Probe

By using alloy materials of Pd, Ag, Ni and Cu with specific composition ratios, the problem of contact resistance variation caused by probe component diffusion was solved, thereby improving probe durability and the stability of the inspection process.

CN118946678APending Publication Date: 2024-11-12YOKOWO CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030120.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-29
Filing Date
2023-03-02
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

When the probe tip repeatedly contacts and electrically connects with the solder, the components contained in the probe are prone to diffusion, which leads to changes in contact resistance, increases the frequency of cleaning and replacement, and affects the operating rate of the inspection process.

Method used

Using alloy materials with specific proportions of Pd, Ag, Ni, and Cu, the diffusion of components is suppressed by controlling the proportions of the material composition, including 20-60% Pd, 3-20% Ag, 3-50% Ni, and 3-74% Cu, or 20-35% Ag, 7-50% Ni, and 3-53% Cu, to combine with Ni to form a dense metal compound film to prevent diffusion.

Benefits of technology

It effectively inhibits the diffusion of probe components into the solder, reduces the consumption of the probe tip, and improves the durability of the probe and the stability of the inspection process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946678A_ABST
    Figure CN118946678A_ABST
Patent Text Reader

Abstract

This probe contains more than 20 mass% and 60 mass% or less of Pd, 3 mass% or more and less than 20 mass% of Ag, 3 mass% or more and 50 mass% or less of Ni, and 3 mass% or more and 74 mass% or less of Cu.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to probes. Background Art

[0002] In order to inspect an inspection object such as an integrated circuit, the inspection object and an inspection substrate may be electrically connected via a probe provided in a socket. The probe may contain an alloy of Pd, Ag, and Cu.

[0003] An example of an alloy of Pd, Ag, and Cu is described in Patent Document 1. The alloy described in Patent Document 1 contains about 35% to 59% of Pd, 4% or more of Ag, and 16% or more and 50% or less of Cu.

[0004] Prior art literature

[0005] Patent Literature

[0006] Patent Document 1: U.S. Patent No. 1935897 Summary of the invention

[0007] Problems to be solved by the invention

[0008] Alloys of Pd, Ag, and Cu are sometimes used as materials for forming probes. However, when the tip of a probe containing an alloy of Pd, Ag, and Cu is repeatedly brought into contact with the solder of an inspection object and electrically connected, there is a tendency for components such as Sn contained in the solder and components contained in the probe to diffuse with each other due to Joule heat and other reasons. If the components contained in the probe diffuse, the tip of the probe is sometimes consumed. When the tip of the probe is consumed, the contact resistance between the probe and the solder sometimes changes. Therefore, when using a probe containing an alloy of Pd, Ag, and Cu, the number of times the tip of the probe is cleaned and replaced becomes more, and the operating rate of the inspection process is sometimes reduced.

[0009] One example of the purpose of the present invention is to suppress the diffusion of components contained in the probe into the solder. Other purposes of the present invention can be understood from the description of this specification.

[0010] Means for solving problems

[0011] One embodiment of the present invention is a probe comprising:

[0012] More than 20 mass % and 60 mass % or less of Pd;

[0013] 3 mass % or more and less than 20 mass % of Ag;

[0014] 3 mass % to 50 mass % Ni; and

[0015] A probe having a Cu content of not less than 3 mass % and not more than 74 mass %.

[0016] Another aspect of the present invention is a probe comprising:

[0017] More than 20 mass % and 60 mass % or less of Pd;

[0018] 20 mass % to 35 mass % of Ag;

[0019] 7 mass % to 50 mass % Ni; and

[0020] 3 mass % or more and 53 mass % or less of Cu.

[0021] According to the above aspect of the present invention, it is possible to suppress the components contained in the probe from diffusing into the solder. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] Figure 1 It is a cross-sectional view of the socket according to the embodiment.

[0023] Figure 2 It is a cross-sectional view of the socket according to the first modified example.

[0024] Figure 3 It is a cross-sectional view of a probe according to a second modified example. DETAILED DESCRIPTION

[0025] Hereinafter, the embodiment and modification of the present invention will be described using the drawings. In all the drawings, the same components are denoted by the same reference numerals, and the description thereof will be appropriately omitted.

[0026] In this specification, unless otherwise specified, ordinal numbers such as "1st", "2nd", and "3rd" are only used to distinguish components with the same name and do not indicate specific characteristics of the components (such as order or importance).

[0027] Figure 1 It is a cross-sectional view of the socket 10 according to the embodiment.

[0028] exist Figure 1 In the figure, the arrow indicated by "+Z" indicates the upward direction of the vertical direction, and the arrow indicated by "-Z" indicates the downward direction of the vertical direction. Hereinafter, the direction perpendicular to the vertical direction will be referred to as the horizontal direction as needed.

[0029] The socket 10 includes a probe 100 and an insulating support 200. The probe 100 is provided in a through hole formed in the insulating support 200. The probe 100 includes a first plunger 110, a second plunger 120, a tube 130, and a spring 140. Figure 1 The state where the inspection object 20 is inspected by using the probe 100 through the inspection substrate 30 is shown. Specifically, Figure 1The illustrated state is a state in which the solder balls 22 of the inspection target 20 and the pads 32 of the inspection substrate 30 are electrically connected via the probes 100 .

[0030] The tube 130 extends in the vertical direction. The spring 140 is located inside the tube 130. The probe 100 may not include the tube 130. The spring 140 is spirally wound around an imaginary axis passing through the center of the tube 130 in the vertical direction.

[0031] The first plunger 110 is located on the upper end side of the spring 140. The first plunger 110 is urged upward by the spring 140, that is, in a direction away from the second plunger 120. When the inspection object 20 is inspected through the inspection substrate 30, the first plunger 110 is connected to the inspection object 20 located above the probe 100, and the front end, that is, the upper end of the first plunger 110 contacts the solder ball 22 of the inspection object 20. Figure 1 In the example shown, the tip of the first plunger 110 has a plurality of tips arranged at equal intervals around an imaginary axis passing through the center of the first plunger 110 in the vertical direction. Figure 1 Example shown.

[0032] The second plunger 120 is located at the lower end side of the spring 140. The second plunger 120 is urged downward, i.e., in a direction away from the first plunger 110, by the spring 140. When the inspection object 20 is inspected by the inspection substrate 30, the second plunger 120 is connected to the inspection substrate 30 located below the probe 100, and the front end, i.e., the lower end, of the second plunger 120 contacts the pad 32 of the inspection substrate 30. The front end of the second plunger 120 is hemispherical. The shape of the front end of the second plunger 120 is not limited to Figure 1 Example shown.

[0033] In the first embodiment, the first plunger 110 includes a material (A). The material (A) includes more than 20 mass % and less than 60 mass % of Pd, more than 3 mass % and less than 20 mass % of Ag, more than 3 mass % and less than 50 mass % of Ni, and more than 3 mass % and less than 74 mass % of Cu. For example, at least the surface of the first plunger 110 is made of the material (A). It should be noted that, for example, the first plunger 110 may be formed entirely of the material (A). Alternatively, the material (A) may cover the surface of the first plunger 110 by a treatment such as plating. In the case where the material (A) covers the surface of the first plunger 110, the portion of the first plunger 110 covered by the material (A) may be formed of a material different from the material (A). In addition, for example, at least the portion of the first plunger 110 that contacts the solder ball 22 may also be made of the material (A). It should be noted that, for example, the material (A) may be coated only on the surface of the portion of the first plug 110 that contacts the solder ball 22 by a process such as plating.

[0034] The lower limit of the mass ratio of Pd contained in the material (A) is determined, for example, from the viewpoint of the corrosion resistance of the material (A). If the mass ratio of Pd contained in the material (A) is 20% by mass or less, the corrosion resistance of the material (A) may be insufficient. If the mass ratio of Pd contained in the material (A) is 20% by mass or less, the corrosion resistance of the material (A) may be insufficient, and therefore, the mass ratio of Pd contained in the material (A) may exceed 20% by mass. The mass ratio of Pd contained in the material (A) may be, for example, 22% by mass or more or 25% by mass or more.

[0035] The upper limit of the mass ratio of Pd contained in the material (A) is determined, for example, from the viewpoint of suppressing the diffusion of the components contained in the material (A) and the components contained in the solder such as the solder ball 22. If the mass ratio of Pd contained in the material (A) exceeds 60% by mass, it is sometimes difficult to fully suppress the diffusion of the components contained in the material (A) and the components contained in the solder. In order to fully suppress the diffusion of the components contained in the material (A) and the components contained in the solder, the mass ratio of Pd contained in the material (A) can be set to 60% by mass or less. The mass ratio of Pd contained in the material (A) can also be set to 55% by mass or less or 50% by mass, for example.

[0036] The mass ratio of Pd contained in the material (A) can be, for example, 22 mass % to 55 mass % or less. Alternatively, the mass ratio of Pd contained in the material (A) can be, for example, 25 mass % to 50 mass %.

[0037] The lower limit of the mass ratio of Ag contained in the material (A) is determined, for example, from the viewpoint of age hardening. Ag can improve the age hardening of the material (A) by combining with Pd and Cu. When the mass ratio of Ag contained in the material (A) is less than 3 mass%, the age hardening of the material (A) sometimes becomes insufficient. When the mass ratio of Ag contained in the material (A) is less than 3 mass%, the age hardening of the material (A) sometimes becomes insufficient, and therefore, the mass ratio of Ag contained in the material (A) can be set to more than 3 mass%. The mass ratio of Ag contained in the material (A) can also be set to more than 4 mass%, for example.

[0038] The upper limit of the mass ratio of Ag contained in the material (A) is determined, for example, from the viewpoint that the mass of Ag contained in the material (A) is relatively small. From the viewpoint that the mass of Ag contained in the material (A) is relatively small, the mass ratio of Ag contained in the material (A) is less than 20 mass %. The mass ratio of Ag contained in the material (A) is, for example, less than 18 mass %.

[0039] The mass ratio of Ag contained in the material (A) may be, for example, 4 mass % or more and 18 mass % or less.

[0040] The lower limit of the mass ratio of Ni contained in the material (A) is determined, for example, from the viewpoint of the mass ratio of Ag contained in the material (A) and the viewpoint of suppressing the diffusion of the components contained in the material (A) and the components contained in the solder such as the solder ball 22. In the first embodiment, the mass of Ag contained in the material (A) is relatively small, less than 20 mass%. When the mass ratio of Ag contained in the material (A) is less than 20 mass%, when the mass ratio of Ni contained in the material (A) is less than 3 mass%, it is sometimes difficult to fully suppress the diffusion of the components contained in the material (A) and the components contained in the solder. In order to fully suppress the diffusion of the components contained in the material (A) and the components contained in the solder, the mass ratio of Ni contained in the material (A) can be set to more than 3 mass%. The mass ratio of Ni contained in the material (A) can also be set to more than 5 mass% or more than 7 mass%, for example.

[0041] The upper limit of the mass ratio of Ni contained in the material (A) is determined, for example, from the viewpoint of plastic working such as cold rolling and wire drawing of the material (A). If the mass ratio of Ni contained in the material (A) exceeds 50 mass %, it is sometimes difficult to perform plastic working such as cold rolling and wire drawing of the material (A). In order to facilitate plastic working such as cold rolling and wire drawing of the material (A), the mass ratio of Ni contained in the material (A) can be set to less than 50 mass %. The mass ratio of Ni contained in the material (A) can also be set to less than 40 mass % or less than 35 mass %.

[0042] The mass ratio of Ni contained in the material (A) may be, for example, 5 mass % to 40 mass %. Alternatively, the mass ratio of Ni contained in the material (A) may be, for example, 7 mass % to 35 mass %.

[0043] The lower limit of the mass ratio of Cu contained in the material (A) is determined, for example, from the viewpoint of the hardness of the material (A). The hardness of the material (A) can be improved by an alloy of Pd and Cu. In addition, the specific resistivity of Cu becomes lower. When the mass ratio of Cu contained in the material (A) is less than 3% by mass, it is sometimes difficult to ensure sufficient hardness of the material (A). When the mass ratio of Cu contained in the material (A) is less than 3% by mass, it is difficult to ensure sufficient hardness of the material (A), so the mass ratio of Cu contained in the material (A) can be set to more than 3% by mass. The mass ratio of Cu contained in the material (A) can also be set to more than 5% by mass, more than 10% by mass or more than 15% by mass, for example.

[0044] The upper limit of the mass ratio of Cu contained in the material (A) is determined, for example, from the viewpoint of the corrosion resistance of the material (A). If the mass ratio of Cu contained in the material (A) exceeds 74 mass %, it is sometimes difficult to ensure the sufficient corrosion resistance of the material (A). If the mass ratio of Cu contained in the material (A) exceeds 74 mass %, it is sometimes difficult to ensure the sufficient corrosion resistance of the material (A), therefore, the mass ratio of Cu contained in the material (A) can be set to below 74 mass %. The mass ratio of Cu contained in the material (A) can also be set to below 70 mass %, below 60 mass % or below 50 mass %.

[0045] The mass ratio of Cu contained in the material (A) may be set to, for example, 5 mass % or more and 70 mass % or less. Alternatively, the mass ratio of Cu contained in the material (A) may be set to, for example, 10 mass % or more and 60 mass % or less. Alternatively, the mass ratio of Cu contained in the material (A) may be set to, for example, 15 mass % or more and 50 mass % or less.

[0046] The material (A) may include at least one of In, Sn, Zn and Ga instead of a part of Cu, and the total amount thereof is 0.2 mass % or more and 2.0 mass % or less.

[0047] The lower limit of the total mass ratio of at least one of In, Sn, Zn and Ga contained in the material (A) is determined, for example, from the viewpoint of the age hardening of the material (A). When the total mass ratio of the at least one element contained in the material (A) is less than 0.2 mass%, the age hardening of the material (A) is almost unchanged compared to the age hardening of the material (A) not containing the at least one element. Since the age hardening of the material (A) is almost unchanged compared to the age hardening of the material (A) not containing the at least one element, the total mass ratio of the one element contained in the material (A) can be set to 0.2 mass% or more. The total mass ratio of the one element contained in the material (A) can also be set to 0.3 mass% or more, for example.

[0048] The upper limit of the total mass ratio of at least one element among In, Sn, Zn and Ga contained in the material (A) is determined, for example, from the viewpoint of plastic processing such as cold rolling and wire drawing of the material (A). If the total mass ratio of the at least one element contained in the material (A) exceeds 2.0 mass%, it is sometimes difficult to perform plastic processing such as cold rolling and wire drawing of the material (A). Since if the total mass ratio of the at least one element contained in the material (A) exceeds 2.0 mass%, it is sometimes difficult to perform plastic processing such as cold rolling and wire drawing of the material (A), the upper limit of the total mass ratio of the at least one element contained in the material (A) can be set to less than 2.0 mass%. The total mass ratio of the at least one element contained in the material (A) can also be set to less than 1.5 mass%, for example.

[0049] The total mass ratio of at least one element among In, Sn, Zn, and Ga contained in the material (A) may be, for example, 0.3 mass % or more and 1.5 mass % or less.

[0050] In the second embodiment, the first plunger 110 includes a material (B) instead of the material (A). The material (B) includes Pd in ​​an amount of more than 20 mass % and less than 60 mass %, Ag in an amount of more than 20 mass % and less than 35 mass %, Ni in an amount of more than 7 mass % and less than 50 mass %, and Cu in an amount of more than 3 mass % and less than 53 mass %. For example, at least the surface of the first plunger 110 is made of the material (B). In the example where at least the surface of the first plunger 110 is made of the material (B), for example, the entire first plunger 110 may be made of the material (B). Alternatively, the material (B) may cover the surface of the first plunger 110 by a treatment such as plating. In the case where the material (B) covers the surface of the first plunger 110, the portion of the first plunger 110 covered by the material (B) may be made of a material different from the material (B). In addition, for example, at least the portion of the first plunger 110 that contacts the solder ball 22 may be made of the material (B). In the example where at least the portion of the first plunger 110 in contact with the solder ball 22 is made of the material (B), the material (B) may cover only the surface of the portion of the first plunger 110 in contact with the solder ball 22 by plating or the like.

[0051] The lower limit of the mass ratio of Pd contained in the material (B) is determined from the viewpoint of the corrosion resistance of the material (B), for example, similarly to the lower limit of the mass ratio of Pd contained in the material (A). From the viewpoint of the corrosion resistance of the material (B), the mass ratio of Pd contained in the material (B) can be set to more than 20 mass %. The mass ratio of Pd contained in the material (B) can also be set to, for example, 22 mass % or more or 25 mass % or more.

[0052] The upper limit of the mass ratio of Pd contained in the material (B) is determined from the viewpoint of suppressing the diffusion of components contained in the material (B) and components contained in the solder such as the solder ball 22, for example, similarly to the upper limit of the mass ratio of Pd contained in the material (A). From the viewpoint of suppressing the diffusion of components contained in the material (B) and components contained in the solder such as the solder ball 22, the mass ratio of Pd contained in the material (B) is set to 60 mass % or less. The mass ratio of Pd contained in the material (B) is, for example, 55 mass % or less or 50 mass % or less.

[0053] The mass ratio of Pd contained in the material (B) may be, for example, 22 mass % to 55 mass % or less. Alternatively, the mass ratio of Pd contained in the material (B) may be, for example, 25 mass % to 50 mass %.

[0054] The lower limit of the mass ratio of Ag contained in the material (B) is determined, for example, from the viewpoint of making the mass of Ag contained in the material (B) more. From the viewpoint of making the mass of Ag contained in the material (B) more, the mass ratio of Ag contained in the material (B) can be set to more than 20 mass%. The mass ratio of Ag contained in the material (B) can also be set to more than 21 mass%, for example.

[0055] The upper limit of the mass ratio of Ag contained in the material (B) is determined, for example, from the viewpoint of suppressing the diffusion of the components contained in the material (B) and the components contained in the solder such as the solder ball 22. If the mass ratio of Ag contained in the material (B) exceeds 35% by mass, it is sometimes difficult to fully suppress the diffusion of the components contained in the material (B) and the components contained in the solder. If the mass ratio of Ag contained in the material (B) exceeds 35% by mass, it is sometimes difficult to fully suppress the diffusion of the components contained in the material (B) and the components contained in the solder, so the mass ratio of Ag contained in the material (B) can be set to 35% by mass or less. The mass ratio of Ag contained in the material (B) can also be set to 33% by mass or less, for example.

[0056] The mass ratio of Ag contained in the material (B) may be, for example, 21 mass % or more and 33 mass % or less.

[0057] The lower limit of the mass ratio of Ni contained in the material (B) is determined, for example, from the viewpoint of the mass ratio of Ag contained in the material (B) and the viewpoint of suppressing the diffusion of the components contained in the material (B) and the components contained in the solder such as the solder ball 22. In the second embodiment, the mass ratio of Ag contained in the material (B) is more than 20 mass %. In the case where the mass ratio of Ag contained in the material (B) is more than 20 mass %, when the mass ratio of Ni contained in the material (B) is less than 7 mass %, it is sometimes difficult to fully suppress the diffusion of the components contained in the material (B) and the components contained in the solder. In order to fully suppress the diffusion of the components contained in the material (B) and the components contained in the solder, the mass ratio of Ni contained in the material (B) can be set to more than 7 mass %. The mass ratio of Ni contained in the material (B) can also be set to more than 8 mass %, more than 10 mass % or more than 11 mass %, for example.

[0058] The upper limit of the mass ratio of Ni contained in the material (B) is determined from the viewpoint of plastic working such as cold rolling and wire drawing of the material (B), for example, similarly to the upper limit of the mass ratio of Ni contained in the material (A). From the viewpoint of plastic working such as cold rolling and wire drawing of the material (B), the mass ratio of Ni contained in the material (B) can be set to 50% by mass or less. The mass ratio of Ni contained in the material (B) can also be set to 40% by mass or less or 35% by mass, for example.

[0059] The mass ratio of Ni contained in the material (B) may be set to, for example, 8% by mass or more and 40% by mass or less. Alternatively, the mass ratio of Ni contained in the material (B) may be set to, for example, 10% by mass or more and 35% by mass or less. Alternatively, the mass ratio of Ni contained in the material (B) may be set to, for example, 11% by mass or more and 35% by mass or less.

[0060] The lower limit of the mass ratio of Cu contained in the material (B) is determined from the viewpoint of the hardness of the material (B), for example, similarly to the lower limit of the mass ratio of Cu contained in the material (A). From the viewpoint of the hardness of the material (B), the mass ratio of Cu contained in the material (B) can be set to 3% by mass or more. The mass ratio of Cu contained in the material (B) can also be set to 5% by mass or more or 10% by mass or more, for example.

[0061] The upper limit of the mass ratio of Cu contained in the material (B) is determined from the viewpoint of the corrosion resistance of the material (B), for example, similarly to the upper limit of the mass ratio of Cu contained in the material (A). From the viewpoint of the corrosion resistance of the material (B), the mass ratio of Cu contained in the material (B) can be set to 53% by mass or less. The mass ratio of Cu contained in the material (B) can also be set to 47% by mass or less or 40% by mass, for example.

[0062] The mass ratio of Cu contained in the material (B) may be, for example, 5 mass % to 47 mass %. Alternatively, the mass ratio of Cu contained in the material (B) may be, for example, 10 mass % to 40 mass %.

[0063] The material (B) may include at least one of In, Sn, Zn, and Ga in place of a portion of Cu, with the total amount thereof being 0.2 mass % to 2.0 mass %.

[0064] The lower limit of the total mass ratio of at least one of In, Sn, Zn and Ga contained in the material (B) is determined from the viewpoint of age hardening of the material (B), for example, similarly to the lower limit of the total mass ratio of at least one of In, Sn, Zn and Ga contained in the material (A). From the viewpoint of age hardening of the material (B), the total mass ratio of the one element contained in the material (B) can be set to 0.2 mass % or more. The total mass ratio of the one element contained in the material (B) can also be set to 0.3 mass % or more, for example.

[0065] The upper limit of the total mass ratio of at least one of In, Sn, Zn and Ga contained in the material (B) is determined from the viewpoint of plastic working such as cold rolling and wire drawing of the material (B), for example, similarly to the upper limit of the total mass ratio of at least one of In, Sn, Zn and Ga contained in the material (A). From the viewpoint of plastic working such as cold rolling and wire drawing of the material (B), the upper limit of the total mass ratio of the at least one element contained in the material (B) can be set to 2.0 mass % or less. The total mass ratio of the at least one element contained in the material (B) can also be set to 1.5 mass % or less, for example.

[0066] The total mass ratio of at least one of In, Sn, Zn, and Ga contained in the material (B) may be, for example, 0.3 mass % to 1.5 mass %.

[0067] Hereinafter, an alloy including Pd, Ag, and Cu and not including Ni will be referred to as a PdAgCu alloy as necessary.

[0068] In the embodiment, compared with the case where the first plug 110 includes a PdAgCu alloy, it is possible to suppress the diffusion of the components included in the first plug 110 into the solder ball 22 at the interface between the tip of the first plug 110 and the surface of the solder ball 22. In addition, in the embodiment, compared with the case where the first plug 110 includes a PdAgCu alloy, it is possible to suppress the consumption of the tip of the first plug 110 by suppressing the diffusion of the components included in the first plug 110 into the solder ball 22.

[0069] In the case of using material (A), the reason for suppressing the diffusion of components contained in material (A) into the solder is presumed to be as follows, compared with the case of using PdAgCu alloy. That is, when material (A) contacts the solder, a dense film containing metal compounds such as Sn-Ni is formed at the interface between material (A) and the solder due to Ni contained in material (A). In the case where the metal compound exists at the interface between material (A) and the solder, the diffusion of components contained in material (A) and the solder is suppressed by the metal compound, compared with the case where the metal compound does not exist at the interface between material (A) and the solder. In contrast, in the case of using PdAgCu alloy, it is difficult to form the above-mentioned metal compound. Therefore, in the embodiment, compared with the case where the first plunger 110 contains PdAgCu alloy, the diffusion of components contained in the first plunger 110 into the solder ball 22 can be suppressed between the front end of the first plunger 110 and the solder ball 22. When the material (B) is used, for the same reason as described above, it is possible to suppress the diffusion of the components contained in the material (B) into the solder compared to the case of using the PdAgCu alloy.

[0070] Material (A) or material (B) does not require a hardness such as the hardness of the existing PdAgCu alloy. However, as the number of inspections increases, the contact surface of the first plunger 110 is sometimes mechanically crushed. Since the contact surface of the first plunger 110 is sometimes mechanically crushed as the number of inspections increases, it is desired that material (A) or material (B) is harder. For example, the first plunger 110 can be used at a hardness of more than 200 HV. In an embodiment, material (A) or material (B) can obtain a hardness of more than 250 HV. It should be noted that the hardness of material (A) or material (B) may also be a processed material hardness based on processing or an aged material hardness based on aging treatment.

[0071] Figure 2 1 is a cross-sectional view of a socket 10A according to a first modification. The socket 10A according to this modification is the same as the probe 100 according to the embodiment except for the following points.

[0072] An extension portion 112A extending downward from the first plunger 110A is provided at the lower end of the first plunger 110A. The first plunger 110A and the extension portion 112A are integrated. Therefore, both the first plunger 110A and the extension portion 112A include material (A) or material (B). A front end 114A is provided at the lower end of the extension portion 112A. The front end 114A may include material (A) or material (B) or may not include material (A) or material (B).

[0073] A base end 122A is provided at the upper end of the second plunger 120A. A hole 124A is formed on the upper surface of the base end 122A, which opens toward the upper side of the base end 122A. A locking portion 126A is provided at a part of the inner wall defining the hole 124A in the base end 122A. The horizontal diameter of the locking portion 126A in the hole 124A is smaller than the horizontal diameter of the portion of the hole 124A located below the locking portion 126A. The front end head 114A enters the hole 124A below the locking portion 126A. In addition, the front end head 114A is movable in the vertical direction below the locking portion 126A in the hole 124A. The horizontal diameter of the front end head 114A is larger than the horizontal diameter of the locking portion 126A in the hole 124A. Therefore, the locking portion 126A can prevent the front end head 114A from falling off toward the upper side of the hole 124A.

[0074] The probe 100A of this modified example does not have a tube corresponding to the tube 130 of the probe 100 of the embodiment. The spring 140A is located between the lower end of the first plunger 110A and the upper end of the base end 122A. In addition, the spring 140A is wound around the extension 112A in a spiral shape. The first plunger 110A, the extension 112A, and the front end 114A are urged upward by the spring 140A. The second plunger 120A and the base end 122A are urged downward by the spring 140A.

[0075] Figure 3 2 is a cross-sectional view of a probe 100B according to a second modification. The probe 100B according to the present modification is the same as the probe 100 according to the embodiment except for the following points.

[0076] exist Figure 3 In the example shown, the first plunger 110B and the tube 130B are integrated. Therefore, both the first plunger 110B and the tube 130B contain material (A) or material (B). In addition, the first plunger 110B and the tube 130B are urged upward by the spring 140B, that is, in a direction away from the second plunger 120B. The second plunger 120B is urged downward by the spring 140B, that is, in a direction away from the first plunger 110B.

[0077] As mentioned above, although embodiment and modification of this invention were demonstrated referring drawings, these are illustrations of this invention, and various structures other than what was described above can also be adopted.

[0078] Example

[0079] One embodiment of the present invention will be described based on examples and comparative examples. The present invention is not limited to the following examples.

[0080] Table 1 is a table showing the compositions (unit: mass %) of Pd, Ag, Ni, Cu, In, Sn, Zn, and Ga contained in the test materials of Examples 1 to 20 and Comparative Examples 1 to 10.

[0081]

Table 1

[0082]

[0083] The test materials of Examples 1 to 20 and Comparative Examples 1 to 10 were prepared as follows.

[0084] Regarding Example 1, as shown in Table 1, 45 mass% of Pd, 3 mass% of Ag, 10 mass% of Ni and 42 mass% of Cu were mixed to obtain a mixture. Regarding Examples 2 to 20 and Comparative Examples 1 to 10, Pd, Ag, Ni, Cu, In, Sn, Zn and Ga were mixed so as to have the compositions of Examples 2 to 20 and Comparative Examples 1 to 10 shown in Table 1 to obtain mixtures. The blank column in the composition column in Table 1 means that the metal corresponding to the blank column is not mixed.

[0085] Next, regarding Examples 1 to 20 and Comparative Examples 1 to 10, the above-mentioned mixtures were respectively melted by arc melting in an argon atmosphere to prepare alloy ingots.

[0086] Next, for Examples 1 to 20 and Comparative Examples 1 to 10, the rolling and heat treatment of the alloy ingots were repeated to prepare plates with a rolling reduction of 75%. The thickness of the alloy ingot before rolling was t1, the thickness of the alloy ingot after rolling was t2, and the rolling reduction ratio RR was determined according to the following formula (1).

[0087] RR = { (t1-t2) / t1}×100 (1)

[0088] With respect to Examples 1 to 20 and Comparative Examples 1 to 3, 5 to 8 and 10, a plate with a rolling reduction of 75% could be prepared. On the other hand, with respect to Comparative Examples 4 and 9, a plate with a rolling reduction of 75% could not be prepared. With respect to Comparative Examples 4 and 9, the measurement described in Table 2 described later was not performed.

[0089] Table 2 shows the measurement results of the resistivity of the test materials, the processed material hardness of the test materials, the aged material hardness of the test materials, and the thickness of the diffusion layer between the test materials and the solder for Examples 1 to 20 and Comparative Examples 1 to 3, 5 to 8 and 10, respectively.

[0090]

Table 2

[0091]

[0092] Regarding Examples 1 to 20 and Comparative Examples 1 to 3, 5 to 8 and 10, the resistivity of the test materials was determined by measuring the electrical resistance R of the test materials at room temperature and calculating the resistivity ρ according to the following formula (2).

[0093] ρ=RS / l (2)

[0094] Here, l is the measured length in the direction of current flow in the test material, and S is the cross-sectional area perpendicular to the direction of current flow in the test material.

[0095] As shown in Table 2, the specific resistance was 50 μΩ·cm or less in Examples 1 to 20 and Comparative Examples 1 to 3, 5 to 8, and 10. Therefore, it can be said that the specific resistance required for the probe can be obtained in Examples 1 to 20.

[0096] Regarding Examples 1 to 20 and Comparative Examples 1 to 3, 5 to 8 and 10, the workpiece hardness of each test material was measured by holding the center of the cross section of the test material at a load of 200 gf for 10 seconds using a micro Vickers hardness tester.

[0097] As shown in Table 2, the hardness of the processed material is 250 HV or more in Examples 1 to 20 and Comparative Examples 1 to 3, 5 to 8, and 10. Therefore, it can be said that the hardness required for the probe can be obtained in Examples 1 to 20.

[0098] For Examples 1 to 20 and Comparative Examples 1 to 3, 5 to 8 and 10, the aging material hardness of the test materials was measured as follows. First, each test material was aged at 300°C to 400°C for 1 hour. Next, the aging material hardness of each test material was measured by holding the center of the cross section of the test material at a load of 200 gf for 10 seconds using a micro Vickers hardness tester.

[0099] As shown in Table 2, the hardness of the aged material is 300 HV or more in Examples 1 to 20 and Comparative Examples 1 to 3, 5 to 8 and 10. Therefore, it can be said that the hardness required for the probe can be obtained in Examples 1 to 20.

[0100] For Examples 1 to 20 and Comparative Examples 1 to 3, 5 to 8 and 10, the thickness of the diffusion layer between each test material and the solder is measured as follows. First, a Sn-Bi solder is placed on a test material of 10 mm × 10 mm × 0.5 mm in thickness. Next, while the Sn-Bi solder is placed on the test material, the test material and the Si-Bi solder are heat treated at 250°C for 1 hour in an N2 atmosphere to melt the solder on the test material. Next, the test material is buried in a resin to expose a cross section containing both the test material and the solder. Next, using EPMA (Electron Probe Micro Analyzer), a line analysis is performed on the interface between the test material and the solder in a direction perpendicular to the surface of the test material on which the solder is placed. The diffusion layer is set as a layer in which both Sn diffused from the solder and Pd diffused from the test material exist. The thickness of the diffusion layer is measured based on the measurement results of EPMA.

[0101] As shown in Table 2, in Comparative Examples 1 to 3, 5 to 8, and 10, the thickness of the diffusion layer is 200 μm or more. In contrast, in Examples 1 to 20, the thickness of the diffusion layer is less than 100 μm. Therefore, compared with Comparative Examples 1 to 3, 5 to 8, and 10, it can be said that in Examples 1 to 20, the components contained in the test material can be suppressed from diffusing into the solder.

[0102] According to the results shown in Table 2, compared with the test materials of Comparative Examples 1 to 3, 5 to 8 and 10, it can be said that the test materials of Examples 1 to 20 can achieve the resistivity, processed material hardness and aging material hardness required by the probe and can inhibit the components contained in the test materials from diffusing into the solder.

[0103] According to this specification, the following aspects are provided.

[0104] (Method 1)

[0105] Mode 1 is a probe comprising:

[0106] More than 20 mass % and 60 mass % or less of Pd;

[0107] 3 mass % or more and less than 20 mass % of Ag;

[0108] 3 mass % to 50 mass % Ni; and

[0109] 3 mass % to 74 mass % Cu.

[0110] According to aspect 1, compared with the case where the probe contains no Ni but contains an alloy composed of Pd, Ag, and Cu, diffusion of components contained in the probe into the solder can be suppressed at the interface between the probe and the solder.

[0111] (Method 2)

[0112] Mode 2 is the probe according to Mode 1, wherein:

[0113] At least one of In, Sn, Zn and Ga is contained in an amount of 0.2 mass % to 2.0 mass % instead of a part of the Cu.

[0114] According to aspect 2, compared with the case where the probe contains no Ni but contains an alloy composed of Pd, Ag, and Cu, diffusion of components contained in the probe into the solder can be suppressed at the interface between the probe and the solder.

[0115] (Method 3)

[0116] Mode 3 is a probe comprising:

[0117] More than 20 mass % and 60 mass % or less of Pd;

[0118] 20 mass % to 35 mass % of Ag;

[0119] 7 mass % to 50 mass % Ni; and

[0120] 3 mass % or more and 53 mass % or less of Cu.

[0121] According to aspect 3, compared with the case where the probe includes an alloy composed of Pd, Ag, and Cu instead of Ni, diffusion of components included in the probe into the solder can be suppressed at the interface between the probe and the solder.

[0122] (Method 4)

[0123] The probe according to aspect 3, wherein at least one of In, Sn, Zn, and Ga is contained in an amount of 0.2 mass % to 2.0 mass % in substitution for a part of the Cu.

[0124] According to aspect 4, compared with the case where the probe contains no Ni but contains an alloy composed of Pd, Ag, and Cu, diffusion of components contained in the probe into the solder can be suppressed at the interface between the probe and the solder.

[0125] This application claims priority based on Japanese patent application No. 2022-052834 filed on March 29, 2022, and all the disclosed contents are incorporated herein by reference.

[0126] Description of Reference Numerals

[0127] 10, 10A socket, 20 inspection object, 22 ball, 30 inspection substrate, 32 pad, 100, 100A, 100B probe, 110, 110A, 110B first plunger, 112A extension portion, 114A front end, 120, 120A, 120B second plunger, 122A base end portion, 124A hole, 126A locking portion, 130, 130B tube, 140, 140A, 140B spring, 200 insulating support

Claims

1. A probe, It is characterized in that Include: More than 20 mass % and 60 mass % or less of Pd; 3 mass % or more and less than 20 mass % of Ag; 3 mass % to 50 mass % Ni; and 3 mass % to 74 mass % Cu.

2. The probe according to claim 1, It is characterized in that At least one of In, Sn, Zn and Ga is contained in an amount of 0.2 mass % to 2.0 mass % instead of a part of the Cu.

3. A probe, It is characterized in that Include: More than 20 mass % and 60 mass % or less of Pd; 20 mass % to 35 mass % of Ag; 7 mass % to 50 mass % Ni; and 3 mass % or more and 53 mass % or less of Cu.

4. The probe according to claim 3, It is characterized in that At least one of In, Sn, Zn and Ga is contained in an amount of 0.2 mass % to 2.0 mass % instead of a part of the Cu.