Gas diffusion electrode, fuel cell, and transport device

By forming a microporous layer containing carbon black and high aspect ratio graphite particles on the conductive porous substrate, the trade-off between the conductivity of the gas diffusion electrode and the gas diffusion property is solved, and the power generation performance and drainage properties of the fuel cell are improved , achieving more efficient gas diffusion and conductivity.

CN118946991APending Publication Date: 2024-11-12TORAY INDUSTRIES INC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380030497.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-12-21
Filing Date
2023-03-24
Publication Date
2024-11-12

AI Technical Summary

Technical Problem

There is a trade-off between insufficient conductivity and gas diffusion and conductivity in fuel cells, resulting in limited power generation performance, especially in the microporous layer structure and material selection, which hinders the conductive pathway and improves. The contradiction of gas permeability.

Method used

By forming a microporous layer on a conductive porous substrate, it contains carbon black and graphite particles with an aspect ratio of more than 10, and by adjusting the thickness, density, fluorine/carbon ratio and waterproofing agent content of the microporous layer, the graphite particles are optimized. shape and distribution to improve conductivity and gas diffusion while controlling the surface roughness and density of the microporous layer.

Benefits of technology

It achieves the reduction of resistance without damaging gas diffusion, improves the power generation performance of fuel cells, enhances the conductivity and drainage of gas diffusion electrodes, and extends the service life of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118946991A_ABST
    Figure CN118946991A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to provide a gas diffusion electrode which does not impair the gas diffusivity, reduces the resistance in the thickness direction, and improves the power generation performance when used in a fuel cell. The present invention is a gas diffusion electrode having a microporous layer on at least one surface of a conductive porous substrate, the gas diffusion electrode being characterized in that: the microporous layer contains carbon black and graphite particles having an aspect ratio of 10 or more; the thickness of the conductive porous base material into which the microporous layer is infiltrated is 5% to 20% inclusive with respect to the thickness of the conductive porous base material into which the microporous layer is not infiltrated.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a gas diffusion electrode used in a fuel cell, and more particularly to a gas diffusion electrode used in a polymer electrolyte fuel cell which is also used as a power source for a fuel cell vehicle or the like. Background Art

[0002] A fuel cell is a mechanism that extracts the energy generated when hydrogen and oxygen react to generate water in the form of electricity. It is expected to be a clean energy source because of its high energy efficiency and the only discharge is water. A solid polymer fuel cell that supplies a fuel gas containing hydrogen to the anode, an oxidizing gas containing oxygen to the cathode, and obtains an electromotive force through an electrochemical reaction at the two poles is generally composed of a separator, a gas diffusion electrode, a catalyst layer, an electrolyte membrane, a catalyst layer, a gas diffusion electrode, and a separator stacked in sequence. The electrode used in the polymer electrolyte fuel cell is sandwiched and arranged between two separators in the polymer electrolyte fuel cell, and has a structure including a catalyst layer formed on the surface of the polymer electrolyte membrane on both sides of the polymer electrolyte membrane and a gas diffusion layer formed on the outside of the catalyst layer. As an individual component for forming the gas diffusion layer in the electrode, the gas diffusion electrode is circulated. And as the performance required of the gas diffusion electrode, for example, gas diffusivity, conductivity for collecting electricity generated in the catalyst layer, and drainage for efficiently removing moisture generated on the surface of the catalyst layer can be cited. In order to obtain such a gas diffusion electrode, a conductive porous substrate having both gas diffusion capability and conductivity is generally used.

[0003] Specifically, carbon felt, carbon paper, carbon cloth, and the like formed of carbon fibers can be used as the conductive porous substrate. Among them, carbon paper is most preferred from the viewpoint of mechanical strength and the like.

[0004] In addition, since a fuel cell is a system that extracts the energy generated when hydrogen and oxygen react to produce water in the form of electricity, if the electrical load increases, that is, if the current extracted from the outside of the battery increases, a large amount of water (water vapor) is generated. If this water vapor condenses at low temperatures and becomes water droplets, it will clog the pores of the gas diffusion electrode, and the supply of gas (oxygen or hydrogen) to the catalyst layer will decrease. If all the pores are eventually clogged, power generation will stop (this phenomenon is called flooding).

[0005] In order to prevent flooding as much as possible, the gas diffusion electrode is required to have water-repellency. Generally, a gas diffusion electrode substrate obtained by subjecting a conductive porous substrate to water-repellency treatment is used to improve water-repellency.

[0006] However, if the above-mentioned conductive porous substrate subjected to water repellent treatment is directly used as a gas diffusion electrode, large water droplets are generated when water vapor condenses due to the rough texture of the fiber, which easily causes overflow. Therefore, sometimes a microporous layer is provided by coating a coating liquid in which conductive microparticles such as carbon black are dispersed on the conductive porous substrate subjected to water repellent treatment and drying and sintering the coating liquid.

[0007] Since such a microporous layer is a component constituting a gas diffusion electrode, it is required to have both gas diffusivity and conductivity in addition to water drainage, similar to the conductive porous substrate. However, it is known that the gas diffusivity and conductivity required of a gas diffusion electrode are generally in a trade-off relationship. In order to break this trade-off relationship, various measures have been taken to improve gas diffusivity and conductivity and improve power generation performance by changing the structure and materials in the microporous layer.

[0008] In patent document 1, a gas diffusion electrode for a fuel cell is proposed, wherein a microporous layer has an impregnated portion impregnated in a conductive porous substrate layer and a non-impregnated portion not impregnated in the conductive porous substrate layer, the thickness of the non-impregnated portion is less than 20.0 μm, and the thickness of the impregnated portion is less than 29% relative to the thickness of the entire microporous layer.

[0009] Patent Document 2 proposes a gas diffusion electrode characterized in that the microporous layer is formed by laminating a microporous layer sheet composed of a binder and a carbon material containing at least flaky graphite to a gas diffusion electrode substrate.

[0010] Prior art literature

[0011] Patent Literature

[0012] Patent Document 1: Japanese Patent Application Publication No. 2021-136056

[0013] Patent Document 2: Japanese Patent Application Publication No. 2013-4343 Summary of the invention

[0014] Problems to be solved by the invention

[0015] However, in the gas diffusion electrode of Patent Document 1, a large amount of water-repellent is added to the microporous layer in order to control the non-impregnation portion within the above range. The conductive path formed by the contact between the conductive fine particles is blocked by the water-repellent, resulting in insufficient conductivity.

[0016] In addition, in the gas diffusion electrode of Patent Document 2, it is recorded that flaky graphite helps to improve the gas permeability of the microporous layer in the thickness direction and the surface direction and reduce the resistance in the surface direction. However, since the sheet-like microporous layer is bonded to the gas diffusion substrate, there is a problem that the contact resistance between the gas diffusion substrate and the microporous layer sheet deteriorates the conductivity.

[0017] Therefore, an object of the present invention is to provide a gas diffusion electrode which can reduce the electrical resistance in the thickness direction without impairing the gas diffusivity and improve the power generation performance when used in a fuel cell.

[0018] Solutions to Solve Problems

[0019] The present invention adopts the following means to solve the above-mentioned problems.

[0020] (1) A gas diffusion electrode having a microporous layer on at least one side of a conductive porous substrate, characterized in that the microporous layer contains carbon black and graphite particles with an aspect ratio of 10 or more, and the thickness of the microporous layer in the conductive porous substrate is not less than 5% and not more than 20% relative to the thickness of the microporous layer in the conductive porous substrate that is not infiltrated.

[0021] (2) The gas diffusion electrode according to (1), wherein the density of the microporous layer is 0.30 g / cm 3 Above and 0.50g / cm 3 the following.

[0022] (3) The gas diffusion electrode according to (1) or (2), wherein a fluorine / carbon ratio of a surface of the conductive porous substrate on the side close to the microporous layer is 0.20 or more and 0.40 or less.

[0023] (4) The gas diffusion electrode according to any one of (1) to (3), wherein the microporous layer contains a water repellent in an amount of 0.1 mass % to 10 mass % based on 100 mass % of the entire mass of the microporous layer.

[0024] (5) The gas diffusion electrode according to any one of (1) to (4), wherein a fluorine / carbon ratio of a surface of the microporous layer that is not close to the conductive porous substrate is 0.01 to 0.20.

[0025] (6) The gas diffusion electrode according to any one of (1) to (5), wherein a fluorine / carbon ratio of a surface of the conductive porous substrate that is not close to the microporous layer is 0.01 to 0.15.

[0026] (7) The gas diffusion electrode according to any one of (1) to (6), wherein the conductive porous substrate contains 2 parts by mass or more and 10 parts by mass or less of a water repellent relative to 100 parts by mass of the conductive porous substrate.

[0027] (8) The gas diffusion electrode according to any one of (1) to (7), wherein the gas diffusivity in the in-plane direction is 50 cc / min to 150 cc / min.

[0028] (9) The gas diffusion electrode according to any one of (1) to (8), wherein the aspect ratio of the graphite particles contained in the microporous layer is 50 or more and 5000 or less.

[0029] (10) The gas diffusion electrode according to any one of (1) to (9), wherein the bulk density of the graphite particles contained in the microporous layer is 0.01 g / cm 3 Above and 0.20g / cm 3 the following.

[0030] (11) The gas diffusion electrode according to any one of (1) to (10), wherein a crystallite size of graphite particles contained in the microporous layer is 15 nm or more and 100 nm or less.

[0031] (12) The gas diffusion electrode according to any one of (1) to (11), wherein the mass of the graphite particles is 10 mass % or more and 50 mass % or less, when the total mass of the carbon black and graphite particles contained in the microporous layer is 100 mass %.

[0032] (13) The gas diffusion electrode according to any one of (1) to (12), wherein the weight per unit area of ​​the microporous layer is 10 g / m 2 Above and 30g / m 2 the following.

[0033] (14) The gas diffusion electrode according to any one of (1) to (13), wherein a surface roughness Sa of a surface of the microporous layer that is not close to the conductive porous substrate is 0.1 μm or more and 7 μm or less.

[0034] (15) A fuel cell comprising an electrolyte membrane, a catalyst layer, a separator, and the gas diffusion electrode according to any one of (1) to (14).

[0035] (16) A transport device using the fuel cell according to (15) as a power supply source.

[0036] Effects of the Invention

[0037] According to the gas diffusion electrode of the present invention, it is possible to obtain a gas diffusion electrode which has reduced electrical resistance without impairing gas diffusivity, and which can improve power generation performance when used in a fuel cell.

[0038] Brief description of the attached figure

[0039] Figure 1 is a schematic cross-sectional view of a gas diffusion electrode of the present disclosure. DETAILED DESCRIPTION

[0040] The present invention is a gas diffusion electrode having a microporous layer on at least one side of a conductive porous substrate, characterized in that the microporous layer contains carbon black and graphite particles with an aspect ratio of 10 or more, and the thickness of the microporous layer infiltrated into the conductive porous substrate is greater than 5% and less than 20% relative to the thickness of the microporous layer in the conductive porous substrate that is not infiltrated.

[0041] As the conductive porous substrate used in the gas diffusion electrode of the present invention, specifically, it is preferable to use a porous substrate containing carbon fibers such as carbon fiber fabric, carbon fiber paper, carbon fiber nonwoven fabric, carbon felt, carbon paper, carbon cloth, etc., and a metal porous substrate such as foamed sintered metal, metal mesh, mesh iron (expanded metal), etc. Among them, from the aspect of excellent corrosion resistance, it is preferable to use a porous substrate such as carbon felt, carbon paper, carbon cloth containing carbon fibers, and further, from the aspect of excellent characteristics of absorbing dimensional changes in the thickness direction of the electrolyte membrane, that is, "springiness", it is suitable to use a substrate containing resin carbide obtained by bonding a carbon fiber paper with a carbide, that is, carbon paper.

[0042] In the present invention, a microporous layer is provided on at least one side of the conductive porous substrate. The microporous layer contains carbon black and graphite particles as conductive substances, and may contain other conductive substances as required. Other conductive substances include, for example, carbon nanotubes, carbon nanofibers, short fibers of carbon fibers, graphene, etc. By including both carbon black and graphite particles in the microporous layer, the graphite particles effectively bridge the carbon black, thereby making it easy to connect conductive paths and improving the conductivity in the microporous layer.

[0043] As the conductive material in the microporous layer, carbon black is used from the viewpoint of low cost and stability of product quality. Examples of carbon black include furnace black, acetylene black, Ketjen black, channel black, lamp black, etc. Among carbon blacks, acetylene black is suitable for use because it has few impurities and is difficult to reduce the activity of the catalyst. In addition, as a standard for the content of impurities in carbon black, ash content can be cited, and carbon black with an ash content of 0.1% by mass or less is preferably used. It should be noted that the less ash content in carbon black, the more preferred, and carbon black with an ash content of 0% by mass, that is, carbon black without ash content, is particularly preferred.

[0044] The graphite particles can improve the conductivity in the microporous layer by effectively bridging the carbon black to form a conductive path. In addition, since the graphite particles are easily oriented in the microporous layer along the surface direction, the penetration of the microporous layer into the conductive porous substrate is suppressed, which helps to improve the gas diffusivity in the surface direction.

[0045] The aspect ratio of the graphite particles contained in the microporous layer of the present invention is 10 or more. If the aspect ratio of the graphite particles is 10 or more, the conductivity in the microporous layer can be improved because a conductive path in the microporous layer is effectively formed. In addition, the penetration of the microporous layer into the conductive porous substrate can be suppressed, and the gas diffusivity in the surface direction can be improved. The aspect ratio in the present invention can be obtained by observing the graphite particles in a magnified state using a scanning electron microscope, a transmission electron microscope, or the like. When the length of the long axis direction of the graphite particles in the magnified image is set as A and the length of the short axis direction is set as B, A / B is measured for any 100 graphite particles, and the average value thereof is set as the aspect ratio of the present invention.

[0046] The aspect ratio of the graphite particles is preferably 50 or more and 5000 or less. If it is 50 or more, the number of graphite particles in the microporous layer can be increased, the conductivity in the microporous layer can be improved, and the penetration of the microporous layer into the conductive porous substrate can be suppressed. It is more preferably 75 or more, and more preferably 100 or more. If it is 5000 or less, it is possible to prevent the gas diffusivity from being reduced due to the clogging of the pores in the microporous layer by the graphite particles. It is more preferably 2500 or less, and more preferably 1000 or less.

[0047] The graphite particles are preferably in the form of flakes. If the graphite particles are in the form of flakes, the aspect ratio of the graphite particles tends to be large, which can improve the conductivity in the microporous layer and inhibit the penetration of the microporous layer into the conductive porous substrate.

[0048] Examples of other graphite particle shapes include spherical, earthy, and scaly shapes.

[0049] The average particle size of the graphite particles is not particularly limited, but is preferably 3 μm or more and 20 μm or less. By setting the average particle size of the graphite particles to be 3 μm or more, the dispersibility is excellent, agglomeration is prevented, the reduction of the conductive path is suppressed, and the conductivity is more excellent. In addition, by setting the average particle size of the graphite particles to be 20 μm or less, it is possible to prevent the graphite particles from clogging the pores in the microporous layer, thereby reducing the gas diffusion or increasing the surface roughness of the microporous layer. The average particle size of the graphite particles refers to the particle size when the cumulative value in the particle size distribution measured by the laser diffraction scattering particle size distribution measurement method is 50%.

[0050] In addition, the bulk density of graphite particles is preferably 0.01 g / cm 3 Above and 0.20g / cm 3The bulk density of graphite particles is 0.20 g / cm 3 Below, more preferably 0.10 g / cm 3 As a result, the graphite particles tend to have a large aspect ratio and a small particle size, and the conductivity and gas diffusion in the microporous layer are more excellent. The bulk density of the graphite particles is 0.01 g / cm 3 More preferably, 0.05 g / cm 3 As described above, the graphite particles tend to have a small aspect ratio and a large particle size, and the contact resistance in the microporous layer can be reduced, making the resistance lower.

[0051] The crystallite size of the graphite particles is preferably 15 nm or more and 100 nm or less. The crystallite size of the graphite particles is 15 nm or more, more preferably 18 nm or more, whereby the graphitization degree of the graphite particles becomes high, and the conductivity in the microporous layer can be further improved. In addition, the crystallite size of the graphite particles is 100 nm or less, more preferably 80 nm or less, whereby the acquisition cost can be suppressed to a low level.

[0052] The mass of ash contained in the graphite particles is preferably 1 mass % or less from the viewpoint of less impurities and less reduction in catalyst activity.

[0053] When the total mass of carbon black and graphite particles contained in the microporous layer is set to 100 mass%, the mass of graphite particles is preferably 10 mass% or more and 50 mass% or less. By making the mass of graphite particles 10 mass% or more, more preferably 15 mass% or more, the conductivity in the microporous layer can be maintained higher, and the resistance of the gas diffusion electrode can be suppressed lower. In addition, the number of graphite particles oriented in the plane direction can be increased, the amount of microporous layer infiltrated into the conductive porous substrate can be suppressed, and the gas diffusivity can be further improved. On the other hand, by making the mass of graphite particles 50 mass% or less, more preferably 40 mass% or less, the viscosity of the coating liquid when forming the microporous layer can be suppressed, the amount of microporous layer infiltrated into the conductive porous substrate can be suppressed, and the reduction of gas diffusivity can be suppressed.

[0054] In addition, since drainage is required for the microporous layer, it is preferred that the microporous layer includes, in addition to carbon black and graphite particles, a water-repellent. Wherein, from the aspect of excellent corrosion resistance, it is preferred to use a fluorine-based polymer as a water-repellent. As the water-repellent included in the microporous layer, PTFE (polytetrafluoroethylene) (such as "Teflon (registered trademark)" (Chemours company system), FEP (tetrafluoroethylene-hexafluoropropylene copolymer), PFA (perfluoroalkoxy fluorinated resin), ETFA (ethylene-tetrafluoroethylene copolymer), PVDF (polyvinylidene fluoride), PVF (polyvinyl fluoride) etc. can be cited. From the viewpoint of particularly high water resistance, PTFE or FEP are preferred.

[0055] The mass of the waterproofing agent in the microporous layer is preferably 0.1% by mass or more and 10% by mass or less in the mass of the entire microporous layer 100% by mass. By making the mass of the waterproofing agent in the microporous layer 0.1% by mass or more, more preferably 1% by mass or more, relative to the mass of the entire microporous layer, the waterproofing property can be more effectively exerted. In addition, by making the mass of the waterproofing agent in the microporous layer 10% by mass or less, more preferably 9% by mass or less relative to the mass of the entire microporous layer, the reduction of conductivity in the microporous layer can be suppressed. In addition, since the density of the waterproofing agent is higher than that of carbon black, the density of the microporous layer can be suppressed to a lower level by suppressing the mass of the waterproofing agent in the microporous layer to a certain amount or less. The mass of the waterproofing agent in the microporous layer relative to the mass of the entire microporous layer can be calculated as follows, that is, the surface of the microporous layer of the gas diffusion electrode is scraped off with a spatula, and the obtained microporous layer powder is heated and sintered at 500°C for about 2 hours with an electric furnace or other equipment to decompose and remove the waterproofing agent, and the mass difference of the microporous layer powder before and after heating at this time is divided by the mass of the microporous layer powder before heating.

[0056] The microporous layer is preferably formed by applying a microporous layer-forming coating liquid on a conductive porous substrate, followed by drying and sintering. The microporous layer-forming coating liquid preferably contains, in addition to carbon black and graphite particles, a solvent and a dispersant for dispersing carbon black and graphite. In addition, other substances such as a thickener and a defoamer may be added as needed without damaging the dispersion of carbon black and graphite.

[0057] As the solvent, water is preferably used. As other solvents, for example, water-soluble organic solvents such as alcohols can be used. These solvents can be used alone or in combination of two or more.

[0058] As the dispersant, there can be mentioned nonionic surfactants such as polyoxyethylene alkyl ether, polyoxyethylene alkenyl ether, polyoxyethylene polyoxypropylene alkyl ether, polyoxyethylene phenyl ether, polyoxyethylene alkyl phenyl ether, polyoxyethylene polystyryl phenyl ether, polyoxyethylene naphthyl ether, polyoxyethylene alkylamine, polyoxyethylene alkylamide, polyoxyethylene polyoxypropylene glycol, polyoxyethylene fatty acid ester, sorbitan fatty acid ester, polyoxyethylene sorbitan fatty acid ester, polyoxyethylene glycerol ether, and one or more thereof can be used. Among them, polyoxyethylene alkyl ether, polyoxyethylene polyoxypropylene alkyl ether, polyoxyethylene alkyl phenyl ether, and polyoxyethylene polystyryl phenyl ether are preferred from the viewpoint of good dispersibility of carbon black.

[0059] In addition, the HLB value of the dispersant is preferably 10 or more and 15 or less. The HLB value is a value indicating the balance between lipophilicity and hydrophilicity in a molecule. By making the HLB value of the dispersant 10 or more, more preferably 11 or more, affinity with the solvent can be effectively obtained. In addition, by making the HLB value of the dispersant 15 or less, more preferably 14 or less, adsorption to carbon black can be effectively obtained. The HLB value can be calculated by the following calculation formula.

[0060] HLB value=(the sum of the formula weights of the hydrophilic part) / (molecular weight)×20...(formula).

[0061] As the thickener, for example, water-soluble polymers such as methyl cellulose, hydroxyethyl cellulose, hydroxypropyl cellulose, carboxymethyl cellulose, polyvinyl alcohol, polyvinyl pyrrolidone, polyethylene glycol, polyacrylic acid, polylactic acid, guar gum, xanthan gum, and starch can be used.

[0062] As the defoaming agent, polyorganosiloxane, phosphoric acid ester, etc. can be used.

[0063] The method of applying the microporous layer-forming coating liquid on the conductive porous substrate is preferably a method of applying by screen printing, rotary screen printing, jet spraying, gravure printing, gravure printing, die coater printing, bar coating, blade coating, knife coater or the like.

[0064] The microporous layer preferably has a weight per unit area of ​​10 g / m 2 Above and 30g / m 2 If the unit area weight of the microporous layer is 10 g / m 2 The above can reliably cover the surface of the conductive porous substrate, promote the back diffusion of generated water, and thus improve the power generation performance. In addition, by making the unit area weight of the microporous layer 30g / m 2 The weight per unit area of ​​the microporous layer is more preferably 26 g / m 2 Below, more preferably 24g / m 2 In addition, it is more preferably 14g / m 2 More preferably, 16 g / m 2 In addition, the gas diffusion electrode of the present invention having the microporous layer formed therein preferably has a weight per unit area of ​​30 to 90 g / m 2 .

[0065] For the gas diffusion electrode of the present invention, a microporous layer is infiltrated in at least one side of the conductive porous substrate. In the present invention, the thickness of the microporous layer infiltrated in the conductive porous substrate is 5% or more and 20% or less relative to the thickness of the microporous layer of the conductive porous substrate that is not infiltrated. In the following, sometimes the part of the conductive porous substrate into which the microporous layer is infiltrated is recorded as the infiltrated part, the part of the conductive porous substrate into which the microporous layer is not infiltrated is recorded as the non-infiltrated part, and the ratio of the thickness of the microporous layer infiltrated in the conductive porous substrate to the thickness of the microporous layer of the conductive porous substrate that is not infiltrated is recorded as the thickness of the infiltrated part / the thickness of the non-infiltrated part. By making the thickness of the infiltrated part / the thickness of the non-infiltrated part 5% or more, preferably 10% or more, the conductive path between the conductive porous substrate and the microporous layer can be ensured, and the conductivity is improved. On the other hand, by making the thickness of the infiltrated part / the thickness of the non-infiltrated part 20% or less, preferably 15% or less, the reduction in the density of the microporous layer can be suppressed, and the reduction in the conductivity in the microporous layer can be suppressed. In addition, the microporous layer infiltrated into the conductive porous substrate can be prevented from clogging the gas flow path in the conductive porous substrate, and the reduction of gas diffusivity can be suppressed. In order to make the thickness of the infiltrated portion / thickness of the non-infiltrated portion 5% or more and 20% or less, the fluorine / carbon ratio (F / C ratio) of the surface of the conductive porous substrate close to the microporous layer and / or the aspect ratio of the graphite particles in the microporous layer can be controlled.

[0066] The F / C ratio of the surface of the conductive porous substrate on the microporous layer side is preferably 0.20 or more and 0.40 or less.

[0067] By making the F / C ratio of the surface of the conductive porous substrate close to the microporous layer be 0.20 or more, more preferably 0.25 or more, the penetration of the conductive porous substrate into the microporous layer can be reduced, and the thickness of the infiltrated portion / thickness of the non-infiltrated portion can be reduced. In addition, the density reduction of the microporous layer can be suppressed, and the reduction of conductivity in the microporous layer can be suppressed. In addition, the microporous layer infiltrated into the conductive porous substrate restricts the gas flow path in the conductive porous substrate, which can prevent the diffusivity from being reduced.

[0068] In addition, by making the F / C ratio of the surface of the conductive porous substrate close to the microporous layer less than 0.40, more preferably less than 0.35, the microporous layer can be effectively infiltrated into the conductive porous substrate, and the thickness of the infiltrated portion / thickness of the non-infiltrated portion can be prevented from being excessively reduced. In addition, since the amount of the water-repellent agent with low conductivity is reduced, the conductivity of the gas diffusion electrode can be improved.

[0069] Here, the F / C ratio of the surface of the conductive porous substrate close to the microporous layer can be obtained as follows: the surface of the conductive porous substrate is magnified 2000 times for observation by a scanning electron microscope, characteristic X-rays reflected by irradiated electron beams are detected by energy dispersive X-ray analysis (EDX), the fluorine content and the carbon content are measured, and the fluorine content / carbon content is calculated.

[0070] In the present invention, the thickness of the infiltrated portion and the thickness of the non-infiltrated portion can be obtained by the following method (also using Figure 1 To be explained). First, use an ion milling device or the like to cut the gas diffusion electrode in the thickness direction, and use a scanning electron microscope to observe the cross section in the thickness direction at a magnification of 200 times and a field of view of 320μm×420μm. In the image obtained by scanning electron microscope observation, the conductive porous substrate and the microporous layer are different in shape and brightness, so they can be distinguished and observed. Since the microporous layer is infiltrated into the conductive porous substrate, the areas of the conductive porous substrate and the microporous layer are repeated in the infiltrated part. For the entire observation range, 20 points corresponding to the surface of the microporous layer 2 are taken at equal intervals in the width direction, and the straight line that is most similar to the line connecting these points is set as the outermost surface 10 of the microporous layer. The continuous part of the microporous layer from the outermost surface 10 of the microporous layer is set as the area of ​​the infiltration part, and the area of ​​the conductive porous substrate where the microporous layer is not infiltrated is set as the area of ​​the non-infiltration part. The straight line parallel to the microporous layer outermost surface 10 passing through point A on the boundary between the infiltration area and the non-infiltration area, which is closest to the outermost surface 10 of the microporous layer in the observation range, is set as the outermost surface 11 of the conductive porous substrate. At this time, sometimes there is an enclave of the conductive porous substrate observed in the infiltration area, but this is not considered as a point on the boundary. In addition, similarly, an enclave of the microporous layer observed in the non-infiltration area is not considered as a point on the boundary. For the points on the boundary between the infiltration area and the non-infiltration area, 20 points are taken at equal intervals in the width direction for the entire observation range, and a straight line parallel to the microporous layer outermost surface 10 that leaves from the microporous layer outermost surface 10 toward the conductive porous substrate side at the average value of the distance between these points and the microporous layer outermost surface 10 is set as the innermost part 12 of the microporous layer. A straight line parallel to the microporous layer outermost surface 10 and passing through point B on the surface of the conductive porous substrate opposite to the conductive porous substrate outermost surface 11 which is farthest from the microporous layer outermost surface 10 in the observation range is set as the conductive porous substrate innermost surface 13. Here, the tip end of the raised hair observed to protrude specifically on the conductive porous substrate is not set as point B. Ten or more images are observed, and the average value of the distance between the conductive porous substrate outermost surface 11 and the microporous layer innermost surface 12 in each image is set as the thickness 16 of the infiltrated portion, and the average value of the distance between the microporous layer innermost surface 12 and the conductive porous substrate innermost surface 13 is set as the thickness 17 of the non-infiltrated portion.

[0071] The thickness of the conductive porous substrate is preferably 120 μm or more and 200 μm or less. When the thickness of the conductive porous substrate is preferably 120 μm or more, and more preferably 130 μm or more, the gas diffusivity in the surface is easily improved, and the mechanical strength of the gas diffusion electrode can be improved. In addition, when the thickness of the conductive porous substrate is preferably 200 μm or less, and more preferably 160 μm or less, the conductive path is easily connected, and the conductivity can be effectively improved. The thickness of the conductive porous substrate is obtained as follows, that is, in more than 10 images obtained by observing the cross section in the thickness direction of the gas diffusion electrode using a scanning electron microscope (SEM) at a magnification of 200 times and a field of view of 320 μm×420 μm, the distance 15 between the outermost surface 11 of the conductive porous substrate and the innermost 13 of the conductive porous substrate is obtained.

[0072] In addition, the density of the conductive porous substrate is preferably 0.15 g / cm 3 Above and 0.50g / cm 3 By making the density of the conductive porous substrate 0.15 g / cm 3 The above can make the strength of the conductive porous substrate sufficient and effectively improve the durability. By making the density of the conductive porous substrate 0.50 g / cm 3 Hereinafter, it is possible to prevent the reduction in drainage performance and gas diffusivity.

[0073] In addition, the density of the microporous layer of the present invention is preferably 0.30 g / cm 3 Above and 0.50g / cm 3 As follows. The density of the microporous layer can be controlled by adjusting the thickness of the infiltration portion / the thickness of the non-infiltration portion or adjusting the content of the waterproofing agent in the microporous layer. It should be noted that the density of the microporous layer of the present invention can be calculated by dividing the mass of the microporous layer by the volume of the microporous layer. The mass of the microporous layer can be calculated by subtracting the mass of the waterproofed conductive porous substrate from the mass of the gas diffusion electrode. When measuring the mass of the conductive porous substrate in the gas diffusion electrode, it can be obtained as follows, that is, by heating and sintering the gas diffusion electrode at 500°C for about 2 hours to remove the waterproofing agent, and then blowing compressed air to remove the microporous layer from the gas diffusion electrode, thereby the mass of the conductive porous substrate can be obtained. The volume of the microporous layer can be calculated based on the area and thickness of the microporous layer. The thickness 14 of the microporous layer is obtained by taking the average value of the distance between the outermost surface 10 of the microporous layer and the innermost surface 12 of the microporous layer in more than 10 images obtained by observing the cross section in the thickness direction of the gas diffusion electrode using SEM at a magnification of 200 times and a field of view of 320μm×420μm.

[0074] By making the density of the microporous layer 0.30 g / cm 3More preferably, 0.35 g / cm 3 As described above, it is possible to prevent the conductivity from becoming insufficient due to insufficient conductive paths in the microporous layer.

[0075] On the other hand, by making the density of the microporous layer preferably 0.50 g / cm 3 Below, more preferably 0.45g / cm 3 This can suppress clogging of the pores in the microporous layer and improve the gas diffusion property of the gas diffusion electrode. In addition, by reducing the spring property of the microporous layer, it is possible to prevent the mechanical strength of the gas diffusion electrode from decreasing.

[0076] The thickness of the microporous layer of the present invention is preferably 120 μm or less. If the thickness of the microporous layer is 120 μm or less, more preferably 100 μm or less, and further preferably 80 μm or less, the gas diffusion electrode itself has excellent gas and water diffusivity (permeability, drainage), and can effectively reduce resistance. In order to cover the roughness of the conductive porous substrate, the thickness of the microporous layer is preferably 20 μm or more.

[0077] The surface roughness Sa of the surface of the microporous layer that is not close to the conductive porous substrate is preferably 7 μm or less, and more preferably 5 μm or less. Here, Sa is the arithmetic mean height in the reference area, which is calculated according to JIS B0681-2: 2018. By making the surface roughness Sa less than 7 μm, more preferably less than 5 μm, the contact area required for conduction can be ensured, and the resistance of the gas diffusion electrode can be effectively reduced. In addition, when used in a fuel cell, the adhesion with the catalyst layer is high, which can improve the power generation performance. In addition, the lower the surface roughness Sa of the microporous layer surface, the better, but from the perspective of the simplicity of the manufacturing process of the gas diffusion electrode, it is preferably 0.1 μm or more. That is, the surface roughness Sa of the surface of the microporous layer that is not close to the conductive porous substrate is preferably 0.1 to 7 μm.

[0078] In addition, the F / C ratio of the surface of the microporous layer that is not close to the conductive porous substrate is preferably 0.20 or less. The F / C ratio of the surface of the microporous layer that is not close to the conductive porous substrate can be controlled by adjusting the mass of the water-repellent in the microporous layer. By making the F / C ratio of the surface of the microporous layer that is not close to the conductive porous substrate preferably 0.20 or less, more preferably 0.14 or less, the conductivity in the microporous layer can be effectively improved. In addition, in order to fully exert the waterproof property, it is preferably 0.01 or more. That is, the F / C ratio of the surface of the microporous layer that is not close to the conductive porous substrate is preferably 0.01 to 0.20.

[0079] The conductive porous substrate used in the gas diffusion electrode of the present invention is preferably a substrate that has been subjected to a water-repellent treatment by imparting a fluororesin. As the water-repellent imparted to the conductive porous substrate, i.e., the fluororesin imparted to the conductive porous substrate, PTFE, FEP, PFA, ETFA, PVDF, PVF, etc. can be cited, and PTFE or FEP that exhibits strong water repellency is preferred.

[0080] The mass of the waterproofing agent in the conductive porous substrate is preferably 2 mass parts or more and 10 mass parts or less relative to 100 mass parts of the mass of the conductive porous substrate before waterproofing. By making the mass of the waterproofing agent 2 mass parts or more, more preferably 3 mass parts or more, the waterproof property can be effectively exerted. In addition, by making the mass of the waterproofing agent 10 mass parts or less, more preferably 7 mass parts or less, the waterproofing agent can be prevented from clogging the pores that become the diffusion path or drainage path of the gas, and the increase of the resistance can be suppressed.

[0081] The mass of the waterproofing agent in the conductive porous substrate can be calculated by subtracting the mass of the waterproofing agent in the microporous layer from the mass of the waterproofing agent in the gas diffusion electrode. The mass of the waterproofing agent in the gas diffusion electrode can be calculated based on the mass difference of the gas diffusion electrode before and after heating when the gas diffusion electrode is heated and sintered at 500°C for about 2 hours using an electric furnace or the like to decompose the waterproofing agent. The mass of the waterproofing agent in the microporous layer can be calculated based on the mass of the above-mentioned microporous layer and the mass of the waterproofing agent in the microporous layer relative to the mass of the above-mentioned microporous layer as a whole. In addition, the mass of the conductive porous substrate can be obtained as the mass after removing the waterproofing agent by heating and sintering the gas diffusion electrode at 500°C for about 2 hours, and then removing the microporous layer from the gas diffusion electrode by blowing compressed air.

[0082] As a method for waterproofing a conductive porous substrate, it is preferred to apply a dispersion containing a waterproofing agent on a conductive porous substrate. Thus, a waterproofing agent can be unevenly present near the surface of the conductive porous substrate close to the microporous layer, and the F / C ratio of the surface of the conductive porous substrate not close to the microporous layer can be reduced with less mass of the waterproofing agent. The F / C ratio of the surface of the conductive porous substrate close to the microporous layer is within the desired range, so it is easy to improve the conductivity of the gas diffusion electrode. As a coating technique for applying a waterproofing agent on a conductive porous substrate, die coating, spraying, etc. can be cited. As other processing methods, processing based on drying processes such as processing techniques for impregnating conductive porous substrates in dispersions containing waterproofing agents, and sputtering of waterproofing agents can also be applied. It should be noted that after waterproofing, a drying process and a sintering process can also be added as needed.

[0083] The F / C ratio of the surface of the conductive porous substrate not close to the microporous layer is preferably 0.01 or more and 0.15 or less. By setting the F / C ratio of the surface of the conductive porous substrate not close to the microporous layer to 0.15 or less, more preferably 0.12 or less, the conductivity of the gas diffusion electrode can be prevented from decreasing. In addition, by setting the F / C ratio of the surface of the conductive porous substrate not close to the microporous layer to 0.01 or more, the water repellency can be fully exerted.

[0084] By making the F / C ratio of the surface of the conductive porous substrate not close to the microporous layer within the above-mentioned range, and making the mass of the water-repellent agent in the conductive porous substrate relative to the mass of the conductive porous substrate within the above-mentioned range, as a result, the F / C ratio of the surface of the conductive porous substrate close to the microporous layer can be adjusted to a preferred range.

[0085] The F / C ratio of the surface of the conductive porous substrate not close to the microporous layer can be obtained by SEM and EDX in the same manner as the measurement of the F / C ratio of the surface of the conductive porous substrate close to the microporous layer.

[0086] The F / C ratio of the surface of the conductive porous substrate that is not close to the microporous layer can be controlled by adjusting the mass of the water-repellent agent in the conductive porous substrate.

[0087] The electrical resistance in the thickness direction of the conductive porous substrate is preferably 4.0 mΩcm when pressurized at 2.0 MPa. 2 If the electrical resistance of the conductive porous substrate in the thickness direction is 4.0 mΩcm when the pressure is 2.0 MPa, 2 If the density of the conductive porous substrate is greater than 10%, the density of the conductive porous substrate tends to decrease, so the gas diffusivity tends to increase.

[0088] The gas diffusion electrode of the present invention preferably has a gas diffusivity in the in-plane direction of 50 cc / min or more and 150 cc / min or less. The in-plane gas diffusivity is preferably 50 cc / min or more, more preferably 70 cc / min or more, so that the reaction gas can be fully supplied and the performance of the fuel cell can be effectively improved. In addition, the in-plane gas diffusivity is preferably 150 cc / min or less, more preferably 100 cc / min or less, so that the mechanical strength of the gas diffusion electrode can be improved.

[0089] In the present invention, a membrane electrode assembly can be formed by bonding the gas diffusion electrode to at least one side of an electrolyte membrane having a catalyst layer on both sides. By arranging the microporous layer of the gas diffusion electrode on the catalyst layer side, it is not only easy to cause the back diffusion of the generated water, but also the contact area between the catalyst layer and the gas diffusion electrode is increased, which can reduce the contact resistance, and is preferred.

[0090] The fuel cell of the present invention comprises the gas diffusion electrode of the present invention. That is, there are separators on both sides of the above-mentioned membrane electrode assembly. That is, the fuel cell is constructed by arranging separators on both sides of the above-mentioned membrane electrode assembly. Usually, a fuel cell is constructed by stacking a plurality of components sandwiched by separators via gaskets on both sides of such a membrane electrode assembly. The catalyst layer is composed of a layer containing an electrolyte and carbon carrying a catalyst. Platinum is usually used as a catalyst. The electrolyte preferably uses a perfluorosulfonic acid-based polymer material with high proton conductivity, oxidation resistance and heat resistance. The structure of such a fuel cell unit and fuel cell itself is well known.

[0091] The fuel cell of the present invention can be used as a power supply source for transportation equipment such as automobiles, ships, and railways.

[0092] Example

[0093] The present invention will be described below using Examples and Comparative Examples.

[0094] [Measurement method]

[0095] (1) Electrical resistance of the conductive porous substrate

[0096] The conductive porous substrate after waterproofing or at a comparable stage was cut into a size of 20 mm × 20 mm, and clamped with gold-plated smooth metal rigid electrodes at the top and bottom, and an average pressure of 2.0 MPa was applied. In this state, the voltage between the upper and lower electrodes when a current of 1 A was passed through the upper and lower electrodes was measured to calculate the resistance per unit area.

[0097] (2) Aspect ratio of graphite particles

[0098] The graphite particles were observed under magnification using a SEM, and the value of the length in the major axis direction / the length in the minor axis direction of 100 randomly selected graphite particles was calculated, and the average value was taken as the aspect ratio of the graphite particles.

[0099] (3) Bulk density of graphite particles

[0100] 10g of graphite particles were placed in a 1000cm 3 The volume of graphite particles (cm 3 The bulk density of graphite particles (g / cm) was calculated using the following formula: 3 ).

[0101] Bulk density of graphite particles (g / cm 3 )=10(g) / (10g volume of graphite particles (cm 3 ))…(Mode).

[0102] (4) Crystallite size of graphite particles

[0103] The crystallite size of graphite particles was measured by X-ray diffraction. In the X-ray diffraction measurement, the half-peak width of the diffraction peak originating from the (002) plane of the graphite structure was measured, and the crystallite size of the graphite particles was calculated using Scherrer's formula. As a measuring device, an X-ray diffraction device (D8 ADVANCE manufactured by BRUKER) was used.

[0104] (5) Weight per unit area of ​​solid content of microporous layer forming coating liquid

[0105] The weight per unit area of ​​the solid content of the coating liquid for forming the microporous layer (the weight per unit area of ​​the microporous layer) was obtained by subtracting the weight per unit area of ​​the waterproof conductive porous substrate from the weight per unit area of ​​the gas diffusion electrode. The weight per unit area of ​​the gas diffusion electrode and the weight per unit area of ​​the conductive porous substrate were obtained by cutting out a 10 cm square test piece and dividing the mass of the test piece by the area of ​​the test piece (0.01 m 2 ) and find the answer.

[0106] (6) Thickness of the infiltrated part / Thickness of the non-infiltrated part

[0107] For the gas diffusion electrode, a cross section perpendicular to the surface (cross section in the thickness direction) was cut out using an ion milling device (IM4000 manufactured by Hitachi High Tech Co., Ltd.), and the image was observed by SEM (S-4800 manufactured by Hitachi, Ltd.) with a magnification of 200 times. The thickness of the infiltrated portion / the thickness of the non-infiltrated portion was calculated as follows, that is, in more than 10 images obtained by observing the cross section in the thickness direction of the gas diffusion electrode using SEM with a magnification of 200 times and a field of view of 320 μm×420 μm, the average value of the distance between the outermost surface 11 of the conductive porous substrate and the innermost layer 12 of the microporous layer was set as the thickness 16 of the infiltrated portion, and the average value of the distance between the innermost layer 12 and the innermost layer 13 of the conductive porous substrate was set as the thickness 17 of the non-infiltrated portion.

[0108] (7) F / C ratio of conductive porous substrate

[0109] The surface of the conductive porous substrate was observed by SEM at a magnification of 2000 times and measured by element distribution analysis. The element distribution analysis was calculated by detecting and quantifying characteristic X-rays reflected by electron beams irradiated at an acceleration voltage of 20 kV using EDX (EX-370 manufactured by Horiba, Ltd.), thereby calculating the fluorine content and the carbon content, and calculating the fluorine content / carbon content.

[0110] (8) Density of microporous layer

[0111] The density of the microporous layer is calculated by dividing the mass of the microporous layer by the volume of the microporous layer. The volume of the microporous layer can be calculated based on the area and thickness of the microporous layer, and the mass of the microporous layer can be calculated by subtracting the mass of the conductive porous substrate that has been waterproofed from the mass of the gas diffusion electrode. The mass of the conductive porous substrate can be obtained by heating and sintering the gas diffusion electrode at 500°C for about 2 hours to remove the waterproofing agent, and then blowing compressed air to remove the microporous layer from the gas diffusion electrode. The thickness 14 of the microporous layer is obtained by the following average value, which is the average value of the distance between the outermost surface 10 of the microporous layer and the innermost 12 of the microporous layer in more than 10 images obtained by observing the cross section of the gas diffusion electrode in the thickness direction using SEM with a magnification of 200 times and a field of view of 320μm×420μm.

[0112] (9) F / C ratio of the surface of the microporous layer not close to the conductive porous substrate

[0113] The measurement was performed in the same manner as in the case of measuring the F / C ratio of the conductive porous substrate, except that the measurement object was the outermost surface 10 of the microporous layer of the gas diffusion electrode.

[0114] (10) Surface roughness of microporous layer

[0115] The gas diffusion electrode was fixed to the device using a shape measuring machine (VR-3200 manufactured by KEYENCE CORPORATION) so that the microporous layer would not float or wrinkle. 2 In the field of view, measurement is performed at any 10 points on the surface of the microporous layer, and the average value of the 10-point arithmetic mean height Sa calculated according to JIS B0681-2:2018 is set as the surface roughness of the microporous layer.

[0116] (11) Gas diffusivity in the in-plane direction of the gas diffusion electrode

[0117] The in-plane gas diffusion property was obtained by flowing nitrogen at a pressure of 5 kPa in a cross section perpendicular to the surface of the gas diffusion electrode (cross section in the thickness direction) and measuring the flow rate (cc / min). The measurement area was 8 mm in the vertical direction and 24 mm in the horizontal direction, and a gas / water vapor diffusion measuring device (MVDP-200C manufactured by Seika Industry Co., Ltd.) was used as the measuring device.

[0118] (12) Resistance of gas diffusion electrode

[0119] The measurement was performed in the same manner as in the case of measuring the resistance of the conductive porous substrate when the pressure was applied at 2.0 MPa, except that the measurement object was a gas diffusion electrode having a size of 20 mm×20 mm.

[0120] [Example 1]

[0121] (Conductive porous substrate)

[0122] Polyacrylonitrile carbon fibers ("TORAYCA (registered trademark)" T300 manufactured by Toray Industries, Ltd.) having an average diameter of 7 μm were cut into pieces having an average length of 12 mm, dispersed in water, and continuously made into paper by a wet papermaking method.

[0123] A 10% by mass aqueous solution of polyvinyl alcohol was applied as a binder to the obtained paper sheet and dried to produce a carbon fiber having a unit weight of 15 g / m 2 The amount of polyvinyl alcohol attached was 20 parts by mass relative to 100 parts by mass of the carbon fibers.

[0124] Next, a phenolic resin obtained by mixing a resol-type phenolic resin and a novolac-type phenolic resin in a non-volatile component mass ratio of 1:1 was used as a thermosetting resin, flaky graphite powder (average particle size 5 μm) was used as a carbon powder, and methanol was used as a solvent. The mass ratio of thermosetting resin (non-volatile component) / carbon powder / solvent was set to 10 / 5 / 85 and mixed and uniformly dispersed to obtain a resin composition.

[0125] Next, the carbon fiber sheet is continuously impregnated with the resin composition, and after the resin impregnation step of being clamped and squeezed by rollers, it is wound into a roll to obtain a carbon fiber sheet with a precursor. At this time, the roller is a smooth metal roller with a structure that can remove excess resin composition with a scraper. Two rollers are arranged horizontally at a certain interval, and the carbon fiber sheet with a precursor is passed horizontally between them and then pulled up vertically to adjust the total amount of resin composition attached. The amount of phenolic resin attached to the carbon fiber sheet with a precursor is 130 parts by mass relative to 100 parts by mass of carbon fiber.

[0126] In a flat press, the hot plates are set in parallel with each other, a spacer is placed on the lower hot plate, and the carbon fiber sheet with the precursor is heat treated at a hot plate temperature of 180°C for 5 minutes. After that, it is introduced into a heating furnace maintained in a nitrogen atmosphere for sintering and carbonization to obtain a conductive porous substrate. The obtained conductive porous substrate has a thickness of 140μm and a density of 0.30g / cm under a pressure of 0.15MPa. 3 .

[0127] (Waterproof processing)

[0128] The conductive porous substrate was coated with a dilute aqueous solution of a PTFE dispersion ("POLYFLON (registered trademark)" D-210C; manufactured by Daikin Industries, Ltd.; 60% by mass of PTFE in the dispersion medium (water)) using a slot die coater so that the PTFE content was 5.0 parts by mass relative to 100.0 parts by mass of the conductive porous substrate before waterproofing, and dried at 120°C to perform waterproofing. The electrical resistance of the conductive porous substrate after waterproofing was 4.6 mΩcm 2 .

[0129] (Coating liquid for forming microporous layer)

[0130] Next, acetylene black ("DENKA BLACK (registered trademark)"; manufactured by Denka Corporation) was used as carbon black, and flake graphite UP-5-α (aspect ratio: 193, bulk density: 0.06 g / cm 3 , crystallite size: 20nm, manufactured by Nippon Graphite Industries (Co., Ltd.), PTFE dispersion ("POLYFLON (registered trademark)" D-210C) as a waterproofing agent, Triton X-100 (manufactured by NACALAI TESQUE (Co., Ltd.) as a dispersant, and purified water are used to prepare a coating solution for forming a microporous layer. At this time, the mass ratio of acetylene black / graphite / waterproofing agent / dispersant / purified water is adjusted to 5.6 mass parts / 1.4 mass parts / 1.1 mass parts / 14.0 mass parts / 77.9 mass parts. At this time, the mass of PTFE is 8.6% relative to the mass of the entire solid component (acetylene black + graphite + PTFE).

[0131] (Coating / Drying)

[0132] The microporous layer-forming coating liquid was applied to the water-repellent-treated conductive porous substrate using a slot die coater so that the solid content per unit area was 20 g / m 2 , dried at 120°C.

[0133] (Heat treatment)

[0134] Next, a heat treatment was performed at 380° C. to obtain a gas diffusion electrode.

[0135] [Example 2]

[0136] When preparing the coating liquid for forming the microporous layer, flake graphite JB-5 (aspect ratio: 36, bulk density 0.08 g / cm 3 , crystallite size 23 nm, manufactured by Nippon Graphite Industries, Ltd.) as graphite particles. Except for this, a gas diffusion electrode was obtained in the same manner as in Example 1.

[0137] [Example 3]

[0138] During the water-repellent treatment, PTFE was applied so as to be 8.0 parts by mass based on 100.0 parts by mass of the conductive porous substrate. A gas diffusion electrode was obtained in the same manner as in Example 1 except for this.

[0139] [Example 4]

[0140] During the water-repellent treatment, PTFE was applied so that the amount of PTFE was 12.5 parts by mass based on 100.0 parts by mass of the conductive porous substrate. A gas diffusion electrode was obtained in the same manner as in Example 1 except for this.

[0141] [Example 5]

[0142] During the water-repellent treatment, PTFE was applied so as to be 2.0 parts by mass based on 100.0 parts by mass of the conductive porous substrate. A gas diffusion electrode was obtained in the same manner as in Example 1 except for this.

[0143] [Example 6]

[0144] In the waterproofing process, the conductive porous substrate was completely immersed in a diluted aqueous solution of a PTFE dispersion ("POLYFLON (registered trademark)" D-210C; manufactured by Daikin Industries, Ltd.; containing 60% by mass of PTFE in a dispersion medium (water)) and then dried at 120°C. The amount of PTFE was 5.0 parts by mass relative to 100.0 parts by mass of the conductive porous substrate. A gas diffusion electrode was obtained in the same manner as in Example 1 except for the above.

[0145] [Example 7]

[0146] In the preparation of the microporous layer forming coating liquid, the mass ratio of acetylene black / graphite / waterproofing agent / surfactant / purified water was adjusted to 5.6 mass parts / 1.4 mass parts / 2.1 mass parts / 14.0 mass parts / 76.9 mass parts. Except for this, a gas diffusion electrode was obtained in the same manner as in Example 1. At this time, the mass of PTFE was 15.0% relative to the mass of the entire solid component (acetylene black+graphite+PTFE).

[0147] [Example 8]

[0148] In the preparation of the microporous layer forming coating liquid, the mass ratio of acetylene black / graphite / waterproofing agent / surfactant / purified water was adjusted to 5.6 mass parts / 1.4 mass parts / 3.7 mass parts / 14.0 mass parts / 75.3 mass parts. Except for this, a gas diffusion electrode was obtained in the same manner as in Example 1. At this time, the mass of PTFE relative to the mass of the entire solid component (acetylene black+graphite+PTFE) was 24.1%.

[0149] [Example 9]

[0150] In the preparation of the microporous layer forming coating liquid, the mass ratio of acetylene black / graphite / water repellent / surfactant / purified water was adjusted to 3.5 mass parts / 3.5 mass parts / 1.1 mass parts / 14.0 mass parts / 77.9 mass parts.

[0151] [Example 10]

[0152] In the coating / drying process, the microporous layer-forming coating liquid was applied to the water-repellent-treated conductive porous substrate using a slot die coater so that the solid content per unit area was 20 g / m 2 Then, the microporous layer was coated again with a slot die coater so that the weight per unit area was 20 g / m 2 , and dried at 120° C. A gas diffusion electrode was obtained in the same manner as in Example 1 except for this.

[0153] [Example 11]

[0154] When preparing the coating liquid for forming the microporous layer, flake graphite BSP-5AK (aspect ratio: 57, bulk density: 0.05 g / cm 3 , crystallite size 16 nm, (manufactured by Chuetsu Graphite Industry Co., Ltd.) as graphite particles. Except for this, a gas diffusion electrode was obtained in the same manner as in Example 1.

[0155] [Example 12]

[0156] When preparing the coating liquid for forming the microporous layer, flake graphite CB-150 (aspect ratio: 26, bulk density: 0.26 g / cm 3 , crystallite size 21 nm, manufactured by Nippon Graphite Industries, Ltd.) as graphite particles. Except for this, a gas diffusion electrode was obtained in the same manner as in Example 1.

[0157] [Example 13]

[0158] When preparing the coating liquid for forming the microporous layer, flake graphite PCE-7 (aspect ratio: 21, bulk density: 0.12 g / cm 3 , crystallite size 14 nm, (manufactured by Chuetsu Graphite Industry Co., Ltd.) as graphite particles. Except for this, a gas diffusion electrode was obtained in the same manner as in Example 1.

[0159] [Comparative Example 1]

[0160] In the preparation of the microporous layer-forming coating liquid, the mass ratio of acetylene black / graphite / water repellent / surfactant / purified water was adjusted to 7.0 mass parts / 0 mass parts / 1.1 mass parts / 14.0 mass parts / 77.9 mass parts.

[0161] [Comparative Example 2]

[0162] Spherical graphite CGB-6R (aspect ratio: 6.5, bulk density: 0.26 g / cm 3 , crystallite size 31 nm, manufactured by Nippon Graphite Industries, Ltd.) as graphite particles for the microporous layer forming coating liquid. Except for this, a gas diffusion electrode was obtained in the same manner as in Example 1.

[0163] [Comparative Example 3]

[0164] A gas diffusion electrode was obtained in the same manner as in Example 1 except that the diluted aqueous solution of the PTFE dispersion was not applied to the conductive porous substrate.

[0165] [Comparative Example 4]

[0166] In the preparation of the microporous layer forming coating liquid, the mass ratio of acetylene black / graphite / water repellent / surfactant / purified water was adjusted to 1.4 mass parts / 5.6 mass parts / 1.1 mass parts / 14.0 mass parts / 77.9 mass parts.

[0167] [Comparative Example 5]

[0168] In the preparation of the microporous layer forming coating liquid, the mass ratio of acetylene black / graphite / waterproofing agent / surfactant / purified water was adjusted to 2.8 mass parts / 0.7 mass parts / 0.6 mass parts (0.55 mass parts) / 7.0 mass parts / 88.9 mass parts. A gas diffusion electrode was obtained in the same manner as in Example 1 except for this.

[0169] [Comparative Example 6]

[0170] (Conductive porous substrate)

[0171] The same conductive porous substrate as that prepared in Example 1 was used.

[0172] (Waterproof processing)

[0173] In the same manner as in Example 1, the conductive porous substrate was subjected to water-repellent treatment.

[0174] (Coating liquid for forming microporous layer)

[0175] A coating liquid for forming a microporous layer was prepared in the same manner as in Example 1 except that the mass ratio of acetylene black / graphite / waterproofing agent / surfactant / purified water was adjusted to 5.6 parts by mass / 1.4 parts by mass / 6.3 parts by mass / 14.0 parts by mass / 72.7 parts by mass. At this time, the mass of PTFE was 35.0% relative to the mass of the entire solid component (acetylene black+graphite+PTFE).

[0176] (Microporous layer membrane)

[0177] The microporous layer-forming coating liquid was applied onto a "Kapton (registered trademark)" (manufactured by DuPont Toray Co., Ltd.) film using a slot die coater so that the weight per unit area was 20 g / m 2 Thereafter, the film was dried at 120° C., heat treated at 380° C., and peeled from the Kapton film to obtain a microporous layer film.

[0178] (Lamination / Joining)

[0179] The microporous layer was laminated on the water-repellent treated conductive porous substrate in the same manner as in Example 1, and the layers were bonded by roll pressing (pressure 2.0 MPa, temperature 100° C., rotation speed 50 mm / s) to obtain a gas diffusion electrode.

[0180] [Example 14]

[0181] (Conductive porous substrate)

[0182] In addition to setting the unit area weight of the carbon fiber in the carbon fiber sheet to 21g / m 2 A conductive porous substrate was obtained in the same manner as in Example 1 except for the above. The thickness of the obtained conductive porous substrate at 0.15 MPa was 190 μm, and the density was 0.30 g / cm 3 .

[0183] (Waterproof processing)

[0184] The conductive porous substrate was subjected to water-repellent treatment in the same manner as in Example 1, so that the amount of PTFE was 5.0 parts by mass relative to 100.0 parts by mass of the conductive porous substrate. The electrical resistance of the conductive porous substrate subjected to water-repellent treatment was 5.3 mΩcm 2 .

[0185] (Coating liquid for forming microporous layer)

[0186] The same microporous layer-forming coating liquid as that used in Example 1 was used.

[0187] (Coating / Drying)

[0188] The microporous layer-forming coating liquid was applied to the water-repellent-treated conductive porous substrate using a slot die coater so that the solid content per unit area was 20 g / m 2 , dried at 120°C.

[0189] (Heat treatment)

[0190] Next, a heat treatment was performed at 380° C. to obtain a gas diffusion electrode.

[0191] [Comparative Example 7]

[0192] In the preparation of the microporous layer-forming coating liquid, the mass ratio of acetylene black / graphite / waterproofing agent / surfactant / purified water was adjusted to 7.0 mass parts / 0 mass parts / 1.1 mass parts / 14.0 mass parts / 77.9 mass parts.

[0193] Tables 1 to 4 show the physical properties and evaluation results of the gas diffusion electrodes of Examples and Comparative Examples.

[0194]

[0195]

[0196]

[0197]

[0198] Industrial Applicability

[0199] The gas diffusion electrode of the present invention is suitable for use as an electrode of a fuel cell, and is suitable for use as an electrode of a polymer electrolyte fuel cell used as a power source for transportation equipment such as a fuel cell vehicle or a fuel cell aircraft.

[0200] Explanation of symbols

[0201] 1Gas Diffusion Electrode

[0202] 2 Microporous layer

[0203] 3. Carbon Fiber

[0204] 10 Microporous layer on the surface

[0205] 11 The surface of the conductive porous substrate

[0206] 12 Microporous layer innermost

[0207] 13 Conductive porous substrate innermost

[0208] 14Thickness of microporous layer

[0209] 15Thickness of the conductive porous substrate

[0210] 16Thickness of penetration part

[0211] 17 Thickness of non-penetrated part

[0212] A is a point on the boundary between the infiltrated portion and the non-infiltrated portion that is closest to the outermost surface 10 of the microporous layer.

[0213] B is a point on the surface of the conductive porous substrate opposite to the outermost surface of the conductive porous substrate, which is farthest from the outermost surface of the microporous layer.

Claims

1. A gas diffusion electrode having a microporous layer on at least one side of a conductive porous substrate, characterized in that: The microporous layer contains carbon black and graphite particles having an aspect ratio of 10 or more, and a thickness of the conductive porous substrate in which the microporous layer has penetrated is 5% or more and 20% or less relative to a thickness of the conductive porous substrate in which the microporous layer has not penetrated.

2. The gas diffusion electrode according to claim 1, wherein: The density of the microporous layer is 0.30 g / cm 3 Above and 0.50g / cm 3 the following.

3. The gas diffusion electrode according to claim 1 or 2, wherein: The fluorine / carbon ratio of the surface of the conductive porous substrate on the side close to the microporous layer is 0.20 or more and 0.40 or less.

4. The gas diffusion electrode according to claim 1 or 2, wherein: The microporous layer contains a water repellent in an amount of 0.1 mass % or more and 10 mass % or less based on 100 mass % of the entire mass of the microporous layer.

5. The gas diffusion electrode according to claim 1 or 2, wherein: The fluorine / carbon ratio of the surface of the microporous layer that is not close to the conductive porous substrate is 0.01 or more and 0.20 or less.

6. The gas diffusion electrode according to claim 1 or 2, wherein: The fluorine / carbon ratio of the surface of the conductive porous substrate that is not close to the microporous layer is 0.01 or more and 0.15 or less.

7. The gas diffusion electrode according to claim 1 or 2, wherein: The conductive porous substrate contains 2 parts by mass or more and 10 parts by mass or less of a water repellent relative to 100 parts by mass of the conductive porous substrate.

8. The gas diffusion electrode according to claim 1 or 2, wherein: The gas diffusivity in the in-plane direction is 50 cc / min or more and 150 cc / min or less.

9. The gas diffusion electrode according to claim 1 or 2, wherein: The aspect ratio of the graphite particles contained in the microporous layer is 50 or more and 5000 or less.

10. The gas diffusion electrode according to claim 1 or 2, wherein: The bulk density of the graphite particles contained in the microporous layer is 0.01 g / cm 3 Above and 0.20g / cm 3 the following.

11. The gas diffusion electrode according to claim 1 or 2, wherein: The crystallite size of the graphite particles contained in the microporous layer is 15 nm or more and 100 nm or less.

12. The gas diffusion electrode according to claim 1 or 2, wherein: When the total mass of the carbon black and the graphite particles contained in the microporous layer is 100 mass %, the mass of the graphite particles is 10 mass % or more and 50 mass % or less.

13. The gas diffusion electrode according to claim 1 or 2, wherein: The microporous layer has a unit area weight of 10 g / m 2 Above and 30g / m 2 the following.

14. The gas diffusion electrode according to claim 1 or 2, wherein: The surface roughness Sa of the surface of the microporous layer that is not close to the conductive porous substrate is 0.1 μm or more and 7 μm or less. 15 . A fuel cell comprising an electrolyte membrane, a catalyst layer, a separator, and the gas diffusion electrode according to claim 1 or 2.

16. A transport device using the fuel cell according to claim 15 as a power supply source.