Polyimide film and method for producing same
By controlling the heating thermal expansion coefficient in the polyimide film and using the imidation reaction of acid dianhydride and diamine, the problem of reducing the dimensional stability of the polyimide film in a humid environment is solved, and the humidity is achieved Polyimide film with excellent dimensional stability in gas environments is suitable for the manufacture of high-quality flexible metal foil laminated plates.
Patent Information
- Application Number
- CN202380030628.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Priority Date
- 2022-03-30
- Filing Date
- 2023-03-28
- Publication Date
- 2024-11-12
AI Technical Summary
The dimensional stability of the polyimide film decreases after exposure in a humid environment, affecting the quality of the flexible metal foil laminated plate.
By providing a polyimide film which is stored under 50% RH humidity for 48 hours, the thermal expansion coefficient of TD direction during the temperature increase of 25°C to 400°C is measured to be -1.5ppm/℃ or above using a thermomechanical analyzer. The imidation reaction is carried out by using acid dianhydride and diamine components below 6 ppm/°C to produce a polyamic acid solution and perform cast coating and imidation treatment to improve dimensional stability.
The polyimide film has excellent dimensional stability in a humid environment, ensuring the quality of flexible metal foil laminated plates, and is suitable for the manufacturing of a variety of electronic equipment.
Smart Images

Figure CN118946618A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to a polyimide film having excellent dimensional stability even after being exposed to moisture for a certain period of time, and a method for producing the same. Background Art
[0002] Polyimide (PI) is a polymer material based on a rigid aromatic main chain and an imide ring with excellent chemical stability. It has the highest level of heat resistance, chemical resistance, electrical insulation, chemical resistance, and weather resistance among organic materials.
[0003] Polyimide films have attracted attention as materials for various electronic devices that require the above-mentioned properties.
[0004] Examples of microelectronic components to which polyimide films are applied include thin circuit boards that are highly integrated and flexible in order to cope with the reduction in weight and size of electronic products. Polyimide films are particularly widely used as insulating films for thin circuit boards.
[0005] The above-mentioned thin circuit substrate generally has a structure in which a circuit including a metal foil is formed on an insulating film. In a broad sense, such a thin circuit substrate is called a flexible metal foil laminate (Flexible Metal Foil Clad Laminate). When a thin copper plate is used as the metal foil, it is also called a flexible copper foil laminate (Flexible Copper Clad Laminate; FCCL) in a narrow sense.
[0006] As methods for manufacturing flexible metal foil laminates, for example, there can be cited: (i) a casting method in which a polyamic acid, which is a precursor of polyimide, is cast or coated on a metal foil and then imidized; (ii) a metallization method in which a metal layer is directly provided on a polyimide film by sputtering; and (iii) a lamination method in which a polyimide film and a metal foil are bonded by thermoplastic polyimide using heat and pressure.
[0007] In particular, the metallization method is a method for producing a flexible metal foil laminate by sputtering a metal such as copper on a polyimide film having a thickness of 20 to 38 μm and then sequentially vapor-depositing a tie layer and a seed layer. This method is advantageous for forming ultra-fine circuits with a circuit pattern pitch of less than 35 μm and is widely used in the manufacture of flexible metal foil laminates for chip on film (COF).
[0008] The polyimide film actually used to manufacture the flexible metal foil laminate undergoes steps such as pre-manufacturing, transportation, and storage, during which it is placed in an environment with changes in humidity, temperature, and the like.
[0009] In particular, the problem of reduced dimensional stability of the polyimide film occurs when the polyimide film is exposed to moisture during the steps of transportation and storage, or during the process of using high temperature in the production step of the flexible metal foil laminate.
[0010] Therefore, there is an urgent need for a polyimide film that maintains dimensional stability even after being exposed to a certain environment (particularly moisture) during the steps of transportation and storage.
[0011] The matters described in the above background technology are used to help understand the background of the invention, and may include matters that are not known to those skilled in the art.
[0012] [Prior art literature]
[0013] [Patent Document]
[0014] (Patent Document 1) Korean Registered Patent No. 10-1258432 Summary of the invention
[0015] Technical issues
[0016] Therefore, an object of the present invention is to provide a polyimide film having excellent dimensional stability even after being exposed to moisture for a certain period of time.
[0017] However, the problems to be solved by the present invention are not limited to the problems mentioned above, and those skilled in the art should be able to clearly understand other problems not mentioned based on the following description.
[0018] Solution to the problem
[0019] In order to achieve the above-mentioned purpose, one aspect of the present invention provides a polyimide film, which after being stored under a humidity condition of 50% RH for 48 hours,
[0020] When the dimensional change during the temperature rise from 25°C to 400°C is measured by a thermomechanical analyzer (TMA), the temperature rise thermal expansion coefficient in the TD direction (50 to 200°C) is not less than -1.5 ppm / °C and not more than 6 ppm / °C.
[0021] The above-mentioned temperature-increasing thermal expansion coefficient (50-200° C.) is the slope of a straight line connecting the dimensional measurement value of the polyimide film in the TD direction measured at 200° C. during the first run (First Run) of the above-mentioned temperature-increasing process and the dimensional measurement value of the polyimide film in the TD direction measured at 50° C. during the first run (First Run) of the above-mentioned temperature-increasing process,
[0022] The dimensional measurement value in the TD direction corresponds to a dimensional change value calculated by converting the length of the sample of the polyimide film used in the measurement with the thermomechanical analyzer into 1 m.
[0023] Another aspect of the present invention provides a method for manufacturing a polyimide film, which as a method for manufacturing the above-mentioned polyimide film, includes: a process of providing a polyamic acid solution obtained from an acid dianhydride component and a diamine component; a process of casting the above-mentioned polyamic acid solution on a support and heating to manufacture a self-supporting film of the polyamic acid solution; and a process of imidizing and stretching the above-mentioned self-supporting film to manufacture a polyimide film.
[0024] Still another aspect of the present invention provides a flexible metal foil laminate comprising the polyimide film and a conductive metal foil.
[0025] Still another aspect of the present invention provides an electronic component including the flexible metal foil laminate.
[0026] Effects of the Invention
[0027] The present invention provides a polyimide film having excellent dimensional stability even after being exposed to moisture for a certain period of time, thereby providing a polyimide film having excellent dimensional stability even in a metal foil lamination process.
[0028] Such a polyimide film can be applied to various fields requiring a polyimide film with excellent dimensional stability, for example, a flexible metal foil laminate produced by a metallization method or an electronic component including such a flexible metal foil laminate. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 This is a graph showing the results of measuring the dimensional change of the polyimide film during the temperature increase from 25° C. to 400° C. using a thermomechanical analyzer (TMA) in Examples 1 and 4 of the present application.
[0030] Figure 2 This is a graph showing the results of measuring the dimensional change of the polyimide film during the temperature increase from 25° C. to 400° C. using a thermomechanical analyzer (TMA) in Comparative Examples 1 and 4 of the present application. DETAILED DESCRIPTION
[0031] The terms or words used in this specification and claims should not be interpreted limited to the usual meaning or dictionary meaning, but should only be interpreted based on the inventor's ability to appropriately define the concept of the term to explain the principle of his invention in the best way, and in accordance with the meaning and concept of the technical idea of the present invention.
[0032] Therefore, the embodiments described in this specification are merely the most preferred embodiments of the present invention and do not represent all technical concepts of the present invention. Therefore, it should be understood that when the present application is filed, there may be multiple equivalents and modifications that can replace these embodiments.
[0033] In this specification, unless the context clearly provides otherwise, expressions in the singular include expressions in the plural. In this specification, it should be understood that the terms "comprising", "having" or "having" are intended to specify the existence of a feature, number, step, constituent element or combination thereof of an implementation, and do not preclude the existence or additional possibility of one or more other features, numbers, steps, constituent elements or combinations thereof.
[0034] In this specification, "dianhydride" is intended to include precursors or derivatives thereof, which, although they may not technically be dianhydrides, will still react with diamines to form polyamic acids, which can again be converted into polyimides.
[0035] In this specification, "diamine" is intended to include precursors or derivatives thereof, which, although they may not technically be diamines, will still react with the dianhydride to form a polyamic acid which can again be converted into a polyimide.
[0036] In the present specification, when the amount, concentration or other value or parameter is given as a range, a preferred range or a preferred upper limit and a preferred lower limit, it should be understood that any pair of all ranges formed by any upper range limit or preferred value and any lower range limit or preferred value are specifically disclosed regardless of whether the range is disclosed separately.
[0037] Where numerical ranges are mentioned in this specification, unless otherwise stated, the ranges are intended to include the endpoints and all integers and fractions therein. The scope of the present invention is not intended to be limited to the specific values mentioned when defining a range.
[0038] When the dimensional change of the polyimide film in a heating process from 25°C to 400°C is measured by a thermomechanical analyzer (TMA) according to one embodiment of the present invention, the thermal expansion coefficient (50-200°C) can be greater than -1.5ppm / °C and less than 6ppm / °C, and the above-mentioned thermal expansion coefficient (50-200°C) can be the slope of a straight line connecting the dimensional measurement value of the polyimide film in the TD direction measured at 200°C during the first run (First Run) in the above-mentioned heating process and the dimensional measurement value of the polyimide film in the TD direction measured at 50°C during the first run (First Run) in the above-mentioned heating process.
[0039] The dimensional measurement value in the TD direction may correspond to a dimensional change value calculated by converting the length of the polyimide film sample used in the measurement with the thermomechanical analyzer into 1 m.
[0040] That is, the slope of the straight line connecting the dimensional measurement values of the polyimide film in the TD direction of the polyimide film measured at 200°C during the first run (First Run) in the above-mentioned heating process and the dimensional measurement values of the polyimide film in the TD direction measured at 50°C during the first run (First Run) in the heating process is greater than -1.5ppm / °C.
[0041] The polyimide film will expand in the MD direction (machine direction) and TD direction (traverse direction) during the heating process. In actual FCCL manufacturing, the pattern advances in the MD direction, while in the TD direction, the PI film and the Cu layer repeatedly form patterns. Therefore, the expansion and contraction in the TD direction, in particular, becomes an important factor in determining the quality of FCCL.
[0042] The slope of the straight line of the polyimide film of the present invention may be preferably 5.5 ppm / °C or less, and more preferably 5.0 ppm / °C or less.
[0043] A polyimide film having a slope of the straight line of -1.5 ppm / °C to 6 ppm / °C has excellent dimensional stability even after exposure to moisture for a certain period of time, and maintains dimensional stability even after lamination of a metal foil by coating, sputtering and / or evaporation.
[0044] A polyimide film having a slope of the straight line of less than -1.5 ppm / °C or greater than 6 ppm / °C has reduced dimensional stability after exposure to moisture for a certain period of time, and the quality of a flexible metal foil laminated board on which a metal foil is laminated by coating, sputtering and / or evaporation is significantly reduced.
[0045] Here, the measurement of dimensional change using the above-mentioned thermomechanical analyzer (TMA) is carried out under the following conditions.
[0046] Measurement mode: tensile mode, load 5g,
[0047] Sample length: 16mm (length in width direction),
[0048] Sample width: 4mm,
[0049] Heating starting temperature: 25℃,
[0050] Heating end temperature: 400℃ (no holding time at 400℃),
[0051] The polyimide film of the present invention may have a thermal expansion coefficient (CTE) in the TD direction of 1 ppm / °C to 10 ppm / °C.
[0052] In addition, the moisture absorption rate of the polyimide film may be 1.5 wt % or less.
[0053] On the other hand, the polyimide film of the present invention can be obtained by subjecting an acid dianhydride component and a diamine component to an imidization reaction, wherein:
[0054] The acid dianhydride component is selected from the group consisting of pyromellitic dianhydride (PMDA), oxydiphthalic dianhydride (ODPA), 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), 2,3,3',4'-biphenyltetracarboxylic dianhydride (a-BPDA), diphenyl sulfone-3,4,3',4'-tetracarboxylic dianhydride (DSDA), bis(3,4-dicarboxyphenyl)sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl) at least one of the group consisting of p-phenylenebis(trimellitic acid monoester anhydride), p-biphenylenebis(trimellitic acid monoester anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)phthalic acid dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic acid dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane dianhydride (BPADA), 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 1,4,5,8-naphthalenetetracarboxylic acid dianhydride and 4,4'-(2,2-hexafluoroisopropylidene)diphthalic acid dianhydride,
[0055] The diamine component is selected from p-phenylenediamine (PPD), m-phenylenediamine, 3,3'-dimethylbenzidine, 2,2'-dimethylbenzidine, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobenzoic acid (DABA), 4,4'-diaminodiphenyl ether (ODA), 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane (methylenediamine), 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, ,5,5'-tetramethyl-4,4'-diaminodiphenylmethane, bis(4-aminophenyl) sulfide, 4,4'-diaminobenzanilide, 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diamino-4,4'-dichlorobenzophenone, 3,3'-diamino-4 ,4'-dimethoxybenzophenone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-aminophenyl)propane, 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenoxy)benzene (TPE-R), 1,4-bis(3-aminophenoxy)benzene (TPE-Q), 1,3-bis(3-aminophenoxy)-4-trifluoromethylbenzene, 3,3'-diamino-4-(4-phenyl)phenoxybenzophenone, 3,3'-diamino-4,4'-di(4-phenylphenoxy)benzophenone, 1,3-bis(3-aminophenyl sulfide)benzene, 1,3-bis(4-aminophenyl sulfide)benzene, 1,4-bis(4-aminophenyl sulfide)benzene, 1,3-bis(3-aminophenyl sulfone)benzene, 1,3-bis(4-aminophenyl sulfone)benzene, 1,4-bis(4-aminophenyl sulfone)benzene, 1,3-bis[2-(4-aminophenyl)isopropyl]benzene, 1,4-Bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-bis[2-(4-aminophenyl)isopropyl]benzene, 3,3'-bis(3-aminophenoxy)biphenyl, 3,3'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[3-(3-aminophenoxy)phenyl]ether, bis[3-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether , bis[3-(3-aminophenoxy)phenyl]ketone, bis[3-(4-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]ketone, bis[3-(3-aminophenoxy)phenyl]sulfide, bis[3-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[3-(3-aminophenoxy)phenyl]sulfone, bis[3-(4-aminophenoxy)phenyl]sulfone, bis[3-(3-aminophenoxy)phenyl]sulfone [4-(3-aminophenoxy)phenyl]sulfone, bis[4-(4-aminophenoxy)phenyl]sulfone, bis[3-(3-aminophenoxy)phenyl]methane, bis[3-(4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]methane, 2,2-bis[3-(3-aminophenoxy)phenyl]propane, 2,2-bis[3-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, One or more selected from the group consisting of [4-(4-aminophenoxy)phenyl]propane (BAPP), 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane.
[0056] The above-mentioned polyimide film can preferably be obtained by subjecting a polyamic acid solution containing an acid dianhydride component and a diamine component to an imidization reaction, wherein the acid dianhydride component contains one or more selected from the group consisting of 3,3',4,4'-biphenyltetracarboxylic dianhydride (s-BPDA), pyromellitic dianhydride (PMDA) and 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), and the diamine component contains one or more selected from the group consisting of p-phenylenediamine (PPD), 4,4'-diaminodiphenyl ether (ODA) and 2,2'-dimethylbenzidine.
[0057] In addition, based on 100 mol % of the total content of the acid dianhydride components, the content of the 3,3',4,4'-biphenyltetracarboxylic dianhydride may be 100 mol % or less, the content of the pyromellitic dianhydride may be 55 mol % or less, and the content of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride may be 60 mol % or less.
[0058] On the other hand, based on 100 mol % of the total content of the diamine components, the content of the p-phenylenediamine may be 50 mol % to 100 mol %, the content of the 4,4'-diaminodiphenyl ether may be 20 mol % or less, and the content of the 2,2'-dimethylbenzidine may be 50 mol % or less.
[0059] When the content of pyromellitic dianhydride exceeds 55 mol %, the moisture absorption rate becomes extremely high, and the dimensional stability of the produced polyimide film with respect to water may be reduced.
[0060] On the other hand, in the case where the content of 3,3′,4,4′-benzophenonetetracarboxylic dianhydride is greater than 60 mol %, the modulus of the manufactured polyimide film may be very high, thereby exhibiting brittle characteristics.
[0061] In addition, when the content of p-phenylenediamine is less than 50 mol % or the content of 4,4′-diaminodiphenyl ether is greater than 20 mol %, the thermal expansion coefficient of the produced polyimide film may be excessively increased, thereby reducing thermal dimensional stability.
[0062] On the other hand, when the content of 2,2′-dimethylbenzidine is greater than 50 mol %, the modulus of the manufactured polyimide film may become very high and may show brittle characteristics.
[0063] In the present invention, the production of polyamic acid can be exemplified by the following method:
[0064] (1) A method in which all diamine components are added to a solvent, and then an acid dianhydride component is added in a substantially equimolar amount to the diamine component to carry out polymerization;
[0065] (2) A method in which all of the acid dianhydride component is added to a solvent, and then the diamine component is added in a substantially equimolar amount to the acid dianhydride component to carry out polymerization;
[0066] (3) A method in which a portion of the diamine component is added to a solvent, a portion of the acid dianhydride component is mixed at a ratio of about 95 to 105 mol % relative to the reaction components, and then the remaining diamine component is added, followed by the remaining acid dianhydride component, thereby polymerizing the diamine component and the acid dianhydride component in substantially equimolar amounts;
[0067] (4) A method in which an acid dianhydride component is added to a solvent, a portion of the diamine compound is mixed at a ratio of about 95 to 105 mol % relative to the reaction components, the remaining acid dianhydride component is added, and then the remaining diamine component is added, thereby polymerizing the diamine component and the acid dianhydride component in a substantially equimolar ratio;
[0068] (5) A method of forming a first composition by reacting a portion of a diamine component with a portion of an acid dianhydride component in a solvent in which either one of the components is in excess, and forming a second composition by reacting a portion of a diamine component with a portion of an acid dianhydride component in another solvent in which either one of the components is in excess, and then mixing the first and second compositions to complete polymerization, wherein, when forming the first composition, if the diamine component is in excess, the acid dianhydride component is in excess in the second composition, and if the acid dianhydride component is in excess in the first composition, the diamine component is in excess in the second composition, thereby mixing the first and second compositions and polymerizing the diamine component and the acid dianhydride component used in their reactions in a substantially equimolar manner; etc.
[0069] In one specific example, the method for producing a polyimide film of the present invention may include:
[0070] A step of providing a polyamic acid solution obtained from an acid dianhydride component and a diamine component;
[0071] The step of casting the polyamic acid solution onto a support and heating it to produce a self-supporting film of the polyamic acid solution; and
[0072] A step of imidizing and stretching the self-supporting film to produce a polyimide film.
[0073] In the present invention, the polymerization method of the polyamic acid as described above can be defined as a random polymerization method. From the viewpoint of maximizing the effect of the present invention of improving flatness, a polyimide film produced from the polyamic acid of the present invention produced by the above process can be preferably used.
[0074] However, the above-mentioned polymerization method can make the length of the repeating unit in the polymer chain described above shorter, so there may be limitations when exerting the various excellent properties of the polyimide chain from the acid dianhydride component. Therefore, the polymerization method of the polyamic acid that can be particularly preferably used in the present invention can be a block polymerization method.
[0075] On the other hand, the solvent used for synthesizing the polyamic acid is not particularly limited, and any solvent can be used as long as it can dissolve the polyamic acid, and an amide-based solvent is preferred.
[0076] Specifically, the above-mentioned organic solvent can be an organic polar solvent, and in detail, it can be an aprotic polar solvent (aprotic polar solvent), for example, it can be one or more selected from the group consisting of N,N-dimethylformamide (DMF), N,N-dimethylacetamide, N-methyl-pyrrolidone (NMP), γ-butyrolactone (GBL), and diethylene glycol dimethyl ether (Diglyme), but is not limited to this, and can be used alone or in combination of two or more as needed.
[0077] In one example, N,N-dimethylformamide and N,N-dimethylacetamide can be particularly preferably used as the above-mentioned organic solvent.
[0078] In addition, fillers can also be added in the polyamic acid manufacturing process to improve various properties of the film such as sliding property, thermal conductivity, corona resistance, Knoop hardness, etc. The added filler is not particularly limited, but as preferred examples, silicon dioxide, titanium oxide, aluminum oxide, silicon nitride, boron nitride, calcium hydrogen phosphate, calcium phosphate, mica, etc. can be cited.
[0079] The particle size of the filler is not particularly limited and can be determined according to the film properties to be modified and the type of filler added. Generally, the average particle size is 0.05 to 100 μm, preferably 0.1 to 75 μm, more preferably 0.1 to 50 μm, and particularly preferably 0.1 to 25 μm.
[0080] If the particle size is smaller than the above range, the modifying effect is less likely to be exhibited, while if it is larger than the above range, the surface properties may be significantly damaged or the mechanical properties may be significantly reduced.
[0081] In addition, the amount of filler added is not particularly limited, and can be determined based on the film properties to be modified or the filler particle size, etc. Generally speaking, the amount of filler added is 0.01 to 100 parts by weight, preferably 0.01 to 90 parts by weight, and more preferably 0.02 to 80 parts by weight, relative to 100 parts by weight of polyimide.
[0082] If the amount of filler added is less than the above range, the modification effect of the filler is not easily manifested, and if it is greater than the above range, the mechanical properties of the film may be greatly damaged. The method of adding the filler is not particularly limited, and any known method may be used.
[0083] In the production method of the present invention, the polyimide film can be produced by a thermal imidization method or a chemical imidization method.
[0084] Alternatively, the polyimide may be produced by a composite imidization method using a thermal imidization method and a chemical imidization method in combination.
[0085] The thermal imidization method is a method in which a chemical catalyst is excluded and an imidization reaction is induced by a heat source such as hot air or an infrared dryer.
[0086] In the thermal imidization method, the gel film may be heat-treated at a variable temperature in the range of 100 to 600° C. to imidize the amic acid groups in the gel film. Specifically, the heat treatment may be performed at 200 to 500° C., more specifically, at 300 to 500° C. to imidize the amic acid groups in the gel film.
[0087] However, a portion of the amic acid (about 0.1 mol % to 10 mol %) may also be imidized during the formation of the gel film. For this purpose, the polyamic acid composition can be dried at a variable temperature in the range of 50°C to 200°C, which also falls within the scope of the above-mentioned thermal imidization method.
[0088] In the case of the chemical imidization method, the polyimide film may be manufactured using a dehydrating agent and an imidization agent according to a method known in the art.
[0089] As an example of the composite imidization method, a dehydrating agent and an imidizing agent are added to a polyamic acid solution, and then partially cured and dried by heating at 80 to 200° C., preferably 100 to 180° C., and then heated at 200 to 400° C. for 5 to 400 seconds to produce a polyimide film.
[0090] The present invention provides a flexible metal foil laminate comprising the above-mentioned polyimide film and a conductive metal foil.
[0091] The metal foil used is not particularly limited, but when the flexible metal foil laminate of the present invention is used in electronic equipment or electrical equipment, for example, it can be a metal foil containing copper or copper alloy, stainless steel or its alloy, nickel or nickel alloy (including 42 alloy), aluminum or aluminum alloy.
[0092] In common flexible metal foil laminates, copper foils such as rolled copper foil and electrolytic copper foil are often used, and they can also be preferably used in the present invention. In addition, the surfaces of these metal foils can also be coated with a rust-proof layer, a heat-resistant layer or an adhesive layer.
[0093] In the present invention, the thickness of the metal foil is not particularly limited as long as it is a thickness that can sufficiently exhibit a function according to the intended use.
[0094] The flexible metal foil laminate of the present invention can be obtained by laminating, coating, sputtering or vapor-depositing a metal foil on at least one surface of the above-mentioned polyimide film.
[0095] In addition, the flexible metal foil laminate can be used as a two-layer FCCL, and can be particularly used for mobile phones, displays (LCD, PDP, OLED, etc.), and can be used for FPCB and COF applications.
[0096] The electronic component including the flexible metal foil laminate may be, for example, a communication circuit for a portable terminal, a communication circuit for a computer, or a communication circuit for aerospace, but is not limited thereto.
[0097] Implementation
[0098] The following describes the functions and effects of the invention in more detail through specific manufacturing examples and embodiments of the invention. However, these manufacturing examples and embodiments are provided only as examples of the invention, and the scope of rights of the invention is not limited thereto.
[0099] Production Example: Production of polyimide film
[0100] The polyimide film of the present invention can be produced by the following common method known in the art: First, the above-mentioned acid dianhydride and diamine component are reacted in an organic solvent to obtain a polyamic acid solution.
[0101] The acid dianhydride and diamine components may be added in the form of powder, bulk or solution. It is preferred that they be added in the form of powder at the initial stage of the reaction to allow the reaction to proceed, and then added in the form of solution to adjust the polymerization viscosity.
[0102] The obtained polyamic acid solution may be mixed with an imidization catalyst and a dehydrating agent and applied to a support.
[0103] Examples of the catalyst used include tertiary amines (e.g., isoquinoline, β-picoline, pyridine, etc.), and examples of the dehydrating agent include acid anhydrides, but are not limited thereto. In addition, examples of the support used above include glass plates, aluminum foils, circulating stainless steel belts or stainless steel drums, but are not limited thereto.
[0104] The film coated on the support is gelled on the support by dry air and heat treatment.
[0105] The gelled membrane is separated from the support and subjected to heat treatment to complete drying and imidization.
[0106] The film that has been heat treated may be heat treated under a certain tension to remove residual stress inside the film generated during the film formation process.
[0107] Specifically, in a reactor equipped with a stirrer and a nitrogen injection / discharge pipe, 500 ml of DMF was added while injecting nitrogen, and after the temperature of the reactor was set to 30°C, 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), pyromellitic dianhydride (PMDA), 3,3',4,4'-benzophenonetetracarboxylic dianhydride (BTDA), p-phenylenediamine (PPD), 4,4'-diaminodiphenyl ether (ODA) and 2,2'-dimethylbenzidine (MTD) were added and completely dissolved according to the adjusted composition ratio and the prescribed order. Then, the temperature of the reactor was heated to 40°C under a nitrogen atmosphere, and stirring was continued for 120 minutes to produce a polyamic acid with a first reaction viscosity of 1,500 cP.
[0108] The polyamic acid produced in this manner is stirred until the final viscosity becomes 100,000 to 120,000 cP.
[0109] The contents of the catalyst and the dehydrating agent are adjusted and added to the prepared final polyamic acid, and then a polyimide film is manufactured using a coater.
[0110] Examples and Comparative Examples
[0111] The polyimide film was produced according to the above-mentioned production example, but the contents of the acid dianhydride and the diamine component of the examples and comparative examples were adjusted as shown in the following Table 1.
[0112] [Table 1]
[0113]
[0114] The dimensional measurement value (200° C.), dimensional measurement value (50° C.), coefficient of thermal expansion (CTE), and moisture absorption rate of the manufactured polyimide film were measured and shown in Table 2 below.
[0115] (1) Determination of thermal expansion coefficient at elevated temperature
[0116] After the polyimide film was stored under a humidity condition of 50% RH for 48 hours, the change in size of the polyimide film during the heating process from 25°C to 400°C was measured using a thermal mechanical analyzer (TMA) at 50°C and 200°C during the first run (First Run), and the slope of the straight line connecting the size measurement value of the polyimide film measured at 200°C during the first run (First Run) in the above heating process and the size measurement value of the polyimide film measured at 50°C during the first run (First Run) in the above heating process was calculated.
[0117] Generally, the coefficient of thermal expansion (CTE) is measured by measuring the ppm / °C slope of the first run temperature drop section or the second run temperature rise section analyzed by a thermomechanical analyzer (TMA). However, in order to simulate the actual process and measure the dimensional change of the polyimide film affected by moisture, it is necessary to measure the slope (ppm / °C) of the first run temperature rise section analyzed by a thermomechanical analyzer (TMA) as in the present application.
[0118] (2) Determination of thermal expansion coefficient
[0119] The coefficient of thermal expansion (CTE) was measured using a thermomechanical analyzer Q400 from TA Corporation. The polyimide film was cut into pieces with a width of 4 mm and a length of 20 mm, and the sample measurement length was 16 mm. At this time, the sample measurement length direction was the TD direction.
[0120] In a nitrogen atmosphere, the temperature was raised from room temperature to 400°C at a rate of 10°C / min while applying a tension of 0.05 N, and then the slope was measured in the range of 50°C to 200°C while cooling again at a rate of 10°C / min. That is, the thermal expansion coefficient is equivalent to the slope measured in the cooling range after the temperature is raised.
[0121] On the other hand, the thermal expansion coefficient corresponding to the slope measured in the temperature drop section of the first run (First Run) shows a value similar to the normal thermal expansion coefficient corresponding to the slope measured in the temperature rise process of the second run (Second Run).
[0122] (3) Determination of moisture absorption rate
[0123] The moisture absorption rate is measured as follows: According to the ASTM D 570 method, the polyimide film is cut into squares of 5 cm x 5 cm to make test pieces, the cut test pieces are dried in an oven at 50°C for more than 24 hours, and then the weight is measured, the measured test pieces are immersed in water at 23°C for 24 hours, and then the weight is measured again, and the difference in weight obtained here is expressed in %.
[0124] [Table 2]
[0125]
[0126] The temperature-increasing thermal expansion coefficient (50 to 200° C.) of the polyimide films of Examples 1 to 6 was in the range of -1.5 ppm / ° C. to 6 ppm / ° C.
[0127] That is, Figure 1 a and Figure 1 As shown in the curve diagram of the dimensional change measurement results of the polyimide films of Examples 1 and 4 respectively represented by b, it can be confirmed that the slope of the straight line connecting the dimensional measurement value of the polyimide film in the TD direction measured at 200°C during the heating process and the dimensional measurement value of the polyimide film in the TD direction measured at 50°C during the above heating process, that is, the range of the thermal expansion coefficient during heating is above -1.5ppm / °C and below 6ppm / °C.
[0128] on the other hand, Figure 1 a and Figure 1 In the dimensional change measurement result graph of b, the dimensional change value on the Y axis represents the dimensional change value corresponding to the length (16 mm) of the polyimide film sample used in the TMA measurement.
[0129] The temperature-increasing thermal expansion coefficient (50 to 200° C.) was calculated as a zone slope obtained by converting the measurement results of the dimensional change measurement result graph into dimensional change values per 1 m length of the polyimide film.
[0130] In addition, the thermal expansion coefficient of the polyimide films of Examples 1 to 6 in the TD direction was 1 ppm / °C to 10 ppm / °C, and the moisture absorption rate was 1.5 wt% or less.
[0131] In contrast, the polyimide films of Comparative Examples 1 and 4 contained pyromellitic dianhydride at a content of more than 55 mol %, and the polyimide film of Comparative Example 5 contained p-phenylenediamine at a content of less than 50 mol % and 2,2'-dimethylbenzidine at a content of more than 50 mol %.
[0132] Therefore, the polyimide films of Comparative Examples 1, 4 and 5 had high moisture absorption or extremely low thermal expansion coefficients, resulting in shrinkage, and showed a value of less than -1.5 ppm / °C in thermal expansion coefficients (50 to 200°C) in heating.
[0133] That is, Figure 2 a and Figure 2 As shown in the curve diagram of the dimensional change measurement results of the polyimide films of Comparative Examples 1 and 4 respectively shown in b, the dimensional measurement values of the polyimide film in the TD direction measured at 200°C during the heating process and the dimensional measurement values of the polyimide film in the TD direction measured at 50°C during the above-mentioned heating process are converted into dimensional change values per 1m of the polyimide film, and the slope of the straight line connecting them is less than -1.5ppm / °C.
[0134] On the other hand, in the polyimide films of Comparative Examples 2 and 3, the content of the p-phenylenediamine was less than 50 mol %, and the content of 4,4′-diaminodiphenyl ether was greater than 20 mol %.
[0135] Therefore, the value of the thermal expansion coefficient (50 to 200° C.) becomes very large and deviates from the range of the thermal expansion coefficient (50 to 200° C.) of the polyimide film of the present application, and the value of the thermal expansion coefficient in the TD direction becomes very large, and the dimensional stability of the polyimide film decreases.
[0136] The embodiments of the polyimide film and the method for manufacturing the polyimide film of the present invention are only preferred embodiments that enable a person skilled in the art to which the present invention belongs to easily implement the present invention, and are not limited to the above embodiments, and therefore do not limit the scope of rights of the present invention. Therefore, the true technical protection scope of the present invention will be defined by the technical ideas of the attached claims. In addition, it is obvious to a person skilled in the art that various substitutions, deformations and changes can be made without departing from the technical ideas of the present invention, and of course, the parts that can be easily changed by a person skilled in the art also belong to the scope of rights of the present invention.
[0137] Industrial Applicability
[0138] The present invention provides a polyimide film having excellent dimensional stability even after being exposed to moisture for a certain period of time, thereby providing a polyimide film having excellent dimensional stability during metal foil lamination.
[0139] Such a polyimide film can be applied to various fields requiring a polyimide film with excellent dimensional stability, for example, a flexible metal foil laminate produced by a metallization method or an electronic component including such a flexible metal foil laminate.
Claims
1. A polyimide film, which after being stored under a humidity condition of 50% RH for 48 hours, When the dimensional change during the temperature rise from 25°C to 400°C was measured using a thermomechanical analyzer TMA, the thermal expansion coefficient during the temperature rise from 50°C to 200°C in the TD direction was -1.5ppm / °C to 6ppm / °C. The 50-200° C. heating thermal expansion coefficient is the slope of a straight line connecting the dimensional measurement value of the polyimide film in the TD direction measured at 200° C. during the first operation in the heating process and the dimensional measurement value of the polyimide film in the TD direction measured at 50° C. during the first operation in the heating process. The dimensional measurement value in the TD direction corresponds to a dimensional change value calculated by converting the length of the sample of the polyimide film used in the measurement with the thermomechanical analyzer into 1 m. 2 . The polyimide film according to claim 1 , wherein the thermal expansion coefficient in the TD direction is 1 ppm / ° C. or more and 10 ppm / ° C. or less. The polyimide film according to claim 1 , which has a moisture absorption rate of 1.5 wt % or less.
4. The polyimide film according to claim 1, which is obtained by imidization reaction of an acid dianhydride component and a diamine component. The acid dianhydride component is selected from pyromellitic dianhydride PMDA, oxydiphthalic dianhydride ODPA, 3,3',4,4'-biphenyltetracarboxylic dianhydride s-BPDA, 2,3,3',4'-biphenyltetracarboxylic dianhydride a-BPDA, diphenyl sulfone-3,4,3',4'-tetracarboxylic dianhydride DSDA, bis(3,4-dicarboxyphenyl)sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,3,3',4'-benzophenonetetracarboxylic dianhydride, 3,3',4,4'-benzophenonetetracarboxylic dianhydride BTDA, bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane At least one of the group consisting of alkane dianhydride, p-phenylene bis(trimellitic acid monoester anhydride), p-biphenylene bis(trimellitic acid monoester anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)phthalic dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane dianhydride BPADA, 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 1,4,5,8-naphthalenetetracarboxylic acid dianhydride and 4,4'-(2,2-hexafluoroisopropylidene)diphthalic acid dianhydride, The diamine component is selected from the group consisting of p-phenylenediamine PPD, m-phenylenediamine, 3,3'-dimethylbenzidine, 2,2'-dimethylbenzidine, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,5-diaminobenzoic acid DABA, 4,4'-diaminodiphenyl ether ODA, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylmethane (methylenediamine), 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane, 3,3',5,5'-tetramethyl 4,4'-diaminodiphenylmethane, bis(4-aminophenyl) sulfide, 4,4'-diaminobenzanilide, 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diamino-4,4'-dichlorobenzophenone, 3,3'-diamino-4,4'-dimethoxybenzophenone ketone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-aminophenyl)propane, 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenoxy)benzene TPE-R, 1,4-bis(3-aminophenoxy)benzene TPE-Q, 1,3-bis(3-aminophenoxy)-4-trifluoromethylbenzene, 3,3'-diamino-4-(4-phenyl)phenoxybenzophenone, 3,3'-diamino-4,4'-di(4-phenylphenoxy)benzophenone, 1,3-bis(3-aminophenyl sulfide)benzene, 1,3-bis(4-aminophenyl sulfide)benzene, 1,4-bis(4-aminophenyl sulfide)benzene, 1,3-bis(3-aminophenyl sulfone)benzene, 1,3-bis(4-aminophenyl sulfone)benzene, 1,4-bis(4-aminophenyl sulfone)benzene, 1,3-bis[2-(4-aminophenyl)isopropyl]benzene, 1,4-bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-Bis[2-(4-aminophenyl)isopropyl]benzene, 3,3'-bis(3-aminophenoxy)biphenyl, 3,3'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4'-bis(4-aminophenoxy)biphenyl, bis[3-(3-aminophenoxy)phenyl]ether, bis[3-(4-aminophenoxy)phenyl]ether, bis[4-(3-aminophenoxy)phenyl]ether, bis[4-(4-aminophenoxy)phenyl]ether, bis[3-(3-aminophenoxy)phenyl ] ketone, bis[3-(4-aminophenoxy)phenyl]ketone, bis[4-(3-aminophenoxy)phenyl]ketone, bis[4-(4-aminophenoxy)phenyl]ketone, bis[3-(3-aminophenoxy)phenyl]sulfide, bis[3-(4-aminophenoxy)phenyl]sulfide, bis[4-(3-aminophenoxy)phenyl]sulfide, bis[4-(4-aminophenoxy)phenyl]sulfide, bis[3-(3-aminophenoxy)phenyl]sulfone, bis[3-(4-aminophenoxy)phenyl]sulfone, bis[4-(3-aminophenoxy)phenyl]sulfone, bis[3-(3-aminophenoxy)phenyl]methane, bis[3-(4-aminophenoxy)phenyl]methane, bis[4-(3-aminophenoxy)phenyl]methane, bis[4-(4-aminophenoxy)phenyl]methane, 2,2-bis[3-(3-aminophenoxy)phenyl]propane, 2,2-bis[3-(4-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(3-aminophenoxy)phenyl]propane, 2,2-bis[4-(4-aminophenoxy)phenyl]propane, One or more selected from the group consisting of 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane and 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane.
5. The polyimide film according to claim 1, which is obtained by subjecting a polyamic acid solution containing an acid dianhydride component and a diamine component to an imidization reaction, The acid dianhydride component includes one or more selected from the group consisting of 3,3',4,4'-biphenyltetracarboxylic dianhydride s-BPDA, pyromellitic dianhydride PMDA and 3,3',4,4'-benzophenonetetracarboxylic dianhydride BTDA, The diamine component includes one or more selected from the group consisting of p-phenylenediamine PPD, 4,4′-diaminodiphenyl ether ODA, and 2,2′-dimethylbenzidine.
6. The polyimide film according to claim 5, based on the total content of the acid dianhydride components as 100 mol %, the content of the 3,3',4,4'-biphenyltetracarboxylic dianhydride is 100 mol % or less, the content of the pyromellitic dianhydride is 55 mol % or less, and the content of the 3,3',4,4'-benzophenonetetracarboxylic dianhydride is 60 mol % or less.
7. The polyimide film according to claim 5, wherein the content of p-phenylenediamine is 50 mol% to 100 mol%, the content of 4,4'-diaminodiphenyl ether is 20 mol% or less, and the content of 2,2'-dimethylbenzidine is 50 mol% or less, based on 100 mol% of the total content of the diamine components.
8. A method for producing a polyimide film, which is a method for producing the polyimide film according to any one of claims 1 to 7, comprising: A step of providing a polyamic acid solution obtained from an acid dianhydride component and a diamine component; The process of casting the polyamic acid solution on a support and heating it to produce a self-supporting film of the polyamic acid solution; and A step of imidizing and stretching the self-supporting film to produce a polyimide film. 9 . A flexible metal foil laminate comprising the polyimide film according to claim 1 and a conductive metal foil. 10 . The flexible metal foil laminate according to claim 9 , wherein the metal foil is formed by coating, sputtering or evaporation. 11 . An electronic component comprising the flexible metal foil laminate according to claim 10 .