Preparation method and application of bimetallic defluorination material
The Fe-Al bimetallic hydroxide was generated by co-precipitation method, which solved the problems of high cost and low adsorption amount of activated alumina adsorbents, and achieved efficient and economical fluoride removal in water. The theoretical maximum adsorption and fluorine removal rate were significant. Improved, and the cost was greatly reduced.
Patent Information
- Application Number
- CN202411298717.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-18
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing activated alumina adsorbents are costly and have low theoretical maximum adsorption amount. The traditional co-precipitation method synthetic materials are complex and expensive to operate, making it difficult to achieve efficient and economical fluoride removal in water.
The preparation method of bimetallic fluorine removal material is adopted to generate Fe-Al bimetallic hydroxide by co-precipitation method, using sodium metaaluminate as an aluminum source, reducing alkali consumption, reducing synthesis cost, and modifying alkali aluminum Improve adsorption performance.
The adsorption efficiency is significantly improved and the cost of use is reduced. The theoretical maximum adsorption volume reaches 29.23 mg/g, the fluorine removal rate can reach 97.90%, and the dose is only one-tenth of that of conventional activated alumina, far lower than the traditional method.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of environmental protection water treatment, and specifically relates to a preparation method and application of a bimetallic defluorination material. Background Art
[0002] Fluoride is one of the essential trace elements for the human body and is beneficial to dental health, especially in preventing tooth decay. However, excessive intake of fluoride can cause serious health effects, including dental fluorosis, skeletal fluorosis, mental decline, hypothyroidism, hyperglycemia, infertility and even osteosarcoma. Fluoride is widely used in many industrial sectors, so a large amount of fluoride-containing wastewater is discharged, such as metal processing, glass, enamel, brick making, semiconductors, coal-fired power plants, electroplating, rubber and fertilizer industries. Fluoride pollution in drinking water is still a health and environmental problem faced by many countries around the world. The maximum fluoride content in drinking water is stipulated to be 1.5 and 1.0 mg / L, but the problem of fluoride poisoning is still widespread around the world.
[0003] Regarding fluoride removal technology, the main methods include ion exchange, chemical precipitation, membrane separation, coagulation, adsorption and reverse osmosis. Among them, the adsorption method removes fluoride ions from water through solid adsorbents. It is simple to operate, low in cost and easy to implement, so it is widely used. Common adsorbents include activated alumina, activated carbon, bone char, ion exchange resins, clay-based materials, metal organic frameworks and layered double hydroxides.
[0004] Activated alumina is one of the most commonly used adsorbents, but its limited adsorption capacity, narrow operating pH range, and easy solubility limit its application in water treatment. In order to improve the adsorption efficiency, a variety of modified adsorbents have been developed, such as modified activated alumina, calcium-based materials, iron-based materials, carbon-based materials, and metal oxides. For example, iron-doped activated alumina can significantly improve the removal efficiency of fluoride ions because its surface positive charge enhances the adsorption capacity of fluoride. Iron salts, as a cheap and effective adsorbent element, are particularly suitable for the synthesis of high-efficiency adsorbent materials. For example, Fe-TNT (Fe 3+ Ion-modified titanate nanotubes) can achieve a fluorine removal efficiency of 96.80% at a dosage of 4.0g / L. However, the performance of single iron oxide for fluorine removal is not ideal enough. Recently, a document prepared a hollow Fe-Al binary metal hydroxide microbox by heat-treated derivatives of Prussian blue analogs, and its theoretical maximum adsorption capacity for fluoride reached 146.59mg / g, which achieved a good breakthrough in performance, but the method is relatively complicated, the raw materials contain polymers, and the cost is relatively expensive. Summary of the invention
[0005] Technical issues solved:
[0006] The cost of currently commonly used activated alumina adsorbents is relatively high, and the theoretical maximum adsorption capacity of fluoride is far below 10 mg / g, which is relatively low. The cost of materials synthesized by the traditional coprecipitation method is relatively high, and the performance improvement is limited. Although the synthesis method assisted by polymer derivatives has significantly improved the performance, it still has the problems of complex operation and high cost. The present invention provides a simpler, cheaper, and environmentally friendly green synthesis method and product of iron and aluminum bimetallic composite materials to achieve efficient and economical removal of fluoride in water.
[0007] Technical solution:
[0008] To achieve the above objectives, this application is implemented through the following technical solutions:
[0009] A method for preparing a bimetallic defluorination material comprises the following steps:
[0010] Step 1: Weigh 2.70g of ferric chloride powder and 0.82-2.50g of sodium aluminate dry powder in different beakers according to the mass-volume ratio, add 100mL and 100-300mL of deionized water to the beakers respectively, stir evenly to obtain ferric chloride solution and sodium aluminate solution.
[0011] Sodium acid solution;
[0012] Step 2: Pour 100 mL of ferric chloride solution into 100-300 mL of sodium aluminate solution, continue stirring at 300 rpm with a magnetic stirrer for 12 hours, and then let it stand for 4 hours;
[0013] Step 3: After the standing period, take out the sample in the beaker and centrifuge it;
[0014] Step 4: After centrifugation, remove the supernatant and wash the sample;
[0015] Step 5: Place the sample washed in step 4 into an oven and dry to constant weight to obtain a bimetallic defluorination material.
[0016] Furthermore, in the third step, the centrifugation is performed at 4000-5000 r / min for 3-5 min.
[0017] Furthermore, the washing step in the fourth step is washing once with distilled water, then washing once with ethanol, and finally washing once with distilled water.
[0018] Furthermore, in the fifth step, the drying temperature is 60-100° C., and the drying time is 4-12 hours.
[0019] The present application also discloses the use of the bimetallic defluorination material prepared by any of the above preparation methods in water treatment and defluorination.
[0020] Beneficial effects:
[0021] The present application provides a preparation method and application of a bimetallic defluorination material, which has the following beneficial effects compared with the prior art:
[0022] 1. The synergistic effect between different metals can significantly improve the performance of the adsorption material. The present application uses sodium aluminate as a new aluminum source, and generates Fe-Al double metal hydroxide with ferric chloride by coprecipitation. Sodium aluminate not only has the ability to neutralize acidic solutions, but also provides aluminum elements. The alkalinity of alkaline aluminum is used to achieve composite modification of the two metals. Different from the conventional coprecipitation method, on the one hand, no external alkali is required, which reduces the consumption of alkali. On the other hand, the cost of sodium aluminate is much lower than that of aluminum chloride (about half of the latter), which greatly reduces the synthesis cost of this method.
[0023] 2. This application can simultaneously achieve different basicity and bimetallic ratios through basic aluminum, with simple operation, adjustable components and easy process control;
[0024] 3. Excellent performance, high fluoride removal efficiency, and low use cost. The adsorbent of the present invention is used to treat a water sample with an initial fluoride concentration of 10 mg / L to meet the drinking water standard. Its dosage is only 0.62 g / L, which is much lower than the similar index of alumina, the latter of which is generally greater than 5 g / g. The dosage of the product of this method is one tenth of that of conventional activated alumina, which significantly reduces the operating cost;
[0025] 4. The theoretical maximum adsorption capacity of the material of the present application can reach 29.23 mg / g, which is significantly improved in adsorption performance compared with traditional activated alumina (<7 mg / g) and iron oxide (<10 mg / g). Under the adsorption conditions of actual initial fluoride concentration of 10 mg / L, adsorbent dosage of 0.75 g / L, and pH of 7, the defluorination rate of the defluoridation agent can reach 97.90%, and the actual adsorption capacity is between 12 and 13 mg / g, which is much greater than the sum of the adsorption capacities of its components, alumina (1.26 mg / g) and iron oxide (1.04 mg / g), not to mention that it is much greater than the sum of the adsorption capacities of the equivalent components of the adsorbent composition. Therefore, the adsorption capacity of this method and the composite material synthesized by this method is much greater than the sum of the adsorption capacities of each component, and has significant technical advancement and substance. DETAILED DESCRIPTION
[0026] In order to further illustrate the present invention, the present invention is further described in detail below in conjunction with embodiments.
[0027] Example 1
[0028] A method for preparing a Fe-Al bimetallic defluorination material comprises the following steps:
[0029] Step 1: Weigh 2.7 g of ferric chloride powder and 2.05 g of sodium aluminate dry powder in different beakers according to the mass-volume ratio, add 100 mL and 250 mL of deionized water to the beakers respectively, stir evenly to obtain ferric chloride solution and sodium aluminate solution;
[0030] Step 2: Pour 100 mL of ferric chloride solution into 250 mL of sodium aluminate solution, continue stirring at 300 rpm with a magnetic stirrer for 12 h, and then let it stand for 4 h;
[0031] Step 3: After standing, centrifuge the sample in the beaker at 4000-5000r / min for 3-5min;
[0032] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;
[0033] Step 5: Place the washed sample in step 4 into an oven and dry it at 100°C for 4 hours. Dry the product to constant weight to obtain the bimetallic defluorination material P01.
[0034] The application of Fe-Al bimetallic defluorination material in water treatment and defluorination. The above P01 sample is placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 0.75 g / L adsorbent dosage, and pH 7. The defluorination rate of the sample can reach 97.90%, and the experimental adsorption amount is 12.61 mg / g.
[0035] Example 2
[0036] A method for preparing a bimetallic defluorination material comprises the following steps:
[0037] Step 1: Weigh 2.7 g of ferric chloride powder and 2.25 g of sodium aluminate dry powder in different beakers according to the mass-volume ratio, add 100 mL and 275 mL of deionized water to the beakers respectively, stir evenly to obtain ferric chloride solution and sodium aluminate solution;
[0038] Step 2: Pour 100 mL of ferric chloride solution into 275 mL of sodium aluminate solution, continue stirring at 300 rpm with a magnetic stirrer for 12 h, and then let it stand for 4 h;
[0039] Step 3: After standing, centrifuge the sample in the beaker at 4000-5000r / min for 3-5min;
[0040] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;
[0041] Step 5: Place the washed sample in step 4 into an oven and dry it at 100°C for 4 hours. Dry the product to constant weight to obtain the bimetallic defluorination material P02.
[0042] The application of Fe-Al bimetallic defluorination material in water treatment and defluorination. The above P02 sample is placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 0.75 g / L adsorbent dosage, and pH 7. The defluorination rate of the sample can reach 94.48%, and the experimental adsorption amount is 12.1 mg / g.
[0043] Example 3
[0044] A method for preparing a Fe-Al bimetallic defluorination material comprises the following steps:
[0045] Step 1: Weigh 2.7 g of ferric chloride powder and 2.50 g of sodium aluminate dry powder in different beakers according to the mass-volume ratio, add 100 mL and 250 mL of deionized water to the beakers respectively, stir evenly to obtain ferric chloride solution and sodium aluminate solution;
[0046] Step 2: Mix the above two salt solutions, continue stirring at 300 rpm with a magnetic stirrer for 12 hours, and then let it stand for 4 hours;
[0047] Step 3: After standing, centrifuge the sample in the beaker at 4000-5000r / min for 3-5min;
[0048] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;
[0049] Step 5: Place the washed sample in step 4 into an oven and dry it at 100°C for 4 hours. Dry the product to constant weight to obtain the bimetallic defluorination material P03.
[0050] The application of Fe-Al bimetallic defluorination material in water treatment and defluorination. The above P03 sample is placed under the adsorption conditions of 10 mg / L initial fluoride ion concentration, 0.75 g / L adsorbent dosage, and pH 7. The defluorination rate of the sample can reach 90.40%, and the experimental adsorption amount is 12.04 mg / g.
[0051] Comparative Example 1
[0052] A method for preparing activated alumina:
[0053] Step 1: The activated alumina used in this comparative example was purchased from a supplier without any modification.
[0054] Step 2: The above sample was placed in an initial fluoride ion concentration of 10 mg / L, an activated alumina adsorbent dosage of 5 g / L, and under adsorption conditions of pH 6 (optimal pH conditions), the activated alumina defluorination rate reached 63%. The adsorption capacity was only 1.26 mg / g.
[0055] Comparative Example 2
[0056] A method for preparing iron oxide:
[0057] Step 1: The iron oxide used in this comparative example was purchased from a supplier without any modification.
[0058] Step 2: The above sample was placed in an initial fluoride ion concentration of 10 mg / L, an activated alumina adsorbent dosage of 5 g / L, and under adsorption conditions of pH 6 (optimal pH conditions), the iron oxide fluoride removal rate reached 52%. The adsorption capacity was only 1.04 mg / g.
[0059] Comparative Example 3
[0060] A method for preparing a conventional Fe-Al bimetallic oxide:
[0061] Step 1: Weigh 2.7g of ferric chloride powder, 6.04g of aluminum chloride powder, and 4g of sodium hydroxide in different beakers according to the mass ratio, add 100mL, 250mL, and 100mL of deionized water to the beakers respectively, and stir evenly;
[0062] Step 2: Pour 100 mL of sodium hydroxide solution into a mixed solution of 250 mL of aluminum chloride and 100 mL of ferric chloride, continue stirring at 300 rpm with a magnetic stirrer for 12 hours, and then let it stand for 4 hours;
[0063] Step 3: After standing, centrifuge the sample in the beaker at 4000-5000r / min for 3-5min;
[0064] Step 4: After centrifugation, remove the supernatant and wash the sample once with distilled water, then once with ethanol, and then once with distilled water;
[0065] Step 5: Place the washed sample in step 4 in an oven at 100°C for 4 hours and dry the product to constant weight to obtain a conventional Fe-Al bimetallic defluorination material, denoted as D01.
[0066] When the above adsorbent is placed under the adsorption conditions of an initial fluoride ion concentration of 10 mg / L, a bimetallic adsorbent dosage of 0.75 g / L, and a pH of 7 (optimal pH conditions), the fluoride removal rate of iron oxide reaches 95.41% and the adsorption capacity is 12.72 mg / g.
[0067] In the above embodiments, the bimetallic defluorination adsorbent synthesized by the preparation method of the present application has an actual adsorption amount greater than 12 mg / g in the adsorption experiment of simulated wastewater, which is much greater than the sum of the adsorption amounts of aluminum oxide (1.26 mg / g) and iron oxide (1.04 mg / g) in the comparative example, and a higher defluorination rate is achieved at a very low dose (0.75 g / L) than that of high dose (all 5 g / g) iron oxide / aluminum oxide, and the performance improvement is beyond expectations; although the composite material synthesized by the conventional coprecipitation method in comparative example D01 also has a similar defluorination effect, in order to obtain the same alkalinity and ratio as the embodiment, the conventional method raw materials are not only of many types (additional alkali needs to be added), large in amount (aluminum chloride), but also high in price (the price of aluminum chloride trihydrate is about twice that of sodium aluminate), and the cost is significantly increased; in short, the preparation method of the present application and the material synthesized by the preparation method achieve unexpected beneficial effects such as large adsorption amount, small amount, high defluorination rate, and low cost, so the present application is technologically progressive and substantial.
[0068] The present invention is described above by way of example. It should be noted that, without departing from the core of the present invention, any simple deformation, modification or other equivalent replacement that can be made by those skilled in the art without inventive effort falls within the protection scope of the present invention.
Claims
1. A method for preparing a bimetallic defluorination material, characterized in that: The specific steps include: Step 1: Weigh 2.70g of ferric chloride powder and 0.82-2.50g of sodium aluminate dry powder in different beakers according to the mass-volume ratio, add 100mL and 100-300mL of deionized water to the beakers respectively, stir evenly to obtain ferric chloride solution and sodium aluminate solution; Step 2: Pour 100 mL of ferric chloride solution into 100-300 mL of sodium aluminate solution, continue stirring at 300 rpm with a magnetic stirrer for 12 hours, and then let it stand for 4 hours; Step 3: After the standing period, take out the sample in the beaker and centrifuge it; Step 4: After centrifugation, remove the supernatant and wash the sample; Step 5: Place the sample washed in step 4 into an oven and dry to constant weight to obtain a bimetallic defluorination material.
2. The method for preparing the bimetallic defluorination material according to claim 1, characterized in that: The centrifugation in the third step is specifically performed at 4000-5000 r / min for 3-5 min.
3. The method for preparing the bimetallic defluorination material according to claim 1, characterized in that: The washing step in the fourth step is washing once with distilled water, then washing once with ethanol, and finally washing once with distilled water.
4. The method for preparing the bimetallic defluorination material according to claim 1, characterized in that: In the fifth step, the drying temperature is 60-100° C. and the drying time is 4-12 hours.
5. Use of a bimetallic defluorination material prepared by the preparation method according to any one of claims 1 to 4 in water treatment and defluorination.
Citation Information
Patent Citations
Method for synthesizing composite hydroxide of iron and aluminum, and application
CN101049972A
Method for preparing iron-titanium oxide serving as defluorination adsorbent
CN102886239A
Preparation method of submicron Fe-Al-Mg composite metal oxide fluorine remover
CN108014746A
Drinking water fluorine removal agent and preparation method and application thereof
CN111569818A
Preparation method and application of metal-doped alumina hydrate with high adsorption performance
CN115501852A