Method for producing chloroprene polymer composition

By polymerizing chloroprene-based polymer B in the presence of diene-based polymer A, the problems of low recovery rate and insufficient performance in the manufacturing process of chloroprene-based polymer are solved, and high recovery rate and excellent results are obtained A chloroprene-based polymer composition with properties is suitable for impregnated moldings of various uses.

CN118946622APending Publication Date: 2024-11-12DENKA CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202380028565.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-31
Filing Date
2023-02-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

The conventional chloroprene-based polymers are prone to adhere to the polymerization container during the manufacturing process, resulting in low recovery and difficult to achieve an impregnated molded product with excellent tensile strength of breakage and 100% elongation modulus.

Method used

By polymerizing in the presence of diene polymer A, a chloroprene-based polymer B with different weight average molecular weights was prepared to form a high recovery rate, low 100% elongation modulus and excellent tensile strength for fracture chloroprene-based polymer composition.

Benefits of technology

A high recovery rate from the polymerization container is achieved, and the obtained chloroprene-based polymer composition has excellent tensile strength of breakage and a modulus of 100% elongation, and is suitable for use in medical gloves and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005049166220000021
    Figure BDA0005049166220000021
  • Figure BDA0005049166220000221
    Figure BDA0005049166220000221
  • Figure BDA0005049166220000301
    Figure BDA0005049166220000301
Patent Text Reader

Abstract

The purpose of the present invention is to provide a method for producing a chloroprene polymer composition with which it is possible to obtain a dip-molded article having a high recovery rate from a polymerization vessel, a low modulus at 100% elongation, and excellent tensile strength at break. According to the present invention, provided is a method for producing a chloroprene polymer composition containing a diene polymer (A) and a chloroprene polymer (B), the diene polymer (A) and the chloroprene polymer (B) having different weight-average molecular weights, and the diene polymer (A) and the chloroprene polymer (B) having different weight-average molecular weights. The method for producing the chloroprene polymer composition includes a polymerization step for obtaining the chloroprene polymer (B) by polymerization in the presence of the diene polymer (A).
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a method for producing a chloroprene polymer composition. Background Art

[0002] Chloroprene-based polymers are known as materials for dip-molded products such as medical surgical gloves, medical examination gloves, industrial gloves, balloons, catheters, rubber boots, and the like.

[0003] Various technologies have been proposed for chloroprene polymer latex for dip-molded products with improved flexibility of chloroprene polymers and dip-molded products of chloroprene polymers. Patent Document 1 describes a polychloroprene latex for use in dip-molded products, which contains 100 parts by mass of modified polychloroprene obtained by copolymerizing chloroprene and methacrylic acid, 90 to 150 parts by mass of water, 1 to 5 parts by mass of an emulsifier, and 0.5 to 2.5 parts by mass of potassium ions, and has a pH of 7 to 14. Patent Document 2 describes a mercaptan-modified polychloroprene latex for use in dip-molded products, wherein chloroprene and 2,3-dichloro-1,3-butadiene are copolymerized, and in the 13C-solid NMR spectrum of the polychloroprene, the peak area (A) of 126.2 to 127.6 ppm, the peak area (B) of 122.0 to 126.2 ppm, and the peak area (C) of 129.9 to 130.3 ppm are in the ranges shown by the following general formula (I). Patent Document 3 describes a chloroprene polymer latex for use in dip-molded products, which contains a high molecular weight polymer and a low molecular weight polymer, and can achieve both excellent softness and mechanical properties in a vulcanized rubber prepared by dip molding. Patent Document 4 describes a chloroprene polymer latex, which has excellent flexibility and exhibits mechanical properties even under mild vulcanization conditions by copolymerizing chloroprene monomers with isoprene monomers as raw materials of isoprene rubber. Patent Document 5 describes an isoprene / chloroprene polymer dip-molded product, which exhibits excellent flexibility even without containing a diphenylguanidine reagent as a vulcanization accelerator by mixing isoprene polymer latex and chloroprene polymer latex. Patent Document 6 describes a dip-molded product, which exhibits excellent mechanical properties by mixing nitrile-butadiene polymer (NBR) latex and isoprene polymer latex with chloroprene polymer latex as a base.

[0004] [Number 1]

[0005]

[0006] [Prior art documents]

[0007] [Patent Document]

[0008] [Patent Document 1] Japanese Patent Application Publication No. 2014-114342

[0009] [Patent Document 2] International Publication No. 2019 / 009038

[0010] [Patent Document 3] Japanese Patent Application Publication No. 2019-143002

[0011] [Patent Document 4] International Publication No. 2021-132460

[0012] [Patent Document 5] Japanese Patent Publication No. 2017-508840

[0013] [Patent Document 6] Japanese Patent Application Publication No. 2020-189963 Summary of the invention

[0014] Problem that the invention aims to solve

[0015] Chloroprene polymer compositions containing chloroprene polymers are widely used in applications such as gloves, balloons, boots, and catheters. In addition, in particular, in medical rubber gloves, there is a tendency to seek a chloroprene polymer composition that can obtain a dip-molded product having excellent flexibility and excellent tensile strength at break, similar to dip-molded products obtained using natural rubber and polyisoprene. In addition, when the production conditions of the chloroprene polymer are adjusted to obtain a dip-molded product with a low modulus at 100% elongation, the chloroprene polymer composition obtained after polymerization may become sticky and adhere to the polymerization container, thereby reducing the recovery rate.

[0016] The present invention has been made in view of the above circumstances and aims to provide a method for producing a chloroprene-based polymer composition which can obtain a dip-molded product having a high recovery rate from a polymerization vessel, a low modulus at 100% elongation, and excellent tensile strength at break.

[0017] Solutions for solving problems

[0018] According to the present invention, there is provided a method for producing a chloroprene polymer composition, wherein the chloroprene polymer composition comprises a diene polymer A and a chloroprene polymer B, the diene polymer A and the chloroprene polymer B having different weight average molecular weights, and the method for producing the chloroprene polymer composition comprises a polymerization step of obtaining the chloroprene polymer B by polymerization in the presence of the diene polymer A.

[0019] As a result of diligent studies, the present inventors have found that a chloroprene polymer composition containing a diene polymer A and a chloroprene polymer B having different weight average molecular weights can be produced by a specific production method, thereby obtaining a chloroprene polymer composition having a high recovery rate from a polymerization vessel, a low modulus at 100% elongation, and excellent tensile strength at break, thereby completing the present invention; the specific production method includes a polymerization step of obtaining the chloroprene polymer B by polymerization in the presence of the diene polymer A.

[0020] Various embodiments of the present invention are described below. The embodiments described below can be combined with each other.

[0021] Preferably, in the above-described method for producing a chloroprene polymer composition, the difference between the weight average molecular weight of the diene polymer A and the weight average molecular weight of the chloroprene polymer B is 100,000 or more.

[0022] Preferably, in the above-described method for producing a chloroprene-based polymer composition, the diene-based polymer A has a weight average molecular weight of 5,000 to 80,000.

[0023] Preferably, in the method for producing a chloroprene polymer composition described above, in the step of polymerizing the chloroprene polymer B, the amount of the diene polymer A added is 5.0 to 60.0 parts by mass based on 100 parts by mass of the chloroprene monomer or raw material monomer added.

[0024] Preferably, in the method for producing a chloroprene-based polymer composition described above, the diene-based polymer A is at least one selected from natural rubber, isoprene-based polymers, butadiene-based polymers, styrene-butadiene-based polymers, chloroprene-based polymers, and acrylonitrile-butadiene-based polymers.

[0025] Effects of the Invention

[0026] According to the chloroprene polymer of the present invention, a chloroprene polymer composition can be prepared which can produce a dip molded product having a high recovery rate from a polymerization vessel, a low modulus at 100% elongation, and excellent tensile strength at break. DETAILED DESCRIPTION

[0027] Hereinafter, the present invention will be described in detail by way of examples of the embodiments of the present invention. The present invention is not limited by these descriptions. The various characteristic matters of the embodiments of the present invention shown below can be combined with each other. In addition, the invention is established independently for each characteristic matter.

[0028] 1. Method for producing chloroprene polymer composition

[0029] The method for producing a chloroprene polymer composition of the present invention includes a polymerization step of obtaining a chloroprene polymer B by polymerization in the presence of a diene polymer A. The chloroprene polymer composition of the present invention includes a diene polymer A and a chloroprene polymer B, and the diene polymer A and the chloroprene polymer B have different weight average molecular weights.

[0030] Hereinafter, the diene polymer A and the chloroprene polymer B of the present invention will be described first.

[0031] 1.1 Diene polymer A

[0032] In the present invention, the diene polymer A refers to a polymer containing a diene monomer unit derived from a diene monomer. The diene polymer A may contain a monomer unit derived from a monomer other than the diene monomer, etc., within the range not impairing the purpose of the present invention.

[0033] The diene polymer A of one embodiment of the present invention may contain 50 to 100% by mass of monomer units derived from diene monomers, preferably 70 to 100% by mass, when the diene polymer A is 100% by mass. The content of the monomer units derived from diene monomers is, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, 100% by mass, and may be within the range between any two of the values ​​exemplified herein.

[0034] The diene monomer may be a conjugated diene monomer having 4 to 6 carbon atoms, and specific examples thereof include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, 2,3-dichloro-1,3-butadiene, and 1-chloro-1,3-butadiene. The diene polymer A preferably contains a chloroprene monomer unit.

[0035] The diene polymer A according to one embodiment of the present invention preferably contains at least one selected from natural rubber, isoprene polymers, butadiene polymers, styrene-butadiene polymers, chloroprene polymers, and acrylonitrile-butadiene polymers.

[0036] The diene polymer A of one embodiment of the present invention preferably contains a monomer unit derived from chloroprene, and more preferably contains a monomer unit derived from 2,3-dichloro-1,3-butadiene. The diene polymer A of one embodiment of the present invention may not contain sulfur, and the diene polymer A of one embodiment of the present invention may also be a polymer having no -SS- structure derived from sulfur in the main chain.

[0037] The diene polymer A of one embodiment of the present invention may contain 50 to 100% by mass of monomer units derived from chloroprene, preferably 70 to 100% by mass, when the diene polymer A is 100% by mass. The content of the monomer units derived from chloroprene is, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100% by mass, and may be within the range between any two of the values ​​exemplified herein.

[0038] The diene polymer A of one embodiment of the present invention may contain 0 to 30% by mass of a monomer unit derived from 2,3-dichloro-1,3-butadiene, based on 100% by mass of the diene polymer A. The content of the monomer unit derived from 2,3-dichloro-1,3-butadiene may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, and may be within the range between any two of the values ​​exemplified herein.

[0039] The diene polymer A and the chloroprene polymer B of the present invention have different weight average molecular weights. The difference between the weight average molecular weight of the diene polymer A of one embodiment of the present invention and the weight average molecular weight of the chloroprene polymer B described below is preferably 100,000 or more, and more preferably 400,000 or more. The difference between the weight average molecular weight of the diene polymer A and the weight average molecular weight of the chloroprene polymer B described below is, for example, 100,000, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,200,000, 1,300,000, 1,400,000, 1,500,000, and may also be within the range between any two of the values ​​exemplified herein.

[0040] For example, the weight average molecular weight of the diene polymer A may be smaller than the molecular weight of the chloroprene polymer B. The weight average molecular weight of the diene polymer A may be 5,000 to 80,000. The weight average molecular weight of the diene polymer A is, for example, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, 22,000, 23,000, 24,000, 25,000, 26,000, 27,000, 28,000, 29,000, 30,000, 35,000, 40,000, 5,0000, 60,000, 70,000, or 80,000, and may be within the range between any two of the values ​​exemplified here.

[0041] In addition, as another example, the weight average molecular weight of the diene polymer A may be greater than the molecular weight of the chloroprene polymer B. The weight average molecular weight of the diene polymer A may be 200,000 to 1,500,000. The weight average molecular weight of the diene polymer A is, for example, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, 1,500,000, and may be within the range between any two of the values ​​exemplified herein.

[0042] The weight average molecular weight of diene polymer A can be obtained by using gel permeation chromatography (GPC) to mix a polymerization solution (such as latex) containing diene polymer A with a large amount of methanol to precipitate it, filtering, drying and dissolving the diene polymer A in tetrahydrofuran to obtain a sample for analysis. The measurement conditions of GPC can be as described in the examples. The weight average molecular weight of diene polymer A can be controlled by adjusting the polymerization formula in the polymerization of diene polymer A, the type and amount of chain transfer agent, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc., and can be especially controlled by adjusting the type and amount of chain transfer agent.

[0043] 1.2 Method for producing diene polymer A

[0044] The method for producing the diene polymer A of the present invention is not particularly limited. For example, the method for producing the diene polymer A according to one embodiment of the present invention may include a diene polymer A polymerization step of polymerizing a raw material monomer containing a diene monomer to obtain a diene polymer.

[0045] In the polymerization step, the raw material monomers include one or more diene monomers and may also include other monomers copolymerizable with the diene monomers. Examples of diene monomers include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, chloroprene, 2,3-dichloro-1,3-butadiene, and 1-chloro-1,3-butadiene. Examples of other monomers copolymerizable with the diene monomers include styrene, methacrylic acid, acrylonitrile, sulfur, and the like.

[0046] It is preferred to adjust the type and amount of each monomer so that the content of each monomer unit in the obtained diene polymer A falls within the above numerical range. As an example, when the diene polymer A contains chloroprene monomer units and 2,3-dichloro-1,3-butadiene monomer units, and contains 0 to 30% by mass of 2,3-dichloro-1,3-butadiene monomer units relative to 100% by mass of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene monomer, the amount of 2,3-dichloro-1,3-butadiene added is preferably in the range of 0 to 30 parts by mass relative to 100 parts by mass of the total of the chloroprene monomer and the 2,3-dichloro-1,3-butadiene monomer.

[0047] When producing the diene polymer A, the raw material monomers are polymerized by polymerization methods such as emulsion polymerization, solution polymerization, suspension polymerization, and bulk polymerization. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as easy control, easy extraction of the polymer from the polymerization solution, and high polymerization rate.

[0048] In the polymerization step of the diene polymer A, the raw material monomers can be put into a polymerization container together with necessary reagents such as a polymerization initiator, a chain transfer agent, and a solvent for polymerization. As an example, when the diene polymer A is polymerized by emulsion polymerization, the raw material monomers can be put into a reaction tank together with a chain transfer agent, water, an alkali (for example, a metal hydroxide such as potassium hydroxide and sodium hydroxide), an emulsifier (dispersant), a reducing agent (for example, sodium bisulfite), a polymerization initiator, etc. for polymerization.

[0049] The polymerization initiator is not particularly limited, and a known polymerization initiator commonly used in the polymerization of diene polymers can be used. Examples of the polymerization initiator include organic peroxides such as potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, and tert-butyl hydroperoxide.

[0050] The type of chain transfer agent used in emulsion polymerization is not particularly limited, and for example, long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, and known chain transfer agents commonly used in the polymerization of diene polymers such as iodoform can be used. The chain transfer agent is preferably a long-chain alkyl mercaptan, and more preferably n-dodecyl mercaptan.

[0051] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the diene polymer A obtained can be adjusted.

[0052] As an example, in order to obtain a diene polymer A having a weight average molecular weight of 5,000 to 80,000, the amount of the chain transfer agent added before the start of emulsion polymerization is preferably 0.5 to 10.0 parts by mass relative to 100 parts by mass of the monomer. In this case, the amount added is, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0 parts by mass, and may be within the range between any two of the values ​​exemplified here.

[0053] In addition, as an example, in order to obtain a diene polymer A having a weight average molecular weight of 200,000 or more, preferably a weight average molecular weight of 500,000 to 1,500,000, the amount of the chain transfer agent added is preferably 0 mass or more and less than 0.40 mass parts relative to 100 mass parts of the monomer. The amount of the chain transfer agent added is more preferably 0.02 to 0.05 mass parts, for example, 0, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.20, 0.30 mass parts, less than 0.40 mass parts, and may also be within the range between any two of the values ​​exemplified herein. In particular, when attempting to obtain a diene polymer A having a weight average molecular weight of 200,000 or more, a chain transfer agent may not be used.

[0054] In the case of emulsion polymerization, the pH of the aqueous emulsion is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and a monomer immediately before the start of the emulsion polymerization, and also includes the case where the composition is changed by adding each component later or adding each component in batches. If the pH of the aqueous emulsion at the start of the emulsion polymerization is 10.5 or more, the polymerization reaction can be controlled more stably. If the pH is 13.5 or less, the excessive increase in viscosity during the polymerization can be suppressed, and the polymerization reaction can be controlled more stably.

[0055] In the polymerization step, the monomers may include chloroprene and 2,3-dichloro-1,3-butadiene, and may also include other monomers copolymerizable with chloroprene and 2,3-dichloro-1,3-butadiene. The other monomers are as described above for the monomer units that may be contained in the chloroprene-based polymer.

[0056] Furthermore, it is preferred to adjust the type and amount of each monomer so that the content of each monomer unit in the obtained chloroprene polymer falls within the above-mentioned numerical range.

[0057] The emulsifier preferably contains rosin acid and / or rosin salt. Examples of rosin salts include alkali metal salts such as sodium salts and potassium salts. The amount of rosin acid and rosin salt added may be 3.0 to 7.0 parts by mass relative to 100 parts by mass of the raw material monomer used. The amount of rosin acid and rosin salt added may be, for example, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, or 7.0 parts by mass, or may be within the range between any two of the values ​​exemplified herein.

[0058] The emulsifier may also contain emulsifiers and dispersants other than rosin acid and rosin salts. As emulsifiers and dispersants other than rosin acid and rosin salts, cationic, anionic, and nonionic emulsifiers and dispersants can be used. In one embodiment of the present invention, as the emulsifier used in the emulsion polymerization step, rosin acid and / or rosin salts, and anionic emulsifiers and dispersants may be included. As anionic emulsifiers and dispersants, from the viewpoint of stabilizing the chloroprene polymer latex when the pH adjuster is added, it is preferred to use sulfate-based and sulfonate-based anionic emulsifiers and dispersants in combination. Specifically, alkyl sulfonates, alkyl aryl sulfates, condensates of sodium β-naphthalenesulfonate and formaldehyde, and sodium alkyl diphenyl ether disulfonate having a carbon number of 8 to 20 can be cited. The amount of anionic emulsifiers and dispersants added can be 0.05 to 5 parts by mass relative to 100 parts by mass of the raw material monomer. The amount of the anionic emulsifier or dispersant added is, for example, 0.05, 0.1, 0.2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass per 100 parts by mass of the raw monomers, or may be within the range between any two of the values ​​exemplified here.

[0059] The polymerization temperature is preferably within a range of 5 to 55° C. It is more preferred that the polymerization temperature is 5° C. or higher because the emulsion does not freeze, and that the polymerization temperature is 55° C. or lower because the diene monomer does not evaporate or boil.

[0060] The polymerization conversion rate is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. When the desired polymerization conversion rate is reached, the polymerization can be terminated by adding a polymerization terminator that stops the polymerization reaction, or by stopping the addition of a polymerization initiator to adjust the polymerization conversion rate.

[0061] As polymerization terminators, for example, there are diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. A polymerization terminator may not be used in the polymerization step of the diene polymer A of one embodiment of the present invention. After the polymerization is completed, unreacted monomers can be removed by conventional methods such as reduced pressure distillation.

[0062] Furthermore, to the composition (e.g., latex) containing the diene polymer A obtained by the production method of one embodiment of the present invention, a freeze stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, etc. may be arbitrarily added after polymerization within a range that does not impair the effects of the present invention.

[0063] In the polymerization step of the diene polymer A, the polymerization may be started after all the raw material monomers and reagents used in the polymerization step are added to the polymerization container before the start of the polymerization, or at least a portion of the raw material monomers and / or reagents used in the polymerization step may be added to the polymerization container before the start of the polymerization and the remaining portion may be added after the start of the polymerization.

[0064] Before the start of polymerization, at least a portion of the raw material monomers and reagents are added to the polymerization container. When the remaining raw material monomers and / or reagents are added after the start of polymerization, the remaining raw material monomers and / or reagents can be added once or in multiple times, or can be added continuously at a certain flow rate. In one embodiment of the present invention, at least a portion of the raw material monomers can be added in portions after the start of polymerization. As an example, when chloroprene and 2,3-dichloro-1,3-butadiene are used as raw material monomers, a portion of chloroprene can be added in portions after the start of polymerization.

[0065] As an example, the batch addition of the remaining raw material monomers and / or reagents can be started when the polymerization rate of the raw material monomers added before the start of polymerization reaches 50 to 95%. The polymerization rate at the start of the batch addition can be, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 95%, or can be within the range between any two of the values ​​exemplified here.

[0066] When at least a portion of the raw material monomers is added after the start of polymerization, 50 parts by mass or less of 100 parts by mass of all the raw material monomers used in the polymerization step may be added after the start of polymerization. In this case, the amount of the raw material monomer added after the start of polymerization may be, for example, 0, 5, 10, 15, 20, 25, 30, 35, 40, 45, or 50 parts by mass, or may be within the range between any two of the values ​​exemplified herein. As an example, the batch addition of the raw material monomers, such as chloroprene, may be performed continuously within 30 to 300 minutes.

[0067] 1.3 Chloroprene polymer B

[0068] In the present invention, the chloroprene polymer refers to a polymer containing monomer units from 2-chloro-1,3-butadiene (hereinafter, also referred to as chloroprene). In addition, the chloroprene polymer of one embodiment of the present invention may also be a copolymer of chloroprene and other monomers copolymerizable with chloroprene, and as other monomers, 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, isoprene, styrene, methacrylic acid, acrylonitrile, sulfur, etc. can be listed, and other monomers may also be used in combination with two or more of them. The chloroprene polymer B of one embodiment of the present invention preferably contains monomer units from 2,3-dichloro-1,3-butadiene. The chloroprene polymer B of one embodiment of the present invention may not contain sulfur, and the chloroprene polymer B of one embodiment of the present invention may also be a polymer that does not have a -SS- structure derived from sulfur in the main chain.

[0069] The chloroprene polymer B of one embodiment of the present invention may contain 50 to 100% by mass of monomer units derived from chloroprene, preferably 70 to 100% by mass, when the chloroprene polymer B is 100% by mass. The content of the monomer units derived from chloroprene is, for example, 50, 55, 60, 65, 70, 75, 80, 85, 90, 91, 92, 93, 94, 95, 96, 97, 98, 99, or 100% by mass, and may be within the range between any two of the values ​​exemplified herein.

[0070] The chloroprene polymer B of one embodiment of the present invention may contain 0 to 30% by mass of a monomer unit derived from 2,3-dichloro-1,3-butadiene, based on 100% by mass of the chloroprene polymer B. The content of the monomer unit derived from 2,3-dichloro-1,3-butadiene may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, 10, 11, 12, 13, 14, 15, 16, 17, 18, 19, 20, 21, 22, 23, 24, 25, 26, 27, 28, 29, or 30% by mass, and may be within a range between any two of the values ​​exemplified herein.

[0071] The chloroprene polymer B of the present invention has a different weight average molecular weight from that of the diene polymer A. As described above, the difference between the weight average molecular weight of the diene polymer A of one embodiment of the present invention and the weight average molecular weight of the chloroprene polymer B described below is preferably 100,000 or more, more preferably 400,000 or more.

[0072] As an example, the weight average molecular weight of chloroprene polymer B may be greater than that of diene polymer A. The weight average molecular weight of chloroprene polymer B may be 200,000 to 1,500,000. The weight average molecular weight of chloroprene polymer B may be, for example, 200,000, 300,000, 400,000, 500,000, 600,000, 700,000, 800,000, 900,000, 1,000,000, 1,100,000, 1,200,000, 1,300,000, 1,400,000, 1,500,000, or may be within the range between any two of the values ​​exemplified herein.

[0073] In addition, as another example, the weight average molecular weight of the chloroprene polymer B may be smaller than the molecular weight of the diene polymer A. The weight average molecular weight of the chloroprene polymer B may be 5,000 to 80,000. The weight average molecular weight of the chloroprene polymer B is, for example, 5,000, 6,000, 7,000, 8,000, 9,000, 10,000, 11,000, 12,000, 13,000, 14,000, 15,000, 16,000, 17,000, 18,000, 19,000, 20,000, 21,000, The amount may be within a range between any two of the values ​​exemplified herein.

[0074] The weight average molecular weight of the chloroprene polymer B can be obtained by analyzing a sample obtained by mixing a polymerization solution containing the chloroprene polymer B (e.g., a chloroprene polymer composition (latex)) with a large amount of methanol to precipitate it, filtering, and drying the chloroprene polymer B dissolved in tetrahydrofuran using gel permeation chromatography (GPC). The measurement conditions of GPC can be described in the examples. The weight average molecular weight of the chloroprene polymer B can be controlled by adjusting the polymerization formula, the type and amount of the chain transfer agent, the polymerization temperature, the polymerization time, the polymerization conversion rate, etc. in the polymerization of the chloroprene polymer B, and can be controlled in particular by adjusting the type and amount of the chain transfer agent.

[0075] 1.4 Polymerization method of chloroprene polymer B

[0076] The method for producing a chloroprene polymer composition of the present invention includes a polymerization step of obtaining a chloroprene polymer B by polymerization in the presence of a diene polymer A.

[0077] According to the present invention, by polymerizing in the presence of a diene polymer A to obtain a chloroprene polymer B, a chloroprene polymer composition can be prepared which can produce a dip-molded article having a high recovery rate from a polymerization vessel, a low modulus at 100% elongation, and excellent tensile strength at break.

[0078] The mechanism by which a chloroprene polymer composition capable of obtaining a dip-molded article having a high recovery rate from a polymerization vessel, a low modulus at 100% elongation, and excellent tensile strength at break can be obtained by polymerizing the chloroprene polymer B in the presence of the diene polymer A is not yet clear, but it is presumed that the chloroprene polymer composition obtained by polymerizing the chloroprene polymer B in the presence of the diene polymer A has highly uniformly mixed diene polymer A and chloroprene polymer B in the chloroprene polymer composition, as compared with a chloroprene polymer composition obtained by polymerizing the diene polymer A and the chloroprene polymer B separately and mixing them after polymerization, and therefore the obtained chloroprene polymer composition and the obtained dip-molded article have excellent physical properties.

[0079] The diene polymer A can be added to the polymerization solution in any form, for example, the polymerization solution after the polymerization of the diene polymer A can be directly used. As an example, when the diene polymer A is polymerized by emulsion polymerization, the latex containing the diene polymer A can be added to the polymerization solution of the chloroprene polymer B. In addition, for example, the diene polymer A can be precipitated from the polymerization solution after the polymerization of the diene polymer A, and the precipitated diene polymer A can be added to the polymerization solution of the chloroprene polymer B. As an example, when the diene polymer A is polymerized by emulsion polymerization, methanol can be used to precipitate the diene polymer A from the latex containing the diene polymer A and add it to the polymerization solution of the chloroprene polymer B, and the diene polymer A obtained by freeze-drying the latex containing the diene polymer A can also be added to the polymerization solution of the chloroprene polymer B.

[0080] In the polymerization step of polymerizing the chloroprene polymer B, when the amount of the chloroprene monomer (or raw material monomer) added is 100 parts by mass, the amount of the diene polymer A added may be 5.0 to 60.0 parts by mass or 40.0 to 95.0 parts by mass.

[0081] In one embodiment of the present invention, when the weight average molecular weight of the diene polymer A is less than the weight average molecular weight of the chloroprene polymer B, for example, when the weight average molecular weight of the diene polymer A is 5,000 to 80,000, the amount of the diene polymer A added can be 5.0 to 60.0 parts by mass relative to 100 parts by mass of the chloroprene monomer (or raw material monomer) added. When the molecular weight of the diene polymer A is greater than the molecular weight of the chloroprene polymer B, for example, when the weight average molecular weight of the diene polymer A is 200,000 to 1,500,000, the amount of the diene polymer A added can be 40.0 to 95.0 parts by mass relative to 100 parts by mass of the chloroprene monomer (or raw material monomer) added.

[0082] When the weight average molecular weight of diene polymer A is less than the weight average molecular weight of chloroprene polymer B, the amount of diene polymer A added is, for example, 5.0, 10.0, 15.0, 20.0, 25.0, 30.0, 35.0, 40.0, 50.0, 60.0 parts by mass relative to 100 parts by mass of chloroprene monomer (or raw material monomer), or it may be in the range between any two numerical values ​​exemplified herein. When the molecular weight of diene polymer A is greater than the molecular weight of chloroprene polymer B, the amount of diene polymer A added is, for example, 40.0, 50.0, 60.0, 65.0, 70.0, 75.0, 80.0, 85.0, 90.0, 95.0 parts by mass relative to 100 parts by mass of chloroprene monomer (or raw material monomer), or it may be in the range between any two numerical values ​​exemplified herein.

[0083] In the polymerization step, the raw material monomer contains chloroprene and may contain other monomers copolymerizable with chloroprene. Examples of other monomers include 1-chloro-1,3-butadiene, 2,3-dichloro-1,3-butadiene, 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, styrene, methacrylic acid, acrylonitrile, sulfur, and the like.

[0084] It is preferred to adjust the type and amount of each monomer so that the content of each monomer unit in the obtained chloroprene polymer B falls within the above-mentioned numerical range.

[0085] When producing the chloroprene polymer B, the raw material monomers are polymerized by a polymerization method such as emulsion polymerization, solution polymerization, suspension polymerization, bulk polymerization, etc. Among these polymerization methods, emulsion polymerization is preferred because it has various advantages such as easy control, easy extraction of the polymer from the polymerization-completed solution, and high polymerization speed.

[0086] In the polymerization step of the chloroprene polymer B, the raw material monomers can be put into a polymerization container together with necessary reagents such as a polymerization initiator, a chain transfer agent, and a solvent to carry out polymerization. As an example, when the chloroprene polymer B is polymerized by emulsion polymerization, the raw material monomers can be put into a reaction tank together with a chain transfer agent, water, an alkali (for example, a metal hydroxide such as potassium hydroxide and sodium hydroxide), an emulsifier (dispersant), a reducing agent (for example, sodium bisulfite), a polymerization initiator, etc. to carry out polymerization.

[0087] The polymerization initiator is not particularly limited, and a known polymerization initiator commonly used in the polymerization of chloroprene-based polymers can be used. Examples of the polymerization initiator include organic peroxides such as potassium persulfate, ammonium persulfate, sodium persulfate, hydrogen peroxide, and tert-butyl hydroperoxide.

[0088] The type of chain transfer agent used in emulsion polymerization is not particularly limited, and for example, long-chain alkyl mercaptans such as n-dodecyl mercaptan and tert-dodecyl mercaptan, dialkyl xanthogen disulfides such as diisopropyl xanthogen disulfide and diethyl xanthogen disulfide, and known chain transfer agents commonly used in the polymerization of chloroprene such as iodoform can be used. The chain transfer agent is preferably a long-chain alkyl mercaptan, and more preferably n-dodecyl mercaptan.

[0089] By adjusting the type and amount of the chain transfer agent, the weight average molecular weight of the chloroprene polymer B obtained can be adjusted.

[0090] As an example, in order to obtain a chloroprene polymer B having a weight average molecular weight of 200,000 or more, preferably a weight average molecular weight of 500,000 to 1,500,000, the amount of the chain transfer agent added is preferably 0 to less than 0.40 parts by mass relative to 100 parts by mass of the monomer. The amount of the chain transfer agent added is more preferably 0 to 0.05 parts by mass, for example, 0, 0.005, 0.01, 0.02, 0.03, 0.04, 0.05, 0.06, 0.07, 0.08, 0.09, 0.10, 0.20, 0.30 parts by mass, less than 0.40 parts by mass, and may also be within the range between any two of the values ​​exemplified herein. In addition, when attempting to obtain a chloroprene polymer B having a weight average molecular weight of 200,000 or more, the chain transfer agent may not be used.

[0091] In addition, as an example, in order to obtain a chloroprene polymer B having a weight average molecular weight of 5,000 to 80,000, the amount of the chain transfer agent added before the start of emulsion polymerization is preferably 0.5 to 10.0 parts by mass relative to 100 parts by mass of the monomer. In this case, the amount added is, for example, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0 parts by mass, and may be within the range between any two of the values ​​exemplified here.

[0092] By adjusting the weight average molecular weights of the diene polymer A and the chloroprene polymer B within the above numerical range, and adjusting the amount of the diene polymer A added relative to 100 parts by mass of the chloroprene monomer added within the above numerical range, a chloroprene polymer composition capable of providing a dip-molded article having a low modulus at 100% elongation and excellent tensile strength at break can be prepared.

[0093] In the case of emulsion polymerization, the pH of the aqueous emulsion is preferably 10.5 to 13.5. The aqueous emulsion refers to a mixed solution of a chain transfer agent and a monomer immediately before the start of the emulsion polymerization, and also includes the case where the composition is changed by adding each component later or adding each component in batches. If the pH of the aqueous emulsion at the start of the emulsion polymerization is 10.5 or more, the polymerization reaction can be controlled more stably. If the pH is 13.5 or less, the excessive increase in viscosity during the polymerization can be suppressed, and the polymerization reaction can be controlled more stably.

[0094] In the polymerization step, the monomers may include chloroprene and 2,3-dichloro-1,3-butadiene, and may also include other monomers copolymerizable with chloroprene and 2,3-dichloro-1,3-butadiene. The other monomers are as described above for the monomer units that may be contained in the chloroprene-based polymer.

[0095] Furthermore, it is preferred to adjust the type and amount of each monomer so that the content of each monomer unit in the obtained chloroprene polymer falls within the above-mentioned numerical range.

[0096] The emulsifier preferably contains rosin acid and / or rosin salt. Examples of rosin salts include alkali metal salts such as sodium salts and potassium salts. The amount of rosin acid and rosin salt added may be 3.0 to 7.0 parts by mass relative to 100 parts by mass of the raw material monomer used. The amount of rosin acid and rosin salt added may be, for example, 3.0, 3.5, 4.0, 4.5, 5.0, 5.5, 6.0, 6.5, or 7.0 parts by mass, or may be within the range between any two of the values ​​exemplified herein.

[0097] The emulsifier may also contain emulsifiers and dispersants other than rosin acid and rosin salts. As emulsifiers and dispersants other than rosin acid and rosin salts, cationic, anionic, and nonionic emulsifiers and dispersants can be used. In one embodiment of the present invention, as the emulsifier used in the emulsion polymerization step, rosin acid and / or rosin salts, and anionic emulsifiers and dispersants may be included. As anionic emulsifiers and dispersants, from the viewpoint of stabilizing the chloroprene polymer latex when the pH adjuster is added, it is preferred to use sulfate-based and sulfonate-based anionic emulsifiers and dispersants in combination. Specifically, alkyl sulfonates, alkyl aryl sulfates, condensates of sodium β-naphthalenesulfonate and formaldehyde, and sodium alkyl diphenyl ether disulfonate having a carbon number of 8 to 20 can be cited. The amount of anionic emulsifiers and dispersants added can be 0.05 to 5 parts by mass relative to 100 parts by mass of the raw material monomer. The amount of the anionic emulsifier or dispersant added is, for example, 0.05, 0.1, 0.2, 0.3, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, or 5.0 parts by mass per 100 parts by mass of the raw monomers, or may be within the range between any two of the values ​​exemplified here.

[0098] The polymerization temperature is preferably in the range of 5 to 55° C. It is more preferred that the polymerization temperature is 5° C. or higher because the emulsion does not freeze, and that the polymerization temperature is 55° C. or lower because the chloroprene monomer does not evaporate or boil.

[0099] The polymerization conversion rate is preferably in the range of 50 to 95%. The polymerization reaction is terminated by adding a polymerization terminator. When the desired polymerization conversion rate is reached, the polymerization can be terminated by adding a polymerization terminator that stops the polymerization reaction.

[0100] Examples of the polymerization terminator include diethylhydroxylamine, thiodiphenylamine, 4-tert-butylcatechol, 2,2'-methylenebis-4-methyl-6-tert-butylphenol, etc. After the polymerization, unreacted monomers can be removed by a conventional method such as reduced pressure distillation.

[0101] Furthermore, to the chloroprene polymer composition (e.g., latex) containing the diene polymer A and the chloroprene polymer B obtained by the production method of one embodiment of the present invention, a freezing stabilizer, an emulsion stabilizer, a viscosity modifier, an antioxidant, a preservative, etc. may be arbitrarily added after polymerization within a range that does not impair the effects of the present invention.

[0102] In the polymerization step of the chloroprene-based polymer B, the polymerization may be started after all the raw material monomers and reagents used in the polymerization step are added to the polymerization container before the start of the polymerization, or at least a portion of the raw material monomers and / or reagents used in the polymerization step may be added to the polymerization container before the start of the polymerization, and the remaining portion may be added after the start of the polymerization.

[0103] Before the start of polymerization, at least a portion of the raw material monomers and reagents are added to the polymerization container. When the remaining raw material monomers and / or reagents are added after the start of polymerization, the remaining raw material monomers and / or reagents can be added once or in multiple times, or can be added continuously at a certain flow rate. In one embodiment of the present invention, at least a portion of the raw material monomers and / or reagents can be added in batches after the start of polymerization. As an example, a portion of the polymerization initiator can be added in batches after the start of polymerization.

[0104] 1.5 Chloroprene polymer composition

[0105] The chloroprene polymer composition according to one embodiment of the present invention includes a diene polymer A and a chloroprene polymer B, and the diene polymer A and the chloroprene polymer B have different weight average molecular weights.

[0106] The chloroprene polymer composition according to one embodiment of the present invention preferably has a peak with a weight average molecular weight of 5,000 to 80,000 and a peak with a weight average molecular weight of 200,000 to 1,500,000 detected in a molecular weight distribution obtained by measuring by gel permeation chromatography a sample obtained by mixing the chloroprene polymer composition with a large amount of methanol to precipitate, filtering and drying the obtained polymer and dissolving it in tetrahydrofuran. More preferably, a peak with a weight average molecular weight of 5,000 to 50,000 and a peak with a weight average molecular weight of 300,000 to 1,500,000 are detected. Further preferably, a peak with a weight average molecular weight of 8,000 to 30,000 and a peak with a weight average molecular weight of 500,000 to 1,500,000 are detected. The chloroprene polymer composition of one embodiment of the present invention preferably contains a diene polymer A having a weight average molecular weight of 5,000 to 80,000 and a chloroprene polymer B having a weight average molecular weight of 200,000 to 1,500,000, or a chloroprene polymer B having a weight average molecular weight of 5,000 to 80,000 and a diene polymer A having a weight average molecular weight of 200,000 to 1,500,000, more preferably a diene polymer A having a weight average molecular weight of 5,000 to 50,000 and a chloroprene polymer B having a weight average molecular weight of 300,000 to 1,500,000. 00, or a chloroprene polymer B with a weight average molecular weight of 5,000 to 50,000 and a diene polymer A with a weight average molecular weight of 300,000 to 1,500,000, and more preferably contains a diene polymer A with a weight average molecular weight of 8,000 to 30,000 and a chloroprene polymer B with a weight average molecular weight of 500,000 to 1,500,000, or a chloroprene polymer B with a weight average molecular weight of 8,000 to 30,000 and a diene polymer A with a weight average molecular weight of 500,000 to 1,500,000.

[0107] The chloroprene polymer composition according to one embodiment of the present invention preferably contains 5 to 40% by mass of a polymer having a weight average molecular weight of 5,000 to 80,000, based on 100% by mass of the polymer contained in the chloroprene polymer composition. The content of the polymer having a weight average molecular weight of 5,000 to 80,000 may be, for example, 5, 10, 15, 20, 25, 30, 35, or 40% by mass, or may be within a range between any two of the values ​​exemplified herein.

[0108] The chloroprene polymer composition according to one embodiment of the present invention preferably contains 60 to 95% by mass of a polymer having a weight average molecular weight of 200,000 to 1,500,000, based on 100% by mass of the polymer contained in the chloroprene polymer composition. The content of the polymer having a weight average molecular weight of 200,000 to 1,500,000 is, for example, 60, 65, 70, 75, 80, 85, 90, or 95% by mass, and may be within the range between any two of the values ​​exemplified herein.

[0109] In the chloroprene polymer composition of one embodiment of the present invention, the recovery rate of the chloroprene polymer composition in the polymerization step of the chloroprene polymer B is preferably 95.0% by mass or more. The recovery rate is, for example, 95.0, 95.5, 96.0, 96.5, 97.0, 97.5, 98.0, 98.5, 99.0, 99.5, or 100.0% by mass, and may be within the range between any two of the values ​​exemplified herein.

[0110] The chloroprene polymer composition of one embodiment of the present invention is polymerized in the presence of a diene polymer A to obtain a chloroprene polymer B, and the adhesion of the chloroprene polymer composition to the polymerization container is reduced, thereby improving the recovery rate. In addition, the recovery rate of the chloroprene polymer composition in the polymerization step of the chloroprene polymer B can be obtained by the method described in the Examples.

[0111] The tensile strength at break of a dip-molded article obtained using the chloroprene polymer composition according to one embodiment of the present invention is preferably 18.0 MPa or more, more preferably 19.0 MPa or more, as measured in accordance with JIS K 6251. The tensile strength at break is, for example, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, and may be within the range between any two of the values ​​exemplified herein.

[0112] In the chloroprene polymer composition of one embodiment of the present invention, the modulus of a dip molded article obtained using the chloroprene polymer composition at 100% elongation measured in accordance with JIS K 6251 is preferably 0.65 MPa or less, more preferably 0.60 MPa or less. The modulus at 100% elongation is, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, or 0.65 MPa, and may be within the range between any two of the values ​​exemplified herein.

[0113] In addition, the dip-molded article obtained by using the chloroprene polymer composition can be obtained through a dip-molding step and a drying step. In the dip-molding step, the dip-molded article is dip-molded by a composition containing the chloroprene polymer composition, and the dip-molded article is obtained. In the drying step, the dip-molded article is dried by heating at 140°C for 1 hour to obtain the dip-molded article. The dip-molded article composition contains the chloroprene polymer composition and may also contain necessary reagents such as metal oxides and antioxidants, and may be specifically formulated as in the examples. The dip-molded article may contain diene polymer A and chloroprene polymer B as base polymers. When the dip-molded article is set to 100% by mass, it may contain 70% by mass or more of diene polymer A and chloroprene polymer B, preferably 80% by mass or more, and more preferably 90% by mass or more. When the dip molded product is taken as 100 mass %, the content of the diene polymer A and the chloroprene polymer B in the dip molded product is, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, or 100 mass %, and may be within the range between any two of the values ​​exemplified here.

[0114] The tensile strength at break and the modulus at 100% elongation of the dip molded article containing the chloroprene polymer composition can be controlled by adjusting the weight average molecular weight, the type and content of the monomer units contained in the diene polymer A and the chloroprene polymer B contained in the dip molded article, the polymerization conditions of each polymer, the blending ratio, etc. In addition, the method for measuring the tensile strength at break and the modulus at 100% elongation can be described in the Examples.

[0115] 2. Method for manufacturing dip-molded article

[0116] The method for producing a dip-molded article according to one embodiment of the present invention may include:

[0117] a dip molding step of dip molding a composition for forming a dip molded body containing the above-described chloroprene polymer composition to obtain a dip molded body; and

[0118] In the drying step, the impregnation molded body is heated and dried to obtain an impregnation molded article.

[0119] 2.1 Composition for forming an impregnated molded body

[0120] The composition for forming a dip molded body according to one embodiment of the present invention contains the chloroprene polymer composition described above. The composition for forming a dip molded body according to one embodiment of the present invention may contain a metal oxide, an antioxidant, and other necessary reagents in addition to the chloroprene polymer composition. The composition for forming a dip molded body according to one embodiment of the present invention may not contain a vulcanizing agent and a vulcanization accelerator, and may not contain sulfur and a vulcanization accelerator such as a thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, thiazole-based, etc.

[0121] 2.1.1 Metal oxides

[0122] The composition for forming an impregnation molded body according to one embodiment of the present invention may contain a metal oxide.

[0123] The metal oxide is not particularly limited, and zinc oxide, lead oxide, lead tetraoxide, magnesium oxide, aluminum oxide, iron oxide, beryllium oxide, titanium oxide, etc. can be cited. The metal oxide preferably contains zinc oxide. Zinc oxide is generally considered to function as a supplement for the dechlorination of chloroprene polymers. In addition, these metal oxides can be used alone or in combination of two or more.

[0124] The amount of the metal oxide added is preferably 0.5 to 15.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming the dip molded body. If the amount of the metal oxide added is 0.5 parts by mass or more, an improvement in the tensile strength at break can be expected due to the crosslinking effect between the polymers. If the amount of the metal oxide added is 15.0 parts by mass or less, a dip molded product with excellent flexibility can be obtained. In addition, from the viewpoint of the physical balance between the flexibility and tensile strength at break of the obtained dip molded product, the amount of the metal oxide added is more preferably 0.5 to 5.0 parts by mass.

[0125] 2.1.2 Antioxidants

[0126] The composition for forming a dip molded article according to one embodiment of the present invention may also contain an antioxidant. The antioxidant is not particularly limited, and phenolic antioxidants, amine antioxidants, heat-resistant antioxidants (aging) agents, ozone-resistant antioxidants, etc. can be used. When the obtained dip molded article is used for medical gloves, a phenolic antioxidant can be used from the viewpoint of color tone, texture, and sanitation of the dip molded article. In particular, hindered phenolic antioxidants have a strong effect as described above. As hindered phenol antioxidants, for example, 2,2'-methylenebis(4-ethyl-6-tert-butylphenol), 2,2'-methylenebis(4-methyl-6-tert-butylphenol), 4,4'-butylene(3-methyl-6-tert-butylphenol), 4,4'-thiobis(3-methyl-6-tert-butylphenol), butylated reaction products of p-cresol and dicyclopentadiene, 2,5'-di-tert-butylhydroquinone, and 2,5'-di-tert-amylhydroquinone can be cited. Among them, butylated reaction products of p-cresol and dicyclopentadiene are generally preferred from the viewpoint of being dispersible in aqueous materials. In addition, these compounds may be used alone or in combination of two or more.

[0127] The amount of the antioxidant added is preferably 0.5 to 10.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming a dip molded body. The amount of the antioxidant added is, for example, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0 parts by mass, or it may be within the range between any two of the values ​​exemplified herein. If the amount of the antioxidant added is 0.5 parts by mass or more, the effect of suppressing the change in color tone of the dip molded product can be obtained. If the amount of the antioxidant added is 10.0 parts by mass or less, the stability of the composition for forming a dip molded product can be ensured. In addition, from the viewpoint of the balance of the physical properties of the softness and tensile strength at break of the obtained dip molded product, the amount of the antioxidant added is more preferably 0.5 to 5.0 parts by mass.

[0128] 2.1.3 Vulcanizing agents and vulcanization accelerators

[0129] The composition for forming a dip molded body according to one embodiment of the present invention may also contain a vulcanizing agent and / or a vulcanization accelerator. In addition, the composition for forming a dip molded body according to one embodiment of the present invention may also be free of sulfur and the above-mentioned thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, thiazole-based and other vulcanization accelerators. That is, the composition for forming a dip molded body includes a composition containing a vulcanizing agent but not containing a vulcanization accelerator, a composition containing no vulcanizing agent but containing a vulcanization accelerator, a composition containing a vulcanizing agent and a vulcanization accelerator, and a composition containing no vulcanizing agent and a vulcanization accelerator. Whether to prepare a vulcanizing agent and a vulcanization accelerator can be determined according to the expected dip molded product.

[0130] Examples of the vulcanizing agent include sulfur, but are not limited thereto. The amount of the vulcanizing agent added may be 0 to 10.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming the dip molded body. The amount of the vulcanizing agent added may be, for example, 0, 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10 parts by mass, or may be within the range between any two of the values ​​exemplified herein.

[0131] Vulcanization accelerator refers to a reagent added during the vulcanization of raw rubber to increase the vulcanization rate by reacting with the vulcanizing agent, shorten the vulcanization time, lower the vulcanization temperature, reduce the vulcanizing agent, and improve the physical properties of the vulcanized rubber. It usually refers to a reagent that promotes sulfur vulcanization reaction.

[0132] Examples of the vulcanization accelerator include, but are not limited to, thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, and thiazole-based accelerators, which may be used alone or in combination of two or more as needed.

[0133] Examples of the thiuram-based vulcanization accelerator include tetramethylthiuram disulfide, tetraethylthiuram disulfide, tetrabutylthiuram disulfide, tetrakis(2-ethylhexyl)thiuram disulfide, tetramethylthiuram monosulfide, and bis(pentamethylene)thiuram tetrasulfide.

[0134] Examples of the dithiocarbamate-based vulcanization accelerator include sodium dibutyldithiocarbamate, zinc dimethyldithiocarbamate, zinc diethyldithiocarbamate, zinc N-ethyl-N-phenyldithiocarbamate, zinc N-pentamethylenedithiocarbamate, copper dimethyldithiocarbamate, iron (III) dimethyldithiocarbamate, tellurium diethyldithiocarbamate, and the like. Zinc dibutyldithiocarbamate is particularly preferably used.

[0135] Examples of the thiourea-based vulcanization accelerator include ethylenethiourea, N,N′-diethylthiourea, trimethylthiourea, and N,N′-diphenylthiourea.

[0136] Examples of the guanidine-based vulcanization accelerator include 1,3-diphenylguanidine, 1,3-di-o-tolylguanidine, 1-o-tolylbiguanide, and di-o-tolylguanidine salt of dicatechol borate.

[0137] Examples of the xanthate-based vulcanization accelerator include butyl zinc xanthate and isopropyl zinc xanthate.

[0138] Examples of the thiazole vulcanization accelerator include 2-mercaptobenzothiazole, di-2-benzothiazole disulfide, 2-mercaptobenzothiazole zinc salt, cyclohexylamine salt of 2-mercaptobenzothiazole, and 2-(4′-morpholinodithio)benzothiazole.

[0139] The amount of the vulcanization accelerator added may be 0 to 5.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming a dip molded body. The amount of the vulcanization accelerator added may be, for example, 0, 0.5, 1.0, 1.5, 2.0, 2.5, 3.0, 3.5, 4.0, 4.5, 5.0, or may be within the range between any two of the values ​​exemplified herein.

[0140] 2.1.4 Other reagents (aromatic heterocyclic compounds)

[0141] The composition for forming a dip molded article according to one embodiment of the present invention may contain an aromatic heterocyclic compound in the chloroprene polymer.

[0142] The aromatic heterocyclic compound contained in the dip-molded article forming composition for obtaining the dip-molded article of one embodiment of the present invention can be represented by chemical formula (1) and has a benzimidazole structure. In addition, the compound having this structure is sometimes mainly used as a secondary antioxidant in the preparation of the rubber composition.

[0143] [Chemistry 1]

[0144]

[0145] In the chemical formula (1), X of the mercapto group represents a hydrogen atom or a metal atom. X may be a group having a thiol group and a hydrogen atom. In addition, X may be a metal atom, and examples of the metal atom include zinc, sodium, copper, nickel, and tellurium, and zinc is preferred.

[0146] R in the chemical formula (1) 1 ~R 4 Each of R represents a hydrogen atom, an alkyl group which may have a substituent, an ether group which may have a substituent, a nitro group, an amino group, or a carboxyl group. 1 ~R 4 The aromatic heterocyclic compounds may be used alone or in combination of two or more.

[0147] As aromatic heterocyclic compounds, for example, 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, 5-nitro-2-mercaptobenzimidazole, 5-amino-2-mercaptobenzimidazole, 5-carboxyl-2-mercaptobenzimidazole, or zinc salts of 2-mercaptobenzimidazole can be cited. Among them, 2-mercaptobenzimidazole, 5-methyl-2-mercaptobenzimidazole, 4-methyl-2-mercaptobenzimidazole, 5-methoxy-2-mercaptobenzimidazole, 4-methoxy-2-mercaptobenzimidazole, and zinc salts of 2-mercaptobenzimidazole are preferred.

[0148] The amount of the aromatic heterocyclic compound added is preferably 0.2 to 10.0 parts by mass relative to 100 parts by mass of the solid content of the chloroprene polymer composition contained in the composition for forming a dip molded body. The amount of the aromatic heterocyclic compound added is, for example, 0.2, 0.3, 0.4, 0.5, 1.0, 2.0, 3.0, 4.0, 5.0, 6.0, 7.0, 8.0, 9.0, 10.0 parts by mass, or it may be in the range between any two of the values ​​exemplified herein. If the amount added is 0.2 parts by mass or more, the dip molded product obtained using the composition can exhibit very high fracture strength. If the amount added is 10.0 parts by mass or less, the stability of the composition for forming a dip molded body can be ensured. In addition, from the viewpoint of the balance of the physical properties of the softness and fracture strength of the obtained dip molded product, the amount added is more preferably 0.3 to 5.0 parts by mass.

[0149] The method for producing a composition for forming an impregnated molded article according to one embodiment of the present invention may include a raw material mixing step of mixing raw materials containing a chloroprene polymer composition, a metal oxide, an antioxidant, and other necessary reagents.

[0150] In the mixing step, an aqueous dispersion containing the metal oxide, antioxidant and other necessary reagents may be prepared in advance, and then the chloroprene polymer composition and the aqueous dispersion may be mixed.

[0151] The mixing step can be performed using a known mixing device such as a ball mill.

[0152] 2.2 Dipping molding steps

[0153] The method for producing a dip-molded article according to one embodiment of the present invention may include a dip-molding step of obtaining a dip-molded article by dip-molding a composition for forming a dip-molded article containing a chloroprene polymer composition obtained by the method for producing a chloroprene polymer composition described above.

[0154] As the method of dip molding of one embodiment of the present invention, for example, dip coagulation method, simple dip method, thermosensitive dip method, electrodeposition method etc. can be cited. From the viewpoint of easy manufacture and easy acquisition of a certain thickness of dip molded body, dip coagulation method can be used. Specifically, the ceramic forming mold coated with calcium system coagulation liquid is immersed in the dip molded body forming composition, and the dip molded body forming composition is solidified. Then, it is dried after removing water-soluble impurities by leaching, and then formed into dip molded film (rubber coating) by heating and vulcanization, and then the dip molded film is demoulded. Thus, a film-like dip molded body can be obtained.

[0155] 2.3 Drying step

[0156] The method for producing a dip-molded article according to one embodiment of the present invention may include a drying step of heating and drying the dip-molded body to obtain the dip-molded article.

[0157] The heat drying temperature can be appropriately set according to the composition of the chloroprene polymer composition, and can be 120 to 180° C. The heating temperature is preferably 120 to 150° C. The heating temperature is, for example, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220° C., and can also be within the range between any two values ​​exemplified herein. The heating time can be appropriately set according to the composition of the chloroprene polymer composition, the shape of the unvulcanized molded body, etc., and can be 10 to 300 minutes. The heating time is, for example, 10, 20, 30, 40, 50, 60, 70, 80, 90, 100, 110, 120, 130, 140, 150, 160, 170, 180, 190, 200, 210, 220, 230, 240, 250, 260, 270, 280, 290, 300 minutes, and may be within the range between any two values ​​exemplified herein. As an example, the dip molded article according to one embodiment of the present invention may be subjected to a heat drying treatment at 140° C. for 1 hour.

[0158] 3. Dip-molded products (dip-molded films and films)

[0159] The dip-molded article of one embodiment of the present invention is obtained using the above-mentioned chloroprene polymer composition. The dip-molded article can be obtained by dip-molding the above-mentioned dip-molded article forming composition alone or by mixing it with other dip-molded article forming compositions. The dip-molded article of the present invention can be a dip-molded article obtained by heat-drying the dip-molded article obtained by dip-molding the dip-molded article forming composition using the dip coagulation method at 140°C for 1 hour. The dip-molded article of the present invention has a high tensile strength at break and a low modulus at 100% elongation. In addition, the recovery rate of the dip-molded article from the polymerization container is high, so it can be produced with good efficiency. The dip-molded article of one embodiment of the present invention can be suitable for use as industrial / general household gloves, medical gloves, balloons, catheters and boots.

[0160] The dip molded article of the present invention may have the components contained in the above-mentioned dip molded article forming composition. In addition, the dip molded article may contain diene polymer A and chloroprene polymer B as base polymers, and when the dip molded article is set to 100% by mass, it may contain 70% by mass or more of diene polymer A and chloroprene polymer B, preferably 80% by mass or more, and more preferably 90% by mass or more. When the dip molded article is set to 100% by mass, the content of diene polymer A and chloroprene polymer B in the dip molded article is, for example, 70, 75, 80, 85, 90, 95, 96, 97, 98, 99, 100% by mass, and may also be within the range between any two values ​​exemplified herein.

[0161] The dip molded article containing the chloroprene polymer of the present invention has a high tensile strength at break and a low modulus at 100% elongation, regardless of whether a vulcanizing agent and a vulcanization accelerator are added. In addition, the dip molded article of one embodiment of the present invention may not contain a vulcanizing agent and a vulcanization accelerator, and may not contain sulfur and a vulcanization accelerator such as a thiuram-based, dithiocarbamate-based, thiourea-based, guanidine-based, xanthate-based, thiazole-based, or other vulcanization accelerator.

[0162] 3.1 Characteristics of impregnated products

[0163] The dip molded product of one embodiment of the present invention preferably has a peak with a weight average molecular weight of 5,000 to 80,000 and a peak with a weight average molecular weight of 200,000 to 1,500,000 in the molecular weight distribution obtained by dissolving the dip molded product in tetrahydrofuran by gel permeation chromatography, more preferably has a peak with a weight average molecular weight of 5,000 to 50,000 and a peak with a weight average molecular weight of 300,000 to 1,500,000, and further preferably has a peak with a weight average molecular weight of 8,000 to 30,000 and a peak with a weight average molecular weight of 500,000 to 1,500,000. The weight average molecular weight and blending ratio of the low molecular weight component and the high molecular weight component may be as described above.

[0164] The chloroprene polymer composition of one embodiment of the present invention preferably has a tensile strength at break of 18.0 MPa or more, more preferably 19.0 MPa or more, as measured in accordance with JIS K6251. The tensile strength at break is, for example, 18.0, 19.0, 20.0, 21.0, 22.0, 23.0, 24.0, 25.0, 26.0, 27.0, 28.0, 29.0, 30.0, 31.0, 32.0, 33.0, 34.0, 35.0, 36.0, 37.0, 38.0, 39.0, or 40.0 MPa, and may be within the range between any two of the values ​​exemplified herein.

[0165] The chloroprene polymer composition of one embodiment of the present invention preferably has a chloroprene polymer-containing dip-molded article having a modulus at 100% elongation measured in accordance with JIS K6251 of 0.65 MPa or less, more preferably 0.60 MPa or less. The modulus at 100% elongation is, for example, 0.30, 0.35, 0.40, 0.45, 0.50, 0.55, 0.60, or 0.65 MPa, and may be within the range between any two of the values ​​exemplified herein.

[0166] The dip-molded article contains a chloroprene polymer and may further contain an antioxidant and a metal oxide. In addition, the dip-molded article may also contain a vulcanizing agent, a vulcanization accelerator and an anti-aging agent. The manufacturing method of the dip-molded article, the tensile strength at break and the modulus at 100% elongation can be described in the examples.

[0167] The tensile strength at break and modulus at 100% elongation of the dip molded product can be controlled by adjusting the types and amounts of raw materials used in polymerizing the diene polymer A and the chloroprene polymer B, the types and amounts of reagents used, and the polymerization conditions.

[0168] 3.2 Shape of the dip-molded product

[0169] The thickness of the dip-molded article (e.g., minimum thickness) may be 0.01 to 0.50 mm. The thickness of the dip-molded article may be, for example, 0.01, 0.05, 0.10, 0.20, 0.30, 0.40, or 0.50 mm, or may be within the range between any two of the values ​​exemplified herein. The thickness of the dip-molded article may be adjusted by the time the molding die is immersed in the composition for forming the dip-molded article, the solid content concentration of the composition for forming the dip-molded article, and the like. When the thickness of the dip-molded article is to be reduced, the immersion time may be shortened or the solid content concentration of the composition for forming the dip-molded article may be reduced.

[0170] The dip molded article may also contain sulfur or a vulcanization accelerator. However, even if the dip molded article does not contain sulfur and a vulcanization accelerator, it has mechanical properties equivalent to or better than those of a vulcanized dip molded article obtained from a composition for forming a dip molded article containing a conventional chloroprene polymer. Therefore, the chloroprene polymer composition of the present invention is suitable for use as a raw material for the dip molded article (dipping molded article) of the chloroprene polymer of the present embodiment.

[0171] The method for producing the dip-molded product according to one embodiment of the present invention may include the steps of subjecting the obtained dip-molded body to a heat drying treatment and vulcanizing the unvulcanized dip-molded body.

[0172] [Example]

[0173] Hereinafter, the present invention will be described in more detail based on examples, but the present invention is not limited to these examples.

[0174] <Preparation of Chloroprene-Based Polymer A>

[0175] (Synthesis Example A-1)

[0176] In a polymerization tank having an internal volume of 30 L, 64 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 77 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "RONDIS K-25", solid content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 3.4 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite were added. Polymerization was carried out by continuously adding a 0.35% by weight potassium persulfate aqueous solution as a polymerization initiator at a polymerization temperature of 35° C. under a nitrogen gas flow. 27 parts by mass of butadiene (monomer) was continuously added over 100 minutes when the polymerization rate of the added monomer reached 80%. When the polymerization rate of the initially added monomers and the continuously added monomers reached 91%, the addition of the potassium persulfate aqueous solution was stopped to terminate the polymerization, thereby obtaining a polymerization solution. The polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer A-1 having a solid content concentration of 60% by weight was obtained by concentration. The obtained latex was used to prepare chloroprene polymer B in Example 7. In addition, a part of the obtained latex was used to precipitate chloroprene polymer A-1 by the method described later, and used for analysis and the preparation of chloroprene polymer B in Examples 1 to 3.

[0177] (Precipitation of Chloroprene Polymer A Using Methanol)

[0178] The obtained latex of chloroprene polymer A-1 was mixed with a large amount of methanol to precipitate the rubber component (chloroprene polymer A-1), filtered and dried to obtain a sample of chloroprene polymer A-1. The obtained sample was subjected to the weight average molecular weight measurement of the chloroprene polymer. In addition, it was used to prepare chloroprene polymer B in Examples 1 to 3 described later. The analysis results are shown in Table 1. In addition, the measurement method is described later.

[0179] (Synthesis Example A-2)

[0180] The polymerization was carried out in the same manner as in Synthesis Example A-1 except that the n-dodecyl mercaptan in Synthesis Example A-1 was changed to 5.3 parts by mass. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer A-2 having a solid content concentration of 60% by weight was obtained by concentration. The obtained latex was used to precipitate chloroprene polymer A-2 in the same manner as in Synthesis Example A-1, and was used to prepare chloroprene polymer B. In addition, the weight average molecular weight of chloroprene polymer A-2 was measured in the same manner as in Synthesis Example A-1. The analysis results are shown in Table 1.

[0181] (Synthesis Example A-3)

[0182] The polymerization was carried out in the same manner as in Synthesis Example A-1 except that the n-dodecyl mercaptan in Synthesis Example A-1 was changed to 2.4 parts by mass. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer A-3 having a solid content concentration of 60% by weight was obtained by concentration. The obtained latex was used to precipitate chloroprene polymer A-3 in the same manner as in Synthesis Example A-1, and was used to prepare chloroprene polymer B. In addition, the weight average molecular weight of chloroprene polymer A-3 was measured in the same manner as in Synthesis Example A-1. The analysis results are shown in Table 1.

[0183] (Synthesis Example A-4)

[0184] The polymerization was carried out in the same manner as in Synthesis Example A-1 except that the n-dodecyl mercaptan in Synthesis Example A-1 was changed to 1.5 parts by mass. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer A-4 having a solid content concentration of 60% by weight was obtained by concentration. The obtained latex was used to precipitate chloroprene polymer A-4 in the same manner as in Synthesis Example A-1, and was used to prepare chloroprene polymer B. In addition, the weight average molecular weight of chloroprene polymer A-4 was measured in the same manner as in Synthesis Example A-1. The analysis results are shown in Table 1.

[0185] (Synthesis Example A-5)

[0186] In a polymerization tank with an internal volume of 30 L, 64 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 351 parts by mass of pure water, 92 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "RONDIS K-25", solid content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 3.4 parts by mass of n-dodecyl mercaptan, 4 parts by mass of potassium hydroxide, 2 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOLN", manufactured by Kao Corporation), and 0.5 parts by mass of sodium hydrogen sulfite were added so that the total amount of liquid added became 18 L. At a polymerization temperature of 35° C. and under a nitrogen flow, a 0.35% by weight potassium persulfate aqueous solution was continuously added as a polymerization initiator to carry out polymerization. At a point when the polymerization rate of the added monomers reached 80%, 27 parts by mass of butadiene (monomer) were continuously added over 100 minutes. When the polymerization rate of the initially added monomer and the continuously added monomer reaches 91%, the addition of the potassium persulfate aqueous solution is stopped to terminate the polymerization, thereby obtaining a polymerization solution. The obtained latex of the chloroprene polymer A-5 (solid content concentration 21.8% by mass) is used in Example 8. In addition, the chloroprene polymer A-5 is precipitated by the same procedure as in Synthesis Example A-1, and the weight average molecular weight of the chloroprene polymer A-5 is measured. The analysis results are shown in Table 1.

[0187] (Synthesis Example A-6)

[0188] In a polymerization tank having an internal volume of 30 L, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 100 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "RONDIS K-25", solid content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.03 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.04 parts by mass of thiourea dioxide were added so that the total amount of liquid added became 25 L. Polymerization was carried out at a polymerization temperature of 13° C. under a nitrogen gas stream while continuously adding a 0.35% by mass potassium persulfate aqueous solution as a polymerization initiator. When the polymerization rate reached 85%, the addition of the potassium persulfate aqueous solution was stopped to terminate the polymerization, thereby obtaining a polymerization solution. The obtained latex of chloroprene polymer A-6 (solid content concentration 41.7% by mass) was used in Example 9. In addition, chloroprene polymer A-6 was precipitated in the same procedure as in Synthesis Example A-1, and the weight average molecular weight of chloroprene polymer A-6 was measured. The analysis results are shown in Table 1.

[0189] [Table 1]

[0190]

[0191] <Preparation of Chloroprene-Based Polymer B>

[0192] (Example 1)

[0193] In a polymerization tank having an internal volume of 30 L, 1.3 parts by mass of chloroprene polymer A-12 prepared and precipitated in Synthesis Example A-1, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 87 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "RONDIS K-25", solid content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOLN", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. Polymerization was carried out at a polymerization temperature of 13° C. under a nitrogen gas stream, while continuously adding a 0.35% by mass potassium persulfate aqueous solution as a polymerization initiator. When the polymerization rate reaches 85%, 0.1 parts by weight of diethylhydroxylamine as a polymerization terminator is added to terminate the polymerization to obtain a polymerization solution. The polymerization solution is subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer B-1 (i.e., chloroprene polymer composition) with a solid content concentration of 60% by weight is obtained by concentration. The obtained chloroprene polymer composition is taken out from the polymerization tank in its entirety, and the actual weight of the chloroprene polymer composition after polymerization is measured. The recovery rate of the chloroprene polymer composition during the polymerization of chloroprene polymer B is calculated from the measured actual weight of the chloroprene polymer composition after polymerization. The calculation results are shown in Table 2. In addition, the calculation method is described below.

[0194] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and a dip-molded article for evaluation was prepared using the remaining chloroprene polymer composition.

[0195] The sampled chloroprene polymer composition was mixed with a large amount of methanol to separate the rubber component, and then filtered and dried to obtain a sample of chloroprene polymer B-1. The weight average molecular weight of chloroprene polymer B-1 was measured for the obtained sample. The analysis results are shown in Table 2. In addition, the measurement method is described below.

[0196] (Example 2, Example 3)

[0197] The polymerization was carried out in the same manner as in Example 1, with the raw material addition amounts and polymerization conditions shown in Table 2. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer B (i.e., chloroprene polymer composition) having a solid content concentration of 60% by weight was obtained by concentration. The obtained chloroprene polymer composition was taken out of the polymerization tank in its entirety, and the recovery rate of the chloroprene polymer composition during the polymerization of chloroprene polymer B was calculated in the same manner as in Example 1. The calculation results are shown in Table 2.

[0198] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and a dip-molded article for evaluation was prepared using the remaining chloroprene polymer composition.

[0199] The sampled chloroprene polymer composition was mixed with a large amount of methanol to precipitate the rubber component, and the mixture was filtered and dried to obtain a sample of chloroprene polymer B. The obtained sample was subjected to measurement of the weight average molecular weight of chloroprene polymer B. The analysis results are shown in Table 2.

[0200] (Example 4)

[0201] In a polymerization tank having an internal volume of 30 L, 21.3 parts by mass of the rubber component of the chloroprene polymer A-2 prepared in Synthesis Example A-2, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 87 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "RONDIS K-25", solid content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. Polymerization was carried out at a polymerization temperature of 13° C. under a nitrogen gas stream, while continuously adding a 0.35% by mass potassium persulfate aqueous solution as a polymerization initiator. When the polymerization rate reaches 85%, 0.1 parts by weight of diethylhydroxylamine as a polymerization terminator is added to terminate the polymerization, thereby obtaining a polymerization solution. The polymerization solution is subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer B-4 (i.e., chloroprene polymer composition) having a solid content concentration of 60% by weight is obtained by concentration. The obtained chloroprene polymer composition is taken out of the polymerization tank in its entirety, and the recovery rate of the chloroprene polymer composition during the polymerization of chloroprene polymer B is calculated by the same procedure as in Example 1. The calculation results are shown in Table 2.

[0202] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and a dip-molded article for evaluation was prepared using the remaining chloroprene polymer composition.

[0203] The sampled chloroprene polymer composition was mixed with a large amount of methanol to separate the rubber component, and then filtered and dried to obtain a sample of chloroprene polymer B-4. The weight average molecular weight of the chloroprene polymer B-4 was measured on the obtained sample. The analysis results are shown in Table 2.

[0204] (Example 5)

[0205] In a polymerization tank having an internal volume of 30 L, 21.3 parts by mass of the rubber component of the chloroprene polymer A-3 prepared in Synthesis Example A-3, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 87 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "RONDIS K-25", solid content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. Polymerization was carried out at a polymerization temperature of 13° C. under a nitrogen gas stream, while continuously adding a 0.35% by mass potassium persulfate aqueous solution as a polymerization initiator. When the polymerization rate reaches 85%, 0.1 parts by weight of diethylhydroxylamine as a polymerization terminator is added to terminate the polymerization, thereby obtaining a polymerization solution. The polymerization solution is subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer B-5 (i.e., chloroprene polymer composition) having a solid content concentration of 60% by weight is obtained by concentration. The obtained chloroprene polymer composition is taken out of the polymerization tank in its entirety, and the recovery rate of the chloroprene polymer composition during the polymerization of chloroprene polymer B is calculated by the same procedure as in Example 1. The calculation results are shown in Table 2.

[0206] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and a dip-molded article for evaluation was prepared using the remaining chloroprene polymer composition.

[0207] The sampled chloroprene polymer composition was mixed with a large amount of methanol to separate the rubber component, and then filtered and dried to obtain a sample of chloroprene polymer B-5. The weight average molecular weight of the chloroprene polymer B-5 was measured on the obtained sample. The analysis results are shown in Table 2.

[0208] (Example 6)

[0209] In a polymerization tank having an internal volume of 30 L, 21.3 parts by mass of the rubber component of the chloroprene polymer A-4 prepared in Synthesis Example A-4, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 87 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "RONDIS K-25", solid content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. Polymerization was carried out at a polymerization temperature of 13° C. under a nitrogen gas stream, while continuously adding a 0.35% by mass potassium persulfate aqueous solution as a polymerization initiator. When the polymerization rate reaches 85%, 0.1 parts by weight of diethylhydroxylamine as a polymerization terminator is added to terminate the polymerization, thereby obtaining a polymerization solution. The polymerization solution is subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer B-6 (i.e., chloroprene polymer composition) having a solid content concentration of 60% by weight is obtained by concentration. The obtained chloroprene polymer composition is taken out of the polymerization tank in its entirety, and the recovery rate of the chloroprene polymer composition containing chloroprene polymer B is calculated by the same procedure as in Example 1. The calculation results are shown in Table 2.

[0210] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and a dip-molded article for evaluation was prepared using the remaining chloroprene polymer composition.

[0211] The sampled chloroprene polymer composition was mixed with a large amount of methanol to separate the rubber component, and then filtered and dried to obtain a sample of chloroprene polymer B-6. The weight average molecular weight of the obtained sample was measured for chloroprene polymer B-6. The analysis results are shown in Table 2.

[0212] (Example 7)

[0213] In a polymerization tank having an internal volume of 30 L, 39 parts by mass of the latex of the chloroprene polymer A-1 prepared in Synthesis Example A-1, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 74 parts by mass of pure water, 13.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "RONDIS K-25", solid content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.6 parts by mass of potassium hydroxide, 0.4 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.4 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. Polymerization was carried out at a polymerization temperature of 13° C. under a nitrogen gas stream, while continuously adding a 0.35% by mass potassium persulfate aqueous solution as a polymerization initiator. When the polymerization rate reaches 85%, 0.1 parts by weight of diethylhydroxylamine as a polymerization terminator is added to terminate the polymerization, thereby obtaining a polymerization solution. The polymerization solution is subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer B-7 (i.e., chloroprene polymer composition) having a solid content concentration of 60% by weight is obtained by concentration. The obtained chloroprene polymer composition is taken out of the polymerization tank in its entirety, and the recovery rate of the chloroprene polymer composition containing chloroprene polymer B is calculated by the same procedure as in Example 1. The calculation results are shown in Table 2.

[0214] After measuring the actual weight of the latex after polymerization, 50 ml of the chloroprene-based polymer composition was sampled, and a dip-molded article for evaluation was prepared using the remaining chloroprene-based polymer composition.

[0215] The sampled chloroprene polymer composition was mixed with a large amount of methanol to separate the rubber component, and then filtered and dried to obtain a sample of chloroprene polymer B-7. The weight average molecular weight of the chloroprene polymer B-7 was measured for the obtained sample. The analysis results are shown in Table 2.

[0216] (Example 8)

[0217] In a polymerization tank with an internal volume of 30 L, 130.8 parts by mass of the latex of the chloroprene polymer A-5 prepared in Synthesis Example A-5, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 0.5 parts by mass of sodium bisulfite, and 0.03 parts by mass of thiourea dioxide were added. At a polymerization temperature of 13° C. and under a nitrogen gas flow, a 0.35% by mass potassium persulfate aqueous solution was continuously added as a polymerization initiator and polymerization was carried out. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization to obtain a polymerization solution. The polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of the chloroprene polymer B-8 (i.e., a chloroprene polymer composition) having a solid content concentration of 60% by weight was obtained by concentration. The obtained chloroprene polymer composition was taken out from the polymerization tank in its entirety, and the recovery rate of the chloroprene polymer composition during the polymerization of the chloroprene polymer B was calculated in the same manner as in Example 1. The calculation results are shown in Table 2.

[0218] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and a dip-molded article for evaluation was prepared using the remaining chloroprene polymer composition.

[0219] The sampled chloroprene polymer composition was mixed with a large amount of methanol to separate the rubber component, and then filtered and dried to obtain a sample of chloroprene polymer B-8. The weight average molecular weight of the chloroprene polymer B-8 was measured for the obtained sample. The analysis results are shown in Table 2.

[0220] (Example 9)

[0221] In a polymerization tank with an internal volume of 30 L, 1000 parts by mass of the latex of the chloroprene polymer A-6 prepared in Synthesis Example A-6, 74 parts by mass of chloroprene (monomer), 7 parts by mass of 2,3-dichloro-1,3-butadiene, 2.7 parts by mass of n-dodecyl mercaptan, 0.4 parts by mass of sodium hydrogen sulfite, and 0.03 parts by mass of thiourea dioxide were added. At a polymerization temperature of 13° C. and under a nitrogen gas flow, a 0.35% by mass potassium persulfate aqueous solution was continuously added as a polymerization initiator and polymerization was carried out. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization to obtain a polymerization solution. The polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of the chloroprene polymer B-9 (i.e., a chloroprene polymer composition) having a solid content concentration of 60% by weight was obtained by concentration. The obtained chloroprene polymer composition was completely taken out from the polymerization tank, and the recovery rate of the chloroprene polymer composition containing the chloroprene polymer B was calculated in the same manner as in Example 1. The calculation results are shown in Table 2.

[0222] After measuring the actual weight of the chloroprene polymer composition after polymerization, 50 ml of the chloroprene polymer composition was sampled, and a dip-molded article for evaluation was prepared using the remaining chloroprene polymer composition.

[0223] The sampled chloroprene polymer composition was mixed with a large amount of methanol to separate the rubber component, and then filtered and dried to obtain a sample of chloroprene polymer B-9. The weight average molecular weight of the chloroprene polymer B-9 was measured for the obtained sample. The analysis results are shown in Table 2.

[0224] (Comparative Example 1)

[0225] In a polymerization tank having an internal volume of 30 L, 91 parts by mass of chloroprene (monomer), 9 parts by mass of 2,3-dichloro-1,3-butadiene, 77 parts by mass of pure water, 17.6 parts by mass of a gum rosin-based disproportionated rosin aqueous solution (trade name "RONDIS K-25", solid content 25% by mass, manufactured by Arakawa Chemical Industries, Ltd.), 0.02 parts by mass of n-dodecyl mercaptan, 0.8 parts by mass of potassium hydroxide, 0.5 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), 0.5 parts by mass of sodium hydrogen sulfite, and 0.04 parts by mass of thiourea dioxide were added. At a polymerization temperature of 13° C. and under a nitrogen gas flow, a 0.35% by mass potassium persulfate aqueous solution was continuously added as a polymerization initiator to carry out polymerization. When the polymerization rate reached 85%, 0.1 parts by mass of diethylhydroxylamine as a polymerization terminator was added to terminate the polymerization to obtain a polymerization liquid. The polymerization liquid was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer C (i.e., chloroprene polymer composition) having a solid content concentration of 60% by weight was obtained by concentration. The obtained chloroprene polymer composition was taken out from the polymerization tank in its entirety, and the recovery rate of the chloroprene polymer composition of chloroprene polymer C was calculated by the same procedure as in Example 1. The calculation results are shown in Table 3. In addition, the obtained chloroprene polymer composition was used to prepare an evaluation dip molded article. In addition, a portion of the obtained chloroprene polymer composition was used in Comparative Example 2.

[0226] (Comparative Example 2)

[0227] The polymerization was carried out in the same manner as in Synthesis Example A-1. The obtained polymerization solution was subjected to reduced pressure distillation to remove unreacted monomers, and a latex of chloroprene polymer D (i.e., chloroprene polymer composition) having a solid content concentration of 60% by weight was obtained by concentration. The obtained chloroprene polymer composition was taken out of the polymerization tank in its entirety, and the recovery rate of the chloroprene polymer composition was calculated in the same manner as in Example 1. The calculation results are shown in Table 3.

[0228] The chloroprene polymer composition of chloroprene polymer C obtained in Comparative Example 1 and the chloroprene polymer composition of chloroprene polymer D were mixed at a weight ratio of C / D = 80 / 20 to obtain a chloroprene polymer composition of chloroprene polymer E. A dip molded article for evaluation was prepared using the obtained chloroprene polymer composition.

[0229] The chloroprene polymers A and B were analyzed by the following method.

[0230] <Measurement of Weight Average Molecular Weight of Chloroprene Polymers A and B>

[0231] As described above, the weight average molecular weight is measured by gel permeation chromatography (GPC) under the following measurement conditions using a sample obtained by dissolving a latex of a chloroprene polymer A and a latex containing a chloroprene polymer (i.e., a chloroprene polymer composition) in 20 ml of tetrahydrofuran, respectively, after precipitating the polymers with methanol, filtering and drying.

[0232] Device name: HLC-8320 (manufactured by Tosoh Corporation)

[0233] Chromatographic columns: 3 TSKgel GMHHR-H connected in series

[0234] Temperature: 40℃

[0235] Detection: Differential Refractive Index

[0236] Solvent: Tetrahydrofuran

[0237] Calibration curve: Prepared using standard polystyrene (PS).

[0238] The recovery rate of the chloroprene-based polymer composition was evaluated by the following method.

[0239] <Recovery Rate of Chloroprene-Based Polymer Composition>

[0240] The recovery rate of the chloroprene polymer composition was calculated according to the following formula from the actual weight of the chloroprene polymer composition after polymerization when the chloroprene polymer composition obtained in each example and comparative example was taken out from the pipe at the bottom of the polymerization tank and the amount of the chloroprene polymer composition added during polymerization. When the chloroprene polymer composition was taken out from the pipe at the bottom of the polymerization tank, the greater the viscosity of the chloroprene polymer composition, the more chloroprene polymer composition adhered to the wall of the polymerization tank, and the smaller the recovery amount. In addition, the theoretical weight is obtained by subtracting the amount removed from the system by the vacuum distillation removal operation of unreacted monomers and the concentration operation from the added amount, which represents the amount of the chloroprene polymer composition existing in the polymerization tank just before the recovery operation from the polymerization tank is performed.

[0241] (Recovery rate of chloroprene polymer composition) = (actual weight of chloroprene polymer composition) / (theoretical weight of chloroprene polymer composition) × 100

[0242] The latex, that is, the composition for forming a dip-molded article containing a chloroprene-based polymer composition was prepared by the following method, the composition was dip-molded to obtain a dip-molded article, and the dip-molded article was further subjected to a heat drying treatment to produce a dip-molded article and evaluated.

[0243] <Production of Dip Molded Articles>

[0244] 100 parts by mass of the solid content of the chloroprene polymer composition containing each chloroprene polymer was mixed with 7.1 parts by mass of the aqueous dispersion, and water was added to adjust the total solid content concentration of the formulation to 30% by mass to prepare a composition for forming an impregnated molded body. The aqueous dispersion was prepared by mixing 2 parts by mass of type 2 zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 0.7 parts by mass of 2-mercaptobenzimidazole (trade name "Nocrac MB", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) as an aromatic heterocyclic compound, 0.1 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and 10.7 parts by mass of water at 20° C. for 16 hours using a ceramic ball mill. The obtained composition for forming a dip molded body contained 2 parts by mass of type 2 zinc oxide, 2 parts by mass of a butylated reaction product of p-cresol and dicyclopentadiene (trade name "Nocrac PBK", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.), 0.7 parts by mass of 2-mercaptobenzimidazole (trade name "Nocrac MB", manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) as an aromatic heterocyclic compound, 0.1 parts by mass of a sodium salt of a β-naphthalenesulfonic acid formalin condensate (trade name "DEMOL N", manufactured by Kao Corporation), and 10.7 parts by mass of water, relative to 100 parts by mass of the solid content of the chloroprene polymer composition.

[0245] A ceramic cylinder with an outer diameter of 50 mm (manufactured by Shinko Co., Ltd.) was immersed in a coagulation solution prepared by mixing 62 parts by mass of water, 35 parts by mass of potassium nitrate tetrahydrate, and 3 parts by mass of calcium carbonate for 1 second and then taken out. After drying for 3 minutes, it was immersed in the composition for forming an impregnated molded body prepared according to the above procedure for 2 minutes. Then, it was washed with running water at 45°C for 1 minute and dried at 140°C for 1 hour to prepare an impregnated molded film for evaluation.

[0246] (film thickness)

[0247] The thickness (film thickness) of the dip-molded film for evaluation of tensile properties was measured at three locations in the center using a test piece thickness meter (manufactured by Kobun Keiki Co., Ltd., trade name: ASKER SDA-12), and the minimum thickness was taken as the thickness of the dip-molded film for evaluation. The results are shown in Tables 2 and 3.

[0248] (Determination of tensile properties)

[0249] Using the dip-molded film for evaluating tensile properties, the modulus at 100% elongation and the tensile strength at break were measured in accordance with JIS K 6251. The results are shown in Tables 2 and 3.

[0250] [Table 2]

[0251]

[0252] [Table 3]

[0253]

Claims

1. A method for producing a chloroprene polymer composition, wherein: The chloroprene polymer composition comprises a diene polymer A and a chloroprene polymer B. The diene polymer A and the chloroprene polymer B have different weight average molecular weights, The method for producing the chloroprene-based polymer composition includes a polymerization step of obtaining the chloroprene-based polymer B by polymerization in the presence of the diene-based polymer A.

2. The method for producing a chloroprene polymer composition according to claim 1, wherein The difference between the weight average molecular weight of the diene polymer A and the weight average molecular weight of the chloroprene polymer B is 100,000 or more.

3. The method for producing a chloroprene polymer composition according to claim 1 or 2, wherein: The diene polymer A has a weight average molecular weight of 5,000 to 80,000.

4. The method for producing a chloroprene polymer composition according to any one of claims 1 to 3, wherein In the polymerization step of polymerizing the chloroprene polymer B, the amount of the diene polymer A added is 5.0 to 60.0 parts by mass based on 100 parts by mass of the chloroprene monomer or the raw material monomer.

5. The method for producing a chloroprene polymer composition according to any one of claims 1 to 4, wherein The diene polymer A is at least one selected from natural rubber, isoprene polymers, butadiene polymers, styrene butadiene polymers, chloroprene polymers, and acrylonitrile butadiene polymers.

Citation Information

Patent Citations

  • Polychloroprene latex, polychloroprene latex composition, and dip molded product

    JP2014114342A

  • Polyisoprene / polychloroprene composition

    JP2017508840A

  • Chloroprene polymer latex and manufacturing method therefor

    JP2019143002A

  • Elastomeric article

    JP2020189963A

  • Mercaptane-modified polychloroprene latex and production method therefor

    WO2019009038A1