Bursting bead and preparation method thereof
By using a two-step cross-linking method and ultraviolet light irradiation, the leakage problem of hyaluronic acid encapsulation material was solved, improving the mechanical strength and taste of popping beads and achieving better popping performance and taste experience.
Patent Information
- Application Number
- CN202411244515.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-11-15
AI Technical Summary
In existing technologies, hyaluronic acid is prone to leakage when used as an encapsulation material, resulting in a loose gel structure and insufficient mechanical strength in popping beads, which affects the product's texture and taste.
Popping beads were prepared using a two-step crosslinking method. First, crosslinking was performed in a coagulation bath, followed by a second crosslinking in a calcium bath. Ultraviolet light was introduced between the two crosslinking steps to reduce the pores of the gel membrane.
It effectively reduces the leakage loss of hyaluronic acid, enhances the load-bearing capacity and texture of popping beads, ensures that the bursting force and bursting strain reach 1000g and 40% or more, and the outer shell layer thickness is 0.08-0.2mm, resulting in excellent taste and bursting sensation.
Smart Images

Figure BDA0005030433350000181 
Figure BDA0005030433350000191 
Figure BDA0005030433350000192
Abstract
Description
Technical Field
[0001] The present application belongs to the field of food processing technology, and specifically relates to a popping bead and a preparation method thereof. Background Art
[0002] Bursting beads are a new product on the market in recent years. The preparation method mainly uses the reverse spheroidization method to drop the core liquid into the coagulation bath, and use the ion replacement reaction between sodium alginate and divalent cations to produce a thin film to wrap liquids such as juice or solid particles. After squeezing, the film breaks and generates an explosive force in the mouth. At the same time, the core liquid contents flow out, giving people a mouthfeel and taste bud enjoyment.
[0003] Hyaluronic acid is a linear high molecular weight acidic mucopolysaccharide composed of D-glucuronic acid (GlcA) and N-acetylglucosamine (GlcNAc) connected alternately by disaccharide units. It has the functions of moisturizing, enhancing immunity, moisturizing and beautifying the skin. On May 26, 2008, the National Health Commission issued the "Notice of the Ministry of Health on the Approval of 7 New Resource Foods Including Lactobacillus Acidophilus", officially approving sodium hyaluronate as a new resource food that can be used in food production. At present, no explosive bead products containing sodium hyaluronate have been found.
[0004] However, as a linear macromolecular mucopolysaccharide, hyaluronic acid has a certain fluidity and is prone to leakage when used as the core material of embedded products, so it has high requirements for the "egg box" structure of the embedding. Sodium alginate is a copolymer of β-1,4-D-mannuronic acid residues (M) and α-1,4-L-guluronic acid residues (G). Only the G segment can react with Ca 2+ The coordination forms an "egg-box" structure. The M / G ratio in sodium alginate ranges from 1.5 to 1.8. The MM block content in the molecule is higher than the GG block, resulting in insufficient cross-linking sites for sodium alginate. 2+ The calcium alginate gel prepared by cross-linking has a loose gel structure and serious leakage problems; at the same time, the insufficient cross-linking sites of sodium alginate will also affect the mechanical strength of the product, especially when embedding hyaluronic acid, a viscoelastic and fluid substance, which will affect the texture of the popping beads and reduce the taste of the product. Therefore, sodium alginate has great limitations as an embedding material for hyaluronic acid. Summary of the invention
[0005] In view of the above-mentioned problems in the prior art, the present application is proposed to prepare a hyaluronic acid-encapsulated popping bead product, reduce the leakage loss of hyaluronic acid and enable it to have a certain load and mass transfer capacity, and have a better chewing taste and popping feeling.
[0006] Specifically, the present application provides a method for preparing popping beads, which comprises the following steps:
[0007] (1) preparing a coagulation bath solution, a core material solution and a calcium bath solution respectively;
[0008] (2) adding the core material liquid into the coagulation bath liquid for primary cross-linking to obtain semi-finished particles;
[0009] (3) After irradiating the semi-finished product particles with ultraviolet light, adding them into the calcium bath for secondary cross-linking to obtain the popping beads.
[0010] Wherein, the coagulation bath solution comprises sodium alginate; the core material solution comprises calcium salt and hyaluronic acid or its salt; and the calcium bath solution comprises calcium salt.
[0011] Furthermore, the viscosity of the sodium alginate is 200 to 1200 cps, and more preferably 400 to 1000 cps.
[0012] Furthermore, in the coagulation bath solution, the content of sodium alginate is 0.5-1.5 wt %.
[0013] Furthermore, in the core liquid, the content of calcium salt is 2-10 wt %, and the content of hyaluronic acid or its salt is 1-10 wt %.
[0014] Furthermore, in the calcium bath, the content of calcium salt is 2-6 wt %.
[0015] Furthermore, the reaction time of the primary cross-linking is 4 to 17 minutes, preferably 5 to 15 minutes; the reaction time of the secondary cross-linking is 2 to 17 minutes, preferably 3 to 15 minutes.
[0016] Furthermore, the wavelength of the ultraviolet light is 320nm to 380nm, the ultraviolet light irradiation time is 10min to 60min, and the light intensity of the ultraviolet light is 1000 to 2000mJ / cm 2 .
[0017] The present application provides a bursting bead, which is prepared by the above method.
[0018] The present application also provides a bursting bead, which includes an outer shell layer and an inner layer wrapped by the outer shell layer. Further, the outer shell layer includes calcium alginate, and the inner layer includes hyaluronic acid or a salt thereof.
[0019] Furthermore, the blasting force of the blasting bead is ≥1000g, the blasting strain is ≥40%, and the thickness of the outer shell layer of the blasting bead is 0.08-0.2mm.
[0020] Effects of the Invention
[0021] The technical solution provided in the present application adopts a primary cross-linking method to prepare a semi-finished product of explosive beads containing hyaluronic acid. After ultraviolet light irradiation, the semi-finished product of the explosive beads is added into a calcium bath for secondary cross-linking, so that the membrane structure of the explosive beads shrinks and the pores are reduced, thereby showing a better load capacity and reducing the leakage loss of hyaluronic acid. The loss rate of hyaluronic acid during storage is less than 6%.
[0022] The technical solution provided in the present application adopts reverse spheroidization to prepare semi-finished popping beads containing hyaluronic acid, and then conducts a secondary calcium bath after ultraviolet light irradiation to improve the texture of the popping beads, with a bursting force ≥1000g, a bursting strain ≥40%, and a shell layer thickness of 0.08-0.2mm, so that the product is not easy to break during the preparation and storage process, the outer skin is easy to chew and has an elastic and suitable chewing taste, and the bursting feeling is obvious. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 This is a real picture of the explosive beads prepared in Example 1 of the present application. DETAILED DESCRIPTION
[0024] The present application is further described in detail below in conjunction with specific implementation methods. The examples given are intended to enable a more thorough understanding of the present application and to fully convey the scope of the present application to those skilled in the art.
[0025] It should be noted that many specific details are set forth in the following description to facilitate a full understanding of the present application, but the present application can also be implemented in other ways different from this description, and those skilled in the art can make similar generalizations without violating the connotation of the present application. Therefore, the present application is not limited to the specific embodiments disclosed below.
[0026] Secondly, the "embodiment" or "specific implementation method" referred to below refers to specific features, structures or characteristics that may be included in at least one implementation method of the present application. The "in one embodiment" that appears in different places in this specification does not all refer to the same embodiment, nor is it a separate or selective embodiment that is mutually exclusive with other embodiments. The subsequent description of the specification is a preferred embodiment for implementing the present application, but the description is for the purpose of the general principles of the specification and is not intended to limit the scope of the present application. The scope of protection of the present application shall be determined as defined by the attached claims.
[0027] The present application provides a method for preparing popping beads, which comprises the following steps:
[0028] (1) preparing a coagulation bath solution, a core material solution and a calcium bath solution respectively;
[0029] (2) adding the core material liquid into the coagulation bath liquid for primary cross-linking to obtain semi-finished particles;
[0030] (3) After irradiating the semi-finished product particles with ultraviolet light, adding them into the calcium bath for secondary cross-linking to obtain the popping beads.
[0031] In a specific embodiment, the coagulation bath solution includes sodium alginate; the core liquid includes calcium salt and hyaluronic acid or its salt; the calcium bath solution includes calcium salt
[0032] In a specific embodiment, the step of preparing the coagulation bath solution includes: uniformly dissolving sodium alginate in water to prepare the coagulation bath solution.
[0033] In a specific embodiment, the step of preparing the core material liquid comprises: uniformly dissolving calcium salt and hyaluronic acid or its salt in water to obtain the core material liquid.
[0034] In a specific embodiment, the preparation step of the calcium bath comprises: uniformly dissolving calcium salt in water to obtain the calcium bath.
[0035] The popping pearls described in this application refer to the same packaging structure as the popping pearls, which contain the corresponding contents. On the basis of being able to wrap the contents, the outer skin is soft and easy to chew, with appropriate elasticity and obvious bursting feeling. It is an emerging product prepared by spheroidization technology on the market in recent years. This technology was invented by Peschardt in 1946 and promoted by the Spanish bulldog restaurant ElBulli. According to different preparation methods, spheroidization technology can be divided into forward spheroidization and reverse spheroidization.
[0036] The preparation method provided by the present application is based on the reverse spheroidization technology, that is, a core liquid containing calcium ions is dropped into a coagulation bath containing sodium alginate, and the calcium ions diffuse outward from the core liquid, and immediately form a calcium alginate gel film layer in the outer direction of the two liquid interfaces after encountering sodium alginate. As the calcium ions move outward, the gel film layer gradually thickens, and this unidirectional diffusion keeps the interior of the sphere in its original state. In addition, the ion gelation reaction and the moment the sphere is removed from the coagulation bath can stop crosslinking, which makes it possible to store the liquid core sphere stably.
[0037] The method for preparing the popping beads provided in the present application includes a two-step cross-linking process. In the first cross-linking, the core liquid is added to the coagulation bath to prepare semi-finished particles; in the second cross-linking, the semi-finished particles are added to the calcium bath to prepare the finished popping beads. In particular, the process step of introducing ultraviolet light irradiation between the two cross-linkings can greatly reduce the pores of the gel membrane, thereby reducing the leakage rate, increasing the mechanical strength, and improving the stability.
[0038] In a specific embodiment, the coagulation bath solution is prepared by the following method: sodium alginate is added to deionized water, stirred, and uniformly dissolved to obtain the coagulation bath solution.
[0039] In a specific embodiment, magnetic stirring can be used in the preparation of the coagulation bath.
[0040] In a specific embodiment, the solution may be left to stand overnight after stirring to remove air bubbles in the coagulation bath.
[0041] In a specific embodiment, the viscosity of the sodium alginate is 200 to 1200 cps. In some preferred embodiments, the viscosity of the sodium alginate is 400 to 1000 cps, for example, the viscosity can be 200 cps, 250 cps, 300 cps, 350 cps, 400 cps, 450 cps, 500 cps, 550 cps, 600 cps, 650 cps, 700 cps, 750 cps, 800 cps, 850 cps, 900 cps, 950 cps, 1000 cps, 1050 cps, 1100 cps, 1150 cps or 1200 cps. The viscosity of the sodium alginate can be tested by an analytical method commonly used in the art, for example, by a rotational viscometer or a cone-plate viscometer. In a specific embodiment of the present application, the viscosity of sodium alginate is tested using a Brookfield DV2T viscometer, the test temperature is 25° C., and the torque is 50%.
[0042] In a specific embodiment, in the coagulation bath, the content of sodium alginate is 0.5-1.5wt%, preferably 0.8-1.2wt%, for example, the content can be 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt%, 1.0wt%, 1.05wt%, 1.1wt%, 1.15wt% or 1.2wt%.
[0043] In a specific embodiment, in the preparation of the coagulation bath solution, polysaccharide and sodium alginate may be dissolved in water to obtain the coagulation bath solution.
[0044] In a specific embodiment, the polysaccharide is selected from pectin, gelatin or carrageenan.
[0045] In a specific embodiment, the mass ratio of sodium alginate to polysaccharide is 2:1 to 10:1.
[0046] In a specific embodiment, the core material liquid is prepared by the following method: calcium salt and hyaluronic acid or its salt are uniformly dissolved in water to obtain the core material liquid.
[0047] In a specific embodiment, calcium salt and hyaluronic acid or its salt are uniformly dissolved in water to obtain a core liquid, and then subjected to high-temperature gelatinization treatment at a gelatinization temperature of 70° C. to 90° C. for a gelatinization time of 1 to 10 min.
[0048] In a specific embodiment, the hyaluronate salt comprises sodium hyaluronate.
[0049] In some specific embodiments, the hyaluronate has a molecular weight of 80 kDa to 4000 kDa, preferably 100 kDa to 1800 kDa, for example, a molecular weight of 80 kDa, 100 kDa, 200 kDa, 300 kDa, 400 kDa, 500 kDa, 600 kDa, 700 kDa, 800 kDa, 900 kDa, 1000 kDa, 1100 kDa, 1200 kDa, 1300 kDa, 1400 kDa, 1500 kDa, 1600 kDa, 1700 kDa, 1800 kDa, 1900 kDa, 2000 kDa, 2100 kDa, 2200 kDa, 2300 kDa, 2400 kDa, 2500 kDa, 2600 kDa, 2700 kDa, 2800 kDa, 2900 kDa, 3000 kDa, 3100 kDa, 3200 kDa, 3300 kDa, 3400 kDa, 3500 kDa, 3600 kDa, 3700 kDa, 3800 kDa, 3900 kDa, 4000 kDa, 4100 kDa, 4200 kDa, 4300 kDa, 4400 kDa, 4500 kDa, 4600 kDa, 4700 kDa, 4800 kDa, 4900 kDa, 500 kDa, 5100 kDa, 5200 kDa, 5300 kDa, 5 00kDa, 1800kDa, 1900kDa, 2000kDa, 2100kDa, 2200kDa, 2300kDa, 2400kDa, 2500kDa, 2600kDa, 2700kDa, 2800kDa, 2 900kDa, 3000kDa, 3100kDa, 3200kDa, 3300kDa, 3400kDa, 3500kDa, 3600kDa, 3700kDa, 3800kDa, 3900kDa, 4000kDa.
[0050] In a specific embodiment, the calcium salt in the core liquid includes one or more of calcium lactate, calcium chloride, calcium carbonate, calcium sulfate, calcium acetate, calcium dihydrogen phosphate or calcium glucose.
[0051] In a preferred embodiment, the calcium salt is calcium lactate.
[0052] In a specific embodiment, the core liquid further comprises auxiliary materials that can be added in the food field, such as flavors, food coloring, sweeteners, acidulants, thickeners, and the like.
[0053] In a specific embodiment, the core liquid is prepared by the following method: calcium salt, hyaluronic acid or its salt and auxiliary materials that can be added in the food field are uniformly dissolved in water to obtain the core liquid, and then subjected to high-temperature gelatinization treatment, the gelatinization temperature is 70°C to 90°C, and the gelatinization time is 1 to 10 minutes.
[0054] In some specific embodiments, the calcium salt content in the core liquid is 2-10wt%, preferably 3-9wt%, for example, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt% or 9wt%, by mass fraction.
[0055] In some specific embodiments, the content of hyaluronic acid or its salt in the core liquid is 1-10wt%, preferably 2-8wt%, for example, the content of hyaluronic acid or its salt is 1wt%, 2wt%, 3wt%, 4wt%, 5wt%, 6wt%, 7wt%, 8wt%, 9wt% or 10wt%.
[0056] In some specific embodiments, a thickener may be added during the preparation of the core liquid.
[0057] In a specific embodiment, the core liquid is prepared by dissolving calcium salt in deionized water, adding hyaluronic acid or its salt and a thickener, dispersing and dissolving at high speed, stirring evenly and then performing high-temperature gelatinization treatment.
[0058] In a specific embodiment, the content of the thickener in the core liquid is 0.5-5 wt %.
[0059] In some specific embodiments, the thickener includes hydroxypropyl distarch phosphate, xanthan gum, sodium carboxymethyl cellulose or guar gum.
[0060] In a specific embodiment, the preparation step of the calcium bath comprises: dissolving calcium salt in water and dispersing the calcium salt uniformly.
[0061] In a specific embodiment, the calcium salt in the calcium bath includes one or more of calcium chloride, calcium carbonate, calcium lactate, calcium sulfate, calcium acetate, calcium dihydrogen phosphate, and calcium glucose.
[0062] In a preferred embodiment, the calcium salt is calcium lactate.
[0063] In a specific embodiment, a thickener may be added during the preparation of the calcium bath.
[0064] In a specific embodiment, the preparation step of the calcium bath comprises: dissolving the calcium salt and the thickener in water and dispersing them uniformly to obtain the calcium bath.
[0065] In a specific embodiment, the dispersion can be performed with a high-speed disperser.
[0066] In a specific embodiment, the thickener includes sodium carboxymethylcellulose, hydroxymethylcellulose or hydroxyethylcellulose.
[0067] In a specific embodiment, the mass ratio of calcium salt to thickener in the calcium bath is 2:1 to 10:1.
[0068] In some specific embodiments, the mass concentration of the calcium salt in the calcium bath is 2-6 wt %.
[0069] In some specific embodiments, the mass concentration of the thickener in the calcium bath is 0.1-3 wt %.
[0070] In a specific embodiment of the present application, the core material liquid is added to the coagulation bath to undergo primary crosslinking to obtain semi-finished particles, and then the semi-finished particles are irradiated with ultraviolet light and added to the calcium bath to undergo secondary crosslinking to obtain popping beads.
[0071] In a specific embodiment, the core material liquid is vertically dripped dropwise into the coagulation bath liquid to prepare semi-finished particles.
[0072] In a specific embodiment, the reaction time of the primary cross-linking is 4 to 17 min, preferably 5 to 15 min, for example, 4 min, 5 min, 6 min, 7 min, 8 min, 9 min, 10 min, 11 min, 12 min, 13 min, 14 min, 15 min, 16 min, 17 min, etc.
[0073] In a specific embodiment, the reaction time of the secondary cross-linking is 2 to 17 minutes, preferably 3 to 15 minutes, for example, it can be 2 minutes, 3 minutes, 4 minutes, 5 minutes, 6 minutes, 7 minutes, 8 minutes, 9 minutes, 10 minutes, 11 minutes, 12 minutes, 13 minutes, 14 minutes, 15 minutes, 16 minutes, 17 minutes, etc.
[0074] In a specific embodiment, in the preparation method, the wavelength of ultraviolet light used for ultraviolet light irradiation is 320-380nm, for example, it can be 320nm, 330nm, 340nm, 350nm, 360nm, 370nm, 380nm; the ultraviolet light irradiation time is 5min-60min, preferably 10min-50min, further preferably 15min-45min, for example, it can be 15min, 20min, 25min, 30min, 35min, 40min.
[0075] In a specific embodiment, the intensity of ultraviolet light is 1000-2000 mJ / cm 2 .
[0076] mJ / cm 2 It is the unit of measurement when using a UV energy meter to measure the intensity of ultraviolet light, that is, the ultraviolet light energy per unit area. In a specific embodiment, the preparation method further includes a storage step: adding the prepared explosive beads to a sugar protection solution, sterilizing them and then storing them.
[0077] In a specific embodiment, the sugar protective liquid is fructose syrup or erythritol.
[0078] The explosive beads provided in the present application can be prepared by the above-mentioned preparation method.
[0079] The present application also provides a bursting bead, which includes an outer shell layer and an inner layer wrapped by the outer shell layer, the outer shell layer includes calcium alginate, and the inner layer includes hyaluronic acid or a salt thereof.
[0080] In a specific embodiment, the outer shell layer is a calcium alginate gel membrane layer formed by cross-linking of calcium ions and sodium alginate.
[0081] In a specific embodiment, the inner layer is a fluid comprising hyaluronic acid or a salt thereof, wherein the fluid is a semisolid or a liquid.
[0082] In a specific embodiment, the bursting force of the bursting beads is ≥ 1000g, preferably the bursting force is 1000-2500g.
[0083] The "blasting force" mentioned in this application refers to the maximum pressure value that the blasting bead withstands when a pressure load is applied to the blasting bead to cause it to rupture. Further, the "blasting strain" mentioned in this application refers to the ratio of the deformation amount of the blasting bead under the blasting force to the original size.
[0084] Within the bursting force range described in the present application, the popping beads are not easy to break during storage, and have suitable mechanical properties and film thickness, so that the elasticity, chewing taste and bursting feeling of the popping beads are optimal; if the bursting force is less than 1000g, the popping beads are easily broken, which is not conducive to storage and transportation, and the taste is poor and has no chewiness; if the bursting force is greater than 2500g, the popping beads are not easy to chew, the film layer is too thin, and the residual feeling in the mouth is heavy.
[0085] In a specific implementation, the bursting strain of the popping beads is ≥40%, preferably 40% to 80%. Within this bursting strain range, it is more suitable for the chewing behavior of the human oral cavity and provides enjoyment to the taste buds.
[0086] In a specific embodiment, the shell layer thickness of the popping bead is 0.08-0.2 mm. If the shell layer is too thin, the residual feeling of the shell in the mouth after the popping bead is aggravated, which is not conducive to swallowing, and the popping bead is easy to break; if the shell layer is too thick, the inner layer of the popping bead is limited in the distance it pops out after breaking, and the popping feeling is not good.
[0087] Example
[0088] The present application provides a general and / or specific description of the materials and test methods used in the experiments. In the following examples, unless otherwise specified, % means wt%, i.e., weight percentage. The reagents or instruments used without indicating the manufacturer are all conventional reagent products that can be obtained commercially.
[0089] In the following examples, sodium alginate was purchased from Lianyungang Tiantian Seaweed Industrial Co., Ltd., and sodium hyaluronate was purchased from Bloomage Biotech Co., Ltd.
[0090] Example 1
[0091] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0092] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0093] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0094] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0095] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0096] Example 2
[0097] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 800-1000 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0098] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0099] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0100] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0101] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0102] Example 3
[0103] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0104] Step 2: Prepare core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 2wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain core liquid;
[0105] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0106] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0107] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0108] Example 4
[0109] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0110] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 8wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0111] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0112] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0113] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0114] Example 5
[0115] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0116] Step 2: Prepare the core liquid: weigh 3wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0117] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0118] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0119] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0120] Example 6
[0121] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0122] Step 2: Prepare the core liquid: weigh 7wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0123] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0124] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0125] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0126] Example 7
[0127] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0128] Step 2: Prepare core liquid: weigh 9wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain core liquid;
[0129] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0130] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0131] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0132] Example 8
[0133] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0134] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0135] Step 3: Prepare calcium bath solution: dissolve 5 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0136] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0137] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0138] Example 9
[0139] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0140] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0141] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0142] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 15 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0143] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0144] Example 10
[0145] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0146] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0147] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0148] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 45 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0149] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0150] Embodiment 11
[0151] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0152] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0153] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0154] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform a cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 320nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0155] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0156] Example 12
[0157] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0158] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0159] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0160] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1000mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0161] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0162] Example 13
[0163] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0164] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and then cool to room temperature to obtain the core liquid;
[0165] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0166] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 3 minutes and then fished out to obtain explosive beads.
[0167] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0168] Embodiment 14
[0169] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0170] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0171] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0172] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 10 minutes and then fished out to obtain explosive beads.
[0173] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0174] Embodiment 15
[0175] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0176] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0177] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0178] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 15 minutes and then fished out to obtain explosive beads.
[0179] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0180] Example 16
[0181] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0182] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0183] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0184] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 10 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0185] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0186] Embodiment 17
[0187] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0188] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0189] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0190] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform a cross-linking for 15 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0191] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0192] Embodiment 18
[0193] Step 1: Prepare a coagulation bath: weigh 1.2 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water. Stir it evenly with a magnetic stirrer and remove bubbles overnight to prepare a coagulation bath solution.
[0194] Step 2: Prepare core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 1550kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a constant temperature water bath at 80℃ for 5 minutes, and then cool to room temperature to obtain core liquid;
[0195] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0196] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 minutes, the beads were placed in a calcium bath for secondary cross-linking for 5 minutes and then fished out to obtain explosive beads.
[0197] The above-mentioned popping beads were placed in a fructose syrup protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0198] Comparative Example 1
[0199] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0200] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0201] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0202] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid into the coagulation bath drop by drop, perform primary cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the residual coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, then put them into a calcium bath for secondary cross-linking for 5 minutes, and then fish them out to obtain the popping beads.
[0203] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0204] Comparative Example 2
[0205] Step 1: Prepare a coagulation bath: weigh 0.8 wt% sodium alginate (viscosity 400-600 cps) and dissolve it in deionized water, stir it evenly with a magnetic stirrer, and remove bubbles overnight to prepare a coagulation bath solution;
[0206] Step 2: Prepare the core liquid: weigh 5wt% calcium lactate and dissolve it in 60℃ deionized water, and add 1wt% hydroxypropyl distarch phosphate and 4wt% sodium hyaluronate (molecular weight 111.6kDa) after cooling to room temperature, dissolve and stir evenly at high speed, and then gelatinize at high temperature, and gelatinize in a 90℃ constant temperature water bath for 3 minutes, and cool to room temperature to obtain the core liquid;
[0207] Step 3: Prepare calcium bath solution: dissolve 3 wt% calcium lactate in water and disperse evenly at high speed for later use;
[0208] Step 4: Preparation of hyaluronic acid liquid core popping beads: vertically drip the prepared core liquid drop by drop into the coagulation bath, perform cross-linking for 5 minutes, drain the popping beads with a nylon filter, rinse the remaining coagulation bath solution on the surface of the popping beads with deionized water to obtain a semi-finished product, and then irradiate it with ultraviolet light at a wavelength of 365nm and an intensity of 1600mJ / cm 2 After irradiation for 30 min, the explosive beads were obtained.
[0209] The above-mentioned popping pearls were placed in erythritol protective solution, sterilized in a 95°C water bath for 30 minutes, and then packed and stored.
[0210] The preparation process parameters of the above examples and comparative examples are shown in Table 1.
[0211] Table 1
[0212]
[0213]
[0214] Experimental Example 1: Determination of hyaluronic acid loss rate
[0215] After the explosive beads prepared in each example and comparative example were stored in a protective solution (accelerated storage at 37° C. for 12 weeks), the sodium hyaluronate content in the protective solution was determined by high performance liquid chromatography.
[0216] The chromatographic conditions were as follows: the chromatographic column was CAPCELL PAK-NH2 (4.6×250mm, 5μm), the column temperature was 40°C, the mobile phase A was water; the mobile phase B was 0.4 mol / L sodium dihydrogen phosphate solution for gradient elution, the flow rate was 0.6 mL / min, the detection wavelength was 232 nm, and the injection volume was 20 μL.
[0217] Hyaluronic acid loss rate % = sodium hyaluronate content in the protective solution / total amount of sodium hyaluronate added in the explosive beads × 100%
[0218] The test results are shown in Table 2.
[0219] Table 2 Loss rate of sodium hyaluronate in each embodiment and comparative example
[0220]
[0221]
[0222] From the results in Table 2, it can be seen that the sodium hyaluronate loss rate of each embodiment of the present application is significantly reduced compared with Comparative Example 1 (without UV irradiation) and Comparative Example 2 (without secondary cross-linking), which indicates that the introduction of UV irradiation between two cross-linkings can greatly reduce the pores of the gel film and reduce the leakage rate of sodium hyaluronate during the storage of the explosive beads. Comparative Example 1 without UV irradiation and Comparative Example 2 without secondary cross-linking can not effectively reduce the pores of the calcium alginate gel film, resulting in an increase in the leakage rate of sodium hyaluronate.
[0223] Experimental Example 2: Determination of blasting performance
[0224] The blasting performance of the above samples was measured using a Shanghai Baosheng Stable Micro Systems physical property analyzer, and the measurement method was as follows: speed before test 1.00 mm / sec; test speed 5.00 mm / sec; speed after test 10.00 mm / sec, trigger force 1.5 g, and pressure strain 95%. The test results are shown in Table 3.
[0225] Table 3 Texture of popping beads
[0226]
[0227]
[0228] From the results in Table 3, it can be seen that the bursting force of each embodiment of the present application is ≥1000g, and the bursting strain is ≥40%. The introduction of ultraviolet light irradiation between the two crosslinkings can greatly improve the bursting force and bursting strain of the popping beads. Comparative Example 1 was not subjected to ultraviolet irradiation, and Comparative Example 2 was not subjected to secondary crosslinking, and both failed to achieve the optimal bursting force and bursting strain.
[0229] Experimental Example 3: Determination of the thickness of the outer shell
[0230] After the popping beads of each embodiment and comparative example were pierced, the skin of the popping beads was wiped clean and the thickness of the outer shell layer was measured using a Dasque precision 0-25mm electronic micrometer. The results are shown in Table 4.
[0231] Table 4 Shell thickness of the popping beads
[0232]
[0233]
[0234] From the results in Table 4, it can be seen that the film thickness of each embodiment of the present application is between 0.08 and 0.2 mm, and the taste of the popping beads within this range is the best. Introducing ultraviolet light irradiation between two cross-linkings can enhance the rigidity of the calcium alginate film skeleton, shrink the structure, and reduce the film thickness. Comparative Example 1 was not subjected to ultraviolet irradiation, and Comparative Example 2 was not subjected to secondary cross-linking, and both failed to achieve the optimal film thickness.
[0235] The above is only a preferred embodiment of the present application and does not limit the present application in any form. Any technician familiar with the profession may use the above disclosed technical content to change or modify it into an equivalent embodiment with equivalent changes. However, any simple modification, equivalent change and modification made to the above embodiment based on the technical essence of the present application without departing from the content of the technical solution of the present application still falls within the protection scope of the technical solution of the present application.
Claims
1. A method for preparing popping beads, comprising the following steps: (1) preparing a coagulation bath solution, a core material solution and a calcium bath solution respectively; (2) adding the core material liquid into the coagulation bath liquid for primary cross-linking to obtain semi-finished particles; (3) After irradiating the semi-finished product particles with ultraviolet light, adding them into the calcium bath for secondary cross-linking to obtain the popping beads.
2. The preparation method according to claim 1, wherein The coagulation bath solution includes sodium alginate; the core liquid includes calcium salt and hyaluronic acid or its salt; The calcium bath includes a calcium salt.
3. The preparation method according to claim 1, wherein The viscosity of the sodium alginate is 200-1200 cps, preferably 400-1000 cps; and the content of the sodium alginate in the coagulation bath is 0.5-1.5 wt %.
4. The preparation method according to claim 1, wherein In the core liquid, the content of calcium salt is 2-10 wt %, and the content of hyaluronic acid or its salt is 1-10 wt %.
5. The preparation method according to claim 1, wherein In the calcium bath, the content of calcium salt is 2-6wt%.
6. The preparation method according to claim 1, wherein The reaction time of the primary cross-linking is 4 to 17 minutes, preferably 5 to 15 minutes; the reaction time of the secondary cross-linking is 2 to 17 minutes, preferably 3 to 15 minutes.
7. The preparation method according to claim 1, wherein The wavelength of the ultraviolet light is 320nm-380nm, the ultraviolet light irradiation time is 10min-60min, and the light intensity of the ultraviolet light is 1000-2000mJ / cm 2 .
8. The explosive beads obtained according to the preparation method according to any one of claims 1 to 7.
9. A popping bead, wherein: The invention comprises an outer shell layer and an inner layer wrapped by the outer shell layer, wherein the outer shell layer comprises calcium alginate, and the inner layer comprises hyaluronic acid or a salt thereof.
10. The popping beads according to claim 9, wherein: The blasting force of the blasting bead is ≥1000g, the blasting strain is ≥40%, and the thickness of the outer shell layer of the blasting bead is 0.08-0.2mm.
Citation Information
Patent Citations
Juice-coated juice explosive pearl composition and manufacturing method thereof
CN102640963A
Method based on photosensitive biomacromolecule-loaded enzyme to prepare biosensor
CN106324054A
Pulp-exploded pearl food with core-shell structure and preparation method thereof
CN109938143A
Continuous preparation method of hydrogel optical fiber based on reactive spinning
CN110541209A
Preparation method of chitosan / sodium alginate dual-network hydrogel
CN111662464A
Cited By
Clean label blasting bead and preparation method thereof
CN119837172A