring dielectric loss tangent)
[0215] The dielectric loss tangent of the laminate at 10 GHz was measured by the cavity resonance method using a network analyzer (N5230A, manufactured by Agilent Technologies) and a cavity resonator (Cavity Resornator CP series) manufactured by Kanto Denshi Application Development Co., Ltd. as measurement devices.
[0216] (Measurement method of glass transition point)
[0217] The laminate was cut into a width of 3.0 mm and a length of 25 mm to produce a test piece used in the glass transition temperature (Tg) measurement. The obtained test piece was placed in a TMA (thermomechanical analysis device), heated to 220°C at a heating rate of 10°C / min under a nitrogen flow, and further heated at 220°C for 20 minutes to remove the residual molding strain. After the test piece was naturally cooled to room temperature, it was fixed to the chuck of the TMA measurement device, and scanned and measured from 30°C to 320°C at a heating rate of 10°C / min under a nitrogen flow, and Tg was obtained by the tangent method.
[0218] (Evaluation method of solder heat resistance)
[0219] The laminate was cut into pieces of 50 mm x 50 mm and placed in a 121°C saturated steam pressure autoclave for 10 hours. The laminate was taken out, the surface moisture was wiped off, and then immersed in a 288°C solder bath for 20 seconds. The expansion of the laminate after immersion was evaluated according to the following evaluation criteria.
[0220] AA: No expansion with a diameter of more than 2 mm
[0221] A: No expansion with a diameter of more than 3 mm occurred
[0222] B: 1 to 3 swellings with a diameter of 3 mm or more occur, and no swelling with a diameter of 5 mm or more occurs
[0223] C: Four or more swellings with a diameter of 3 mm or more occurred, or one or more swellings with a diameter of 5 mm or more occurred.
Claims
1. A multifunctional vinyl aromatic copolymer comprising structural units derived from a divinyl aromatic compound and structural units derived from a monovinyl aromatic compound, wherein: The meta-isomer ratio of the divinyl aromatic compound is 60 mol % or more, and the molecular weight distribution dispersity (Mw / Mn) of the multifunctional vinyl aromatic copolymer, represented by the ratio of weight average molecular weight to number average molecular weight, is 1 or more and 2.5 or less.
2. The multifunctional vinyl aromatic copolymer according to claim 1, wherein The ratio of the meta-isomer of the divinyl aromatic compound is less than 100 mol%.
3. The multifunctional vinyl aromatic copolymer according to claim 2, wherein The ratio of the meta-isomer of the divinyl aromatic compound is less than 96 mol%.
4. The multifunctional vinyl aromatic copolymer according to claim 1, wherein The number average molecular weight is 300 to 7,000.
5. The multifunctional vinyl aromatic copolymer according to claim 1, wherein In the molecular weight distribution, the area value occupied by components having a molecular weight of 10,000 or more accounts for 60% or less of the entire area.
6. The multifunctional vinyl aromatic copolymer according to claim 1, wherein The molecular weight distribution is unimodal.
7. The multifunctional vinyl aromatic copolymer according to claim 1, wherein The alkylstyrene-based structural units contain 1 mol% to 99 mol% of structural units derived from an alkylstyrene having an alkyl group having 3 to 20 carbon atoms, based on 100 mol% of the total of all structural units.
8. The multifunctional vinyl aromatic copolymer according to claim 7, wherein The alkylstyrene is an alkylstyrene having an alkyl group having 6 to 10 carbon atoms.
9. The multifunctional vinyl aromatic copolymer according to claim 8, wherein The alkylstyrene is 4-n-octylstyrene.
10. A curable resin composition comprising: The multifunctional vinyl aromatic copolymer according to any one of claims 1 to 9; and One or more selected from the group consisting of a curable reaction type compound, a curable reaction type resin, a thermoplastic resin, and a radical polymerization initiator. 11 . The curable resin composition according to claim 10 , comprising a curable reactive compound, wherein the curable reactive compound is a trialenyl isocyanurate and / or a trialenyl cyanurate. 12 . The curable resin composition according to claim 10 , comprising a curable reactive resin, wherein the curable reactive resin is polyphenylene ether. 13 . The curable resin composition according to claim 10 , further comprising a flame retardant and / or a filler. 14 . A cured product obtained by curing the curable resin composition according to claim 10 .
15. A curable composite material comprising the curable resin composition according to claim 10 and a substrate, wherein: The base material constitutes 1% to 99% by mass based on the total mass of the curable composite material. 16 . A cured composite material obtained by curing the curable composite material according to claim 15 .
17. A laminate comprising a plurality of layers of the cured composite material according to claim 16.
18. A metal-clad laminate comprising a layer of the curable composite material according to claim 15 and a metal foil layer.
19. A metal foil with resin, comprising: Metal foil, and A film formed by curing the curable resin composition according to claim 10 on one surface of the metal foil.
20. A resin composition varnish comprising: Organic solvents, and The curable resin composition according to claim 10 dissolved in the organic solvent.