Preparation method and application of metal-supported catalyst of hydrotalcite and derivative
Through the combination of magnesium-aluminum hydrotalcite and its composite metal oxides and precious metals, a supported catalyst is constructed, which solves the problems of high cost and poor stability of existing precious metal catalysts, and achieves efficient catalytic degradation and stability improvement of volatile organic compounds.
Patent Information
- Application Number
- CN202411007976.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-25
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The existing supported precious metal catalysts have problems of high cost, easy poisoning and poor thermal stability in the catalytic degradation of volatile organic matter, and hydrotalcite supported metal catalysts are rarely used in this field.
Magnesium-aluminum hydrotalcite and its calcined composite metal oxide combined with precious metal impregnation reduction to construct a supported hydrotalcite and composite metal oxide catalyst. Through pre-activation and ultrasonic dispersion, efficient dispersion of active sites is achieved and the activity of the catalyst is improved. and stability.
The prepared catalyst has high dispersion and high specific surface area, achieves high selectivity and high activity, exhibits efficient catalytic degradation properties in catalytic oxidation of toluene, and remains stable in the presence of water vapor.
Smart Images

Figure CN118949977A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a preparation method and application of a catalyst, in particular to a preparation method and application of a supported metal catalyst of hydrotalcite and its derivatives, belonging to the field of catalysts. Background Art
[0002] Volatile organic compounds (VOCs) have attracted increasing attention due to their serious harm to the ecological environment and human health. Therefore, various VOC reduction technologies have been developed, such as adsorption, biofiltration, photocatalysis, and catalytic oxidation. Among them, catalytic oxidation is an efficient technology that catalytically converts VOCs into water, carbon dioxide, and less harmful molecules under mild conditions. The key issue is to develop high-performance catalysts with high activity, high stability, and low cost. It is well known that supported precious metal catalysts show good catalytic performance for the catalytic degradation of VOCs, but they have limitations such as high cost, easy poisoning, and poor thermal stability. It is highly desired to develop supported precious metal catalysts by selecting suitable carriers to provide highly dispersed active sites for the effective degradation of VOCs.
[0003] Layered double hydroxide (LDHs)-based materials have become one of the latest and most attractive topics as novel catalysts in recent years. LDHs are tunable in chemical composition, electronic structure, and morphology, have unique structural features, and superior physicochemical properties, showing great potential in environmental applications. Summary of the invention
[0004] In view of this, the present invention provides a preparation method and application of a supported metal catalyst of hydrotalcite and its derivatives. Existing hydrotalcite-supported metal catalysts are rarely used in VOCs catalytic degradation applications. The present invention adopts magnesium-aluminum hydrotalcite and composite metal oxides obtained by calcining the composite metal oxides combined with precious metal impregnation reduction to construct corresponding supported hydrotalcite and supported composite metal oxide catalysts for catalytic oxidation of toluene, which can effectively disperse active sites and provide diffusion activation sites for VOCs and O2, thereby achieving efficient catalytic degradation performance, and achieving high selectivity, high activity and high stability.
[0005] In order to achieve the above object, the present invention adopts the following technical solution:
[0006] A method for preparing a metal-loaded catalyst of hydrotalcite and its derivatives, wherein the catalyst is loaded with a single metal or a double metal, comprising the following steps:
[0007] S1. Mixing an aluminum compound, a magnesium compound and urea in ultrapure water, heating and stirring until the reaction is complete;
[0008] S2. After the reaction is complete, stirring is stopped for aging, the precipitate is filtered, washed with ultrapure water, and dried to obtain magnesium aluminum hydrotalcite;
[0009] S3, calcining magnesium aluminum hydrotalcite to obtain magnesium aluminum composite oxide;
[0010] S4, pre-activating magnesium aluminum hydrotalcite or magnesium aluminum composite oxide and ultrasonically dispersing it in ultrapure water, adding chloroplatinic acid solution or silver nitrate solution under stirring conditions to mix evenly, centrifugally separating the precipitate, washing and drying, and re-dispersing it in ultrapure water, adding sodium borohydride and sodium hydroxide under stirring conditions to react, centrifugally separating the precipitate and vacuum drying to obtain silver-loaded and platinum-loaded hydrotalcite and magnesium aluminum composite oxide, respectively;
[0011] S5. Disperse the silver-loaded hydrotalcite in ultrapure water, add chloroplatinic acid solution dropwise while stirring under a nitrogen atmosphere, heat to reflux for reaction, centrifuge and wash, and vacuum dry to obtain bimetallic-loaded hydrotalcite.
[0012] On the basis of the above technical solution, the present invention further defines the solution as follows:
[0013] Further, in step S1, the molar ratio of the aluminum compound to the magnesium compound is 1:5 to 6:1; the molar ratio of urea to the aluminum compound is 5:1 to 20:1;
[0014] The heating and stirring temperature is 95-120°C and the time is 8-12h.
[0015] Furthermore, the aluminum compound is one of AlCl3, Al2(NO3)3, and Al2(SO4)3; the magnesium compound is one of MgCl2, Mg(NO3)2, and MgSO4.
[0016] Further, the aging time in step S2 is 12 to 24 hours;
[0017] Washing was performed by centrifugation three times with ultrapure water;
[0018] The drying temperature is 60-90°C and the time is 12-24 hours.
[0019] Furthermore, in step S3, the calcination temperature is 500-700° C. and the calcination time is 1-5 hours.
[0020] Further, in step S4, the amount of chloroplatinic acid solution added is 1 to 50 mmol, and the amount of silver nitrate solution added is 1 to 50 mmol;
[0021] The amount of sodium borohydride added is 0.1-0.5 mol, and the amount of sodium hydroxide added is 0.2-0.8 mol.
[0022] Further, the pre-activation temperature in step S4 is 120-150° C. and the time is 8-12 h;
[0023] The reaction time under stirring conditions is 0.5 to 2 hours;
[0024] The centrifugal speed is 8000-10000 rpm, and the washing is performed by centrifugal washing three times with ultrapure water;
[0025] The vacuum drying temperature is 60-90°C and the time is 12-24 hours.
[0026] Further, in step S5, the temperature of the heating reflux reaction is 80 to 120° C., and the time is 0.5 to 2 h;
[0027] The centrifugal speed is 8000-10000 rpm, and the washing is performed by centrifugal washing three times with ultrapure water;
[0028] The vacuum drying temperature is 60 to 90°C and the time is 12 to 24 hours.
[0029] The present invention also provides the use of a supported metal catalyst of the hydrotalcite and its derivatives prepared by the above preparation method in the catalytic degradation of volatile organic compounds, wherein the volatile organic compound is toluene.
[0030] The beneficial effects of the present invention are:
[0031] The present invention adopts magnesium aluminum hydrotalcite and the composite metal oxide obtained by calcining thereof in combination with noble metal impregnation reduction and substitution reaction to construct the corresponding hydrotalcite and composite metal oxide supported metal catalyst. The prepared catalyst has better dispersibility and higher specific surface area, thus having higher catalytic activity, and the obtained material has certain resistance to the influence of water vapor, thus having higher catalytic activity and stability, and achieving high selectivity and high activity in catalytic oxidation of toluene. BRIEF DESCRIPTION OF THE DRAWINGS
[0032] Figure 1 The X-ray powder diffraction pattern of the supported hydrotalcite prepared in the present invention;
[0033] Figure 2 This is a TEM image of the supported hydrotalcite prepared in the present invention;
[0034] Figure 3 This is a graph showing the results of a degradation test of toluene by the supported magnesium aluminum hydrotalcite catalyst provided in Examples 1-4 of the present invention;
[0035] Figure 4 This is a graph showing the degradation test results of toluene by the supported magnesium aluminum hydrotalcite catalyst provided in Examples 1-4 of the present invention;
[0036] Figure 5 This is a graph showing the results of a test on toluene degradation by the supported composite metal oxide catalyst provided in Examples 5 and 6 of the present invention;
[0037] Figure 6 This is a graph showing the test results of catalytic degradation of toluene by the platinum-supported hydrotalcite catalyst provided in Example 2 of the present invention in the presence of water vapor;
[0038] Figure 7 This is a graph showing the test results of the catalytic degradation of toluene by the silver-supported hydrotalcite catalyst provided in Example 3 of the present invention in the presence of water vapor;
[0039] Figure 8 This is a graph showing the test results of catalytic degradation of toluene in the presence of water vapor by the platinum-silver bimetallic supported hydrotalcite catalyst provided in Example 4 of the present invention;
[0040] Fig. 9 This is a graph showing the test results of catalytic degradation of toluene by the supported composite metal oxide catalyst in Example 6 of the present invention in the presence of water vapor. DETAILED DESCRIPTION
[0041] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0042] Example 1
[0043] The preparation method of magnesium aluminum hydrotalcite is as follows:
[0044] 0.75g aluminum nitrate, 1.54g magnesium nitrate, and 2.4g urea were dissolved in 60mL ultrapure water and reacted for 10 hours in an oil bath at 105°C. After aging for 12 hours, the mixture was separated by suction filtration, washed with ultrapure water three times, and dried at 60°C for 12 hours to obtain MgAl-LDH. Its X-ray powder diffraction pattern is shown below: Figure 1 shown.
[0045] Example 2
[0046] The preparation method of platinum-loaded magnesium aluminum hydrotalcite is as follows:
[0047] The MgAl-LDH obtained in Example 1 was pre-activated in a vacuum oven at 120°C for 12 hours; 0.2 g of the activated MgAl-LDH was ultrasonically dispersed in 50 mL of ultrapure water; under stirring, a chloroplatinic acid solution prepared with a theoretical loading of 2 wt% was added, and the mixture was stirred at room temperature for 0.5 hours. The stirred sample was centrifuged and washed. The solid obtained after drying was redispersed in ultrapure water, and 5 mL of freshly prepared sodium borohydride and sodium hydroxide solution was quickly added under stirring and continued to be stirred for 30 minutes; after centrifugal separation and washing 3 times, it was vacuum dried at 120°C to obtain highly dispersed, highly active, and high specific surface area Pt / MgAl-LDH. Its X-ray powder diffraction pattern and transmission electron microscope image are shown as follows. Figure 1 and Figure 2 shown.
[0048] Example 3
[0049] The preparation method of silver-loaded magnesium aluminum hydrotalcite is as follows:
[0050] The steps are the same as those in Example 2, except that: MgAl-LDH is pre-activated in a vacuum oven at 120°C for 12 hours; 0.2 g of the activated MgAl-LDH is ultrasonically dispersed in 50 mL of ultrapure water; under stirring, a silver nitrate solution prepared with a theoretical loading of 6 wt% is added, and the mixture is stirred at room temperature for 0.5 hours. The stirred sample is centrifuged and washed. After drying, the obtained solid is redispersed in ultrapure water, and 5 mL of freshly prepared sodium borohydride and sodium hydroxide solutions are quickly added under stirring and stirring is continued for 30 minutes; after centrifugal separation and washing 3 times, it is vacuum dried at 120°C to obtain highly dispersed, highly active, and high specific surface area Ag / MgAl-LDH. Its X-ray powder diffraction pattern is shown as follows Figure 1 shown.
[0051] Example 4
[0052] The preparation method of platinum-silver loaded magnesium-aluminum hydrotalcite is as follows:
[0053] The Ag / MgAl-LDH obtained in Example 3 was ultrasonically dispersed in 50 mL of ultrapure water under nitrogen protection; under stirring, a 1 wt% platinum chloride solution was added dropwise, and the mixture was stirred and refluxed at 100°C for 1 hour. After the reaction, the sample was centrifuged and washed 3 times, and then vacuum dried at 120°C to obtain AgPt / MgAl-LDH. Its X-ray powder diffraction pattern is shown in FIG. Figure 1 shown.
[0054] Example 5
[0055] The preparation method of the composite metal oxide based on magnesium aluminum hydrotalcite is as follows:
[0056] The MgAl-LDH obtained in Example 1 was calcined in a muffle furnace at 400 degrees for 2 hours to obtain a composite metal oxide.
[0057] Example 6
[0058] The preparation method of the platinum-loaded composite metal oxide is as follows:
[0059] The composite metal oxide obtained in Example 5 was pre-activated in a vacuum oven at 120°C for 12 hours; 0.2g of the activated composite metal oxide was ultrasonically dispersed in 50mL of ultrapure water; under stirring, a chloroplatinic acid solution prepared with a theoretical loading of 2wt% was added, and the mixture was stirred at room temperature for 0.5 hours, and the stirred sample was centrifuged and washed. After drying, the obtained solid was redispersed in ultrapure water, and 5mL of freshly prepared sodium borohydride and sodium hydroxide solution was quickly added under stirring and continued to stir for 30 minutes; after centrifugal separation and washing for 3 times, it was vacuum dried at 120°C to obtain a highly dispersed, highly active, and high specific surface area platinum-loaded composite metal oxide.
[0060] Example 7
[0061] Comparison of degradation tests on toluene using the supported magnesium aluminum hydrotalcite catalysts provided in Examples 1-4:
[0062] The catalyst activity evaluation was carried out in a fixed bed continuous flow reactor. The reactor was a quartz glass tube with an inner diameter of 6 mm. The catalyst loading was 20 mg, the feed gas concentration was 500 ppm, and the gas flow rate was 20 mL / min. After 1 to 2 hours of reaction, the volatile organic pollutants in the product gas were analyzed online by a Kechuang GC-9800 gas chromatograph equipped with a hydrogen ion flame detector. The reaction activity was expressed by the toluene conversion rate and carbon dioxide yield. The results are shown in Figure 2. Figure 3 , 4 shown.
[0063] Depend on Figure 3 and Figure 4 Analysis shows that Example 2, namely Pt / MgAl-LDH, has the best catalytic effect, and the temperature for complete degradation of toluene is 220°C, and toluene can be completely converted into carbon dioxide at 220°C. The catalytic effect of Example 4, namely AgPt / MgAl-LDH, is second, and the complete degradation temperature is 260°C, which is due to the low loading of platinum. Example 3, namely Ag / MgAl-LDH, has basically no effect at low temperatures and needs to be completely degraded at high temperatures, and its complete degradation temperature is 300°C. For Example 1, namely MgAl-LDH, it has basically no catalytic effect on toluene degradation. These show that the supported hydrotalcite catalyst has high catalytic activity and selectivity.
[0064] Example 8
[0065] Comparison of toluene degradation tests conducted using supported composite metal oxide catalysts provided in Examples 5 and 6:
[0066] The catalyst activity evaluation was carried out in a fixed bed continuous flow reactor. The reactor was a quartz glass tube with an inner diameter of 6 mm. The catalyst loading was 20 mg, the feed gas concentration was 500 ppm, and the gas flow rate was 20 mL / min. After 1 to 2 hours of reaction, the volatile organic pollutants in the product gas were analyzed online by a Kechuang GC-9800 gas chromatograph equipped with a hydrogen ion flame detector. The reaction activity was expressed by the toluene conversion rate and carbon dioxide yield. The results are shown in Figure 2. Figure 5 shown.
[0067] Depend on Figure 5 It can be seen that the composite metal oxide obtained by calcining hydrotalcite, that is, Example 5, has almost no catalytic activity for toluene. However, the platinum-loaded composite metal oxide obtained in Example 6 has greatly improved catalytic activity, and its complete degradation temperature is 160°C.
[0068] Example 9
[0069] Comparison of the catalytic degradation test of toluene in the presence of water vapor by the supported hydrotalcite provided in Examples 2, 3, and 4 and the supported composite metal oxide catalyst in Example 6:
[0070] The catalyst activity was evaluated in a fixed bed continuous flow reactor. The reactor was a quartz glass tube with an inner diameter of 6 mm, the catalyst loading was 20 mg, the feed gas concentration was 500 ppm, and the gas flow rate was 20 mL / min. At the complete degradation temperature corresponding to the embodiment, the change of catalytic performance over time was investigated. In addition, 15% by volume of H2O was introduced into the reaction gas through a water saturator to study the effect of water vapor on the catalytic activity. The results are shown in Figure 2. Figure 6-9 shown.
[0071] Depend on Figure 6-Figure 9 It can be seen that the catalytic activities of platinum, silver and platinum-silver loaded hydrotalcite and platinum loaded composite metal oxides are basically not affected by water vapor, indicating that the prepared supported hydrotalcite catalyst and supported composite metal oxide have high catalytic activity, selectivity and stability.
Claims
1. A method for preparing a supported metal catalyst of hydrotalcite and its derivatives, It is characterized in that The catalyst is loaded with a single metal or a double metal, comprising the following steps: S1. Mixing an aluminum compound, a magnesium compound and urea in ultrapure water, heating and stirring until the reaction is complete; S2. After the reaction is complete, stirring is stopped for aging, the precipitate is filtered, washed with ultrapure water, and dried to obtain magnesium aluminum hydrotalcite; S3, calcining magnesium aluminum hydrotalcite to obtain magnesium aluminum composite oxide; S4, pre-activating magnesium aluminum hydrotalcite or magnesium aluminum composite oxide and ultrasonically dispersing it in ultrapure water, adding chloroplatinic acid solution or silver nitrate solution under stirring conditions to mix evenly, centrifugally separating the precipitate, washing and drying, and re-dispersing it in ultrapure water, adding sodium borohydride and sodium hydroxide under stirring conditions to react, centrifugally separating the precipitate and vacuum drying to obtain silver or platinum loaded hydrotalcite and magnesium aluminum composite oxide respectively; S5. Disperse the silver-loaded hydrotalcite in ultrapure water, add chloroplatinic acid solution dropwise while stirring under a nitrogen atmosphere, heat to reflux for reaction, centrifuge and wash, and vacuum dry to obtain bimetallic-loaded hydrotalcite.
2. The method for preparing the supported metal catalyst of hydrotalcite and its derivatives according to claim 1, It is characterized in that In step S1, the molar ratio of the aluminum compound to the magnesium compound is 1:5 to 6:1; the molar ratio of urea to the aluminum compound is 5:1 to 20:1; The heating and stirring temperature is 95-120°C and the time is 8-12h.
3. A method for preparing a supported metal catalyst of hydrotalcite and its derivatives according to claim 1 or 2, It is characterized in that The aluminum compound is AlCl 3 、Al 2 (NO 3 ) 3 、Al 2 (SO 4 ) 3 One of the following; the magnesium compound is MgCl 2 Mg(NO 3 ) 2 MgSO 4 One of them.
4. The method for preparing the supported metal catalyst of hydrotalcite and its derivatives according to claim 1, It is characterized in that The aging time in step S2 is 12 to 24 hours; Washing was performed by centrifugation three times with ultrapure water; The drying temperature is 60-90°C and the time is 12-24 hours.
5. The method for preparing the supported metal catalyst of hydrotalcite and its derivatives according to claim 1, It is characterized in that The calcination temperature in step S3 is 500-700° C. and the calcination time is 1-5 hours.
6. The method for preparing the supported metal catalyst of hydrotalcite and its derivatives according to claim 1, It is characterized in that In step S4, the amount of chloroplatinic acid solution added is 1 to 50 mmol, and the amount of silver nitrate solution added is 1 to 50 mmol; The amount of sodium borohydride added is 0.1-0.5 mol, and the amount of sodium hydroxide added is 0.2-0.8 mol.
7. A method for preparing a supported metal catalyst of hydrotalcite and its derivatives according to claim 1 or 6, It is characterized in that The pre-activation temperature in step S4 is 120-150° C. and the time is 8-12 hours; The reaction time under stirring conditions is 0.5 to 2 hours; The centrifugal speed is 8000-10000 rpm, and the washing is performed by centrifugal washing three times with ultrapure water; The vacuum drying temperature is 60-90°C and the time is 12-24 hours.
8. The method for preparing the supported metal catalyst of hydrotalcite and its derivatives according to claim 1, It is characterized in that In step S5, the temperature of the heating reflux reaction is 80-120° C. and the time is 0.5-2 h; The centrifugal speed is 8000-10000 rpm, and the washing is performed by centrifugal washing three times with ultrapure water; The vacuum drying temperature is 60 to 90°C and the time is 12 to 24 hours.
9. Use of the supported metal catalyst of the hydrotalcite and its derivatives prepared by the preparation method according to any one of claims 1 to 8 in the catalytic degradation of volatile organic compounds.
10. The use according to claim 9, It is characterized in that The volatile organic compound is toluene.
Citation Information
Patent Citations
Preparation of loaded bimetallic nano-catalyst
CN102773097A
Preparation method and application of aluminum-magnesium-holmium composite oxide loaded samarium-platinum catalyst prepared from hydrotalcite and carbon precursor
CN111185165A
Preparation method and application of gadolinium terbium nickel magnesium aluminum composite supported platinum catalyst taking hydrotalcite as precursor
CN111185195A
Catalyst for catalyzing formaldehyde at room temperature and preparation method thereof
CN115739113A