Ru-based catalyst as well as preparation method and application thereof

By supporting Ru on the cerium-tin composite oxide support, Ru-based catalyst with excellent low-temperature activity and N2 selectivity was prepared, which solved the problems of insufficient low-temperature activity and excessive by-products in the existing NH3-SCO technology, and achieved high efficiency catalytic oxidation effect of ammonia.

CN118949979AActive Publication Date: 2024-11-15INST OF URBAN ENVIRONMENT CHINESE ACAD OF SCI
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411165218.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-23
Publication Date
2024-11-15
Estimated Expiration
2044-08-23

AI Technical Summary

Technical Problem

In the existing ammonia-selective catalytic oxidation (NH3-SCO) technology, precious metal catalysts have insufficient low temperature activity and N2 selectivity, and too many by-products such as N2O and NOx, which affects the environmental protection effect.

Method used

The Ru-based catalyst is prepared by using cerium-tin composite oxide as the support and Ru as the active component to ensure the good dispersion and low-temperature activity of Ru, and improve the low-temperature activity and N2 selectivity of the catalyst.

Benefits of technology

The excellent low-temperature activity and N2 selectivity of the catalyst are achieved, the generation of by-products is reduced, the market demand is met, and there is good practical application prospect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118949979A_ABST
    Figure CN118949979A_ABST
Patent Text Reader

Abstract

The invention relates to a Ru-based catalyst as well as a preparation method and application thereof. The Ru-based catalyst comprises a cerium-tin composite oxide carrier and an active component Ru loaded on the carrier, the total mass of the Ru-based catalyst is 100 wt%, the content of the active component Ru is 0.5-2 wt%, and the balance is the cerium-tin composite oxide carrier; the cerium-tin composite oxide is used as the carrier, the Ru is used as the active component to prepare the catalyst, the Ru has good dispersity, the catalyst can have good low-temperature activity, N2 selectivity and thermal stability under the condition that the content of the active component is low, and compared with a conventional catalyst carrier, the catalyst has the advantages that the cost is low; the cerium-tin composite oxide carrier has certain catalytic activity, and after Ru is loaded on the cerium-tin composite oxide carrier, oxygen vacancies and active sites are increased, so that the catalytic activity is further improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of catalysts, and in particular to a Ru-based catalyst and a preparation method and application thereof. Background Art

[0002] Ammonia (NH3) in the environment mainly comes from agriculture, animal husbandry, industry, transportation and other aspects, and its emissions directly affect the environment and human health. The emission of ammonia in motor vehicle exhaust is considered to be the main source of ammonia in cities, including gasoline vehicles equipped with three-way catalysts and diesel vehicles using urea selective catalytic reduction (NH3-SCR) denitrification technology. In particular, the latter, in the use of NH3-SCR exhaust, nitrogen oxides (NO x ) process, NH3 slip is likely to occur, so it is necessary to add an NH3 purification device at the end of the NH3-SCR purification system.

[0003] At present, the control technologies of NH3 pollution mainly include biological method, adsorption method, catalytic decomposition method, photocatalysis and ammonia selective catalytic oxidation (NH3-SCO). Among them, NH3-SCO is an efficient and environmentally friendly NH3 purification technology, and its core is an efficient and stable NH3 oxidation catalyst. NH3 oxidation catalysts mainly include precious metal catalysts, modified zeolite catalysts and transition metal oxide catalysts. Precious metal catalysts are generally considered to be the most effective NH3 oxidation catalysts because they have excellent NH3 oxidation activity. For example, Pt / Al2O3 catalyst is currently a commercial NH3 oxidation catalyst. However, due to the excessive oxidation of NH3, more by-products such as N2O and NO are produced. x wait.

[0004] Therefore, it is urgent to develop an NH3-SCO catalyst with excellent low-temperature activity and high N2 selectivity. Summary of the invention

[0005] In order to solve the above technical problems, the purpose of the present invention is to provide a Ru-based catalyst and a preparation method and use thereof. The Ru-based catalyst has good low-temperature activity, N2 selectivity and thermal stability, the preparation method is simple, has excellent low-temperature activity and N2 selectivity, can meet the current market demand, and has good practical application prospects.

[0006] To achieve this object, the present invention adopts the following technical solutions:

[0007] In the first aspect, the present invention provides a Ru-based catalyst, which includes a cerium-tin composite oxide carrier and an active component Ru loaded on the carrier; based on the total mass of the Ru-based catalyst as 100wt%, the content of the active component Ru is 0.5-2.0wt%, for example, it can be 0.5wt%, 0.6wt%, 0.7wt%, 0.8wt%, 0.9wt%, 1.0wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt% or 2.0wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, and the balance is the cerium-tin composite oxide carrier.

[0008] The Ru-based catalyst of the present invention adopts a cerium-tin composite oxide as a carrier and Ru as an active component. Ru has good dispersion. The active component can make the catalyst have good low-temperature activity, N2 selectivity and thermal stability at a relatively low content. Compared with conventional catalyst carriers, the cerium-tin composite oxide carrier of the present invention itself has certain catalytic activity. After Ru is loaded thereon, oxygen vacancies and active sites are increased, thereby further improving the catalytic activity of the catalyst.

[0009] The following are preferred technical solutions of the present invention, but are not intended to limit the technical solutions provided by the present invention. Through the following preferred technical solutions, the technical objectives and beneficial effects of the present invention can be better achieved and realized.

[0010] Preferably, the chemical formula of the cerium-tin composite oxide support is Ce x Sn 1-x O2, wherein 0.20≤x≤0.90, for example, it can be 0.20, 0.25, 0.3, 0.35, 0.4, 0.45, 0.5, 0.55, 0.6, 0.65, 0.7, 0.75, 0.8, 0.85 or 0.90, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably 0.55≤x≤0.65.

[0011] The chemical formula of the cerium-tin composite oxide carrier in the present invention is Ce x Sn 1-x O2, where the value of x will affect the reaction activity of the catalyst.

[0012] Preferably, based on the total mass of the Ru-based catalyst as 100wt%, the content of the active component Ru is 1.0-2.0wt%, for example, it can be 1.0wt%, 1.1wt%, 1.2wt%, 1.3wt%, 1.4wt%, 1.5wt%, 1.6wt%, 1.7wt%, 1.8wt%, 1.9wt% or 2.0wt%, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, and the balance is the cerium-tin composite oxide support.

[0013] Preferably, the cerium-tin composite oxide support is a nanorod structure.

[0014] Preferably, the average diameter of the cerium-tin composite oxide support is 5-7 nm, for example, 5 nm, 5.5 nm, 6 nm, 6.5 nm or 7 nm, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0015] Preferably, the average length of the cerium-tin composite oxide support is 40-50 nm, for example, 40 nm, 41 nm, 42 nm, 43 nm, 44 nm, 45 nm, 46 nm, 47 nm, 48 nm, 49 nm or 50 nm, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0016] Preferably, the specific surface area of ​​the cerium-tin composite oxide carrier is 100-130 m 2 / g, for example, it can be 100m 2 / g, 102m 2 / g、104m 2 / g、106m 2 / g、108m 2 / g, 110m 2 / g, 112m 2 / g, 114m 2 / g, 115m 2 / g, 116m 2 / g, 117m 2 / g, 118m 2 / g, 120m 2 / g, 121m 2 / g, 122m 2 / g, 124m 2 / g, 126m 2 / g, 128m 2 / g or 130m 2 / g, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0017] The cerium-tin composite oxide carrier of the present invention has a specific structure. The nanorod-like structure has a high specific surface area and is conducive to the loading and uniform dispersion of active components.

[0018] In a second aspect, the present invention provides a method for preparing the Ru-based catalyst as described in the first aspect, the preparation method comprising the following steps:

[0019] The Ru source and water are uniformly mixed to obtain a first mixture; the cerium-tin composite oxide carrier is mixed with the first mixture, impregnated, ultrasonicated, stirred, and then subjected to rotary evaporation, first drying, and first calcination to obtain the Ru-based catalyst.

[0020] The present invention adopts an impregnation method to prepare the catalyst, which has low cost and simple synthesis method. During the impregnation process, the Ru species generated by the Ru source can be evenly dispersed on the surface of the cerium-tin composite oxide carrier, which is conducive to the active components to play a role.

[0021] Preferably, the Ru source includes any one of ruthenium trichloride, ruthenium acetate or ammonium chlororuthenate or a combination of at least two of them. Typical but non-limiting combinations include a combination of ruthenium trichloride and ruthenium acetate, a combination of ruthenium acetate and ammonium chlororuthenate, a combination of ruthenium trichloride and ammonium chlororuthenate, a combination of ruthenium trichloride, ruthenium acetate and ammonium chlororuthenate, preferably ruthenium trichloride.

[0022] Preferably, the mass ratio of the Ru source to water is (6-10):1000, for example, 6:1000, 7:1000, 8:1000, 9:1000 or 10:1000, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable, preferably (7-9):1000.

[0023] Preferably, the ultrasound time is 15-60 min, for example, it can be 15 min, 20 min, 25 min, 30 min, 35 min, 40 min, 45 min, 50 min, 55 min or 60 min, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0024] Preferably, the stirring time is 0.5-2 h, for example, 0.5 h, 1 h, 1.5 h or 2 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0025] Preferably, the gauge pressure during the rotary evaporation is -0.08 MPa or less, for example, it can be -0.098 MPa, -0.096 MPa, -0.094 MPa, -0.090 MPa, -0.088 MPa, -0.086 MPa, -0.084 MPa, -0.082 MPa or -0.08 MPa, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0026] Preferably, the rotary evaporation temperature is 50-70°C, for example, 50°C, 55°C, 60°C, 65°C or 70°C, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0027] Preferably, the first drying temperature is 90-110°C, for example, 90°C, 95°C, 100°C, 105°C or 110°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0028] Preferably, the first drying time is 12-24 hours, for example, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0029] Preferably, the temperature of the first calcination is 500-600°C, for example, it can be 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0030] In the present invention, the product after impregnation is subjected to a first calcination at 500-600° C. The calcination process allows the active component Ru to be tightly combined with the carrier. If the temperature of the first calcination is too low, the prepared catalyst fails to form the target nanorod structure and the Ru distribution is uneven; if the temperature of the first calcination is too high, the nanorod structure of the prepared catalyst is destroyed and Ru agglomerates, thereby affecting the catalytic activity of the catalyst.

[0031] Preferably, the first calcination time is 2-4 h, for example, 2 h, 2.5 h, 3 h, 3.5 h or 4 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0032] Preferably, the preparation method of the cerium-tin composite oxide carrier comprises:

[0033] The cerium source, the tin source and water are uniformly mixed to obtain a second mixture; the sodium hydroxide solution is mixed with the second mixture, stirred uniformly and then subjected to hydrothermal reaction, and the cerium-tin composite oxide carrier is obtained after solid-liquid separation, washing, second drying and second calcination.

[0034] Preferably, the cerium source includes any one of hexahydrated cerium nitrate, cerium carbonate or cerium oxalate, or a combination of at least two of them. Typical but non-limiting combinations include a combination of hexahydrated cerium nitrate and cerium carbonate, a combination of cerium carbonate and cerium oxalate, a combination of hexahydrated cerium nitrate and cerium oxalate, and a combination of hexahydrated cerium nitrate, cerium carbonate and cerium oxalate, preferably cerium nitrate hexahydrate.

[0035] Preferably, the tin source comprises any one of tin tetrachloride pentahydrate, tin acetate or tin iodide or a combination of at least two thereof, typical but non-limiting combinations include a combination of tin tetrachloride pentahydrate and tin acetate, a combination of tin acetate and tin iodide, a combination of tin tetrachloride pentahydrate and tin iodide, a combination of tin tetrachloride pentahydrate, tin acetate and tin iodide, preferably tin tetrachloride pentahydrate.

[0036] Preferably, the molar ratio of the cerium source to the tin source is (0.25-9):1, for example, it can be 0.25:1, 0.3:1, 0.4:1, 0.5:1, 0.6:1, 0.7:1, 0.8:1, 0.9:1, 1:1, 1.1:1, 1.2:1, 1.3:1, 1.4:1, 1.5:1, 1.6:1, 1.7:1, 1.8:1, 1.9:1, 2:1, 2.1:1, 2.2:1, 2.3:1, 2.4:1, 2.5:1, 2.6:1, 2.7:1, 2.8:1, 2.9:1, 3:1, 4:1, 5:1, 5.7:1, 7:1, 8:1 or 9:1, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0037] Preferably, the total concentration of metal ions in the second mixture is 0.20-0.25 mol / L, for example, it can be 0.20 mol / L, 0.21 mol / L, 0.22 mol / L, 0.23 mol / L, 0.24 mol / L or 0.25 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0038] Preferably, the concentration of the sodium hydroxide solution is 6-8 mol / L, for example, 6 mol / L, 6.5 mol / L, 7 mol / L, 7.5 mol / L or 8 mol / L, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0039] Preferably, the molar ratio of the metal ions in the cerium source to the solute in the sodium hydroxide solution is (0.004-0.017):1, for example, it can be 0.004:1, 0.005:1, 0.006:1, 0.007:1, 0.008:1, 0.009:1, 0.010:1, 0.011:1, 0.012:1, 0.013:1, 0.014:1, 0.015:1, 0.016:1 or 0.017:1, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0040] Preferably, the temperature of the hydrothermal reaction is 90-110°C, for example, 90°C, 95°C, 100°C, 105°C or 110°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0041] The hydrothermal reaction during the preparation of the cerium-tin composite oxide carrier of the present invention affects the morphology of the carrier. When the temperature of the hydrothermal reaction is controlled within the range of 90-110° C., a carrier with a nanorod-like structure is obtained. If the temperature of the hydrothermal reaction is too low, the prepared cerium-tin composite oxide carrier is not fully crystallized, thereby affecting the activity of the catalyst. If the temperature of the hydrothermal reaction is too high, the pore structure of the prepared cerium-tin composite oxide carrier is destroyed, thereby reducing the specific surface area of ​​the catalyst, which is not conducive to the loading of active components.

[0042] Preferably, the hydrothermal reaction time is 10-14 h, for example, 10 h, 11 h, 12 h, 13 h or 14 h, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0043] Preferably, the end point of the washing is that the pH of the washing liquid is 6-8, for example, it can be 6, 6.5, 7, 7.5 or 8, but it is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable.

[0044] Preferably, the second drying temperature is 90-110°C, for example, 90°C, 95°C, 100°C, 105°C or 110°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0045] Preferably, the second drying time is 12-24 hours, for example, 12 hours, 14 hours, 16 hours, 18 hours, 20 hours, 22 hours or 24 hours, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Preferably, the temperature of the second calcination is 500-600°C, for example, it can be 500°C, 510°C, 520°C, 530°C, 540°C, 550°C, 560°C, 570°C, 580°C, 590°C or 600°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0047] Preferably, the second calcination time is 3-5 h, for example, 3 h, 3.5 h, 4 h, 4.5 h or 5 h, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable.

[0048] Preferably, the preparation method comprises the following steps:

[0049] (1) a cerium source and a tin source are dissolved in water at a molar ratio of (0.3-3):1 to obtain a second mixture with a total metal ion concentration of 0.20-0.25 mol / L, a sodium hydroxide solution with a concentration of 6-8 mol / L is mixed and stirred evenly with the second mixture, and then a hydrothermal reaction is carried out at 90-110° C. for 10-14 h, solid-liquid separation is performed, washing is performed until the washing liquid is neutral, a second drying is performed at 90-110° C. for 12-24 h, and then a second calcination is performed at 500-600° C. for 3-5 h to obtain the cerium-tin composite oxide support;

[0050] The molar ratio of the metal ions in the cerium source to the solute in the sodium hydroxide solution is (0.004-0.017):1;

[0051] (2) A Ru source and water are uniformly mixed in a mass ratio of (6-10):1000 to obtain a first mixture, the cerium-tin composite oxide support obtained in step (1) is mixed with the first mixture, impregnated, ultrasonicated for 15-60 minutes, stirred for 0.5-2 hours, and then rotary evaporated at a pressure of -0.08 MPa or less and a temperature of 50-70°C, first dried at 90-110°C for 12-24 hours, and then first calcined at 500-600°C for 2-4 hours to obtain the Ru-based catalyst.

[0052] In a third aspect, the present invention provides a use of the Ru-based catalyst described in the first aspect, wherein the Ru-based catalyst is used for selective catalytic oxidation of ammonia.

[0053] The Ru-based catalyst of the present invention has excellent low-temperature activity and N2 selectivity, exhibits excellent ammonia catalytic oxidation activity, meets current market demand, and has good practical application prospects.

[0054] Preferably, the operating temperature of the Ru-based catalyst for selective catalytic oxidation of ammonia is 150-300°C, for example, 150°C, 200°C, 250°C or 300°C, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0055] The numerical range described in the present invention not only includes the point values ​​listed above, but also includes any point values ​​between the above numerical ranges that are not listed. Due to space limitations and for the sake of simplicity, the present invention no longer exhaustively lists the specific point values ​​included in the range.

[0056] Compared with the prior art, the present invention has at least the following beneficial effects:

[0057] (1) The present invention uses cerium-tin composite oxide as a carrier and Ru as an active component to prepare a catalyst. The content of the active component Ru is 0.5-2.0wt%. Ru has good dispersion. When the content of the active component is very low, the catalyst can have good low-temperature activity and thermal stability.

[0058] (2) The present invention adopts an impregnation method to prepare the catalyst, which has low cost and simple synthesis method. During the impregnation process, the Ru species generated by the Ru source can be evenly dispersed on the surface of the cerium-tin composite oxide support.

[0059] (3) The Ru-based catalyst of the present invention has excellent low-temperature activity, exhibits excellent ammonia catalytic oxidation activity, meets current market demand, and has good practical application prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] Figure 1 is a graph showing the conversion rate of NH3 of the catalysts prepared in Example 1 of the present invention and Comparative Examples 3, 4 and 5;

[0061] Figure 2 It is a N2 selectivity curve diagram of the catalysts prepared in Example 1 of the present invention and Comparative Examples 3, 4, and 5. DETAILED DESCRIPTION

[0062] The technical solution of the present invention is further described below in conjunction with the accompanying drawings and through specific implementation methods. However, the following examples are only simplified examples of the present invention and do not represent or limit the scope of protection of the present invention. The scope of protection of the present invention shall be subject to the claims.

[0063] In the following examples, unless otherwise specified, all reagents and consumables were purchased from conventional reagent manufacturers in the field; unless otherwise specified, the experimental methods and technical means used were conventional methods and means in the field.

[0064] Example 1

[0065] This embodiment provides a Ru-based catalyst. Based on the total mass of the Ru-based catalyst being 100 wt%, the content of the active component Ru is 1 wt%, and the remainder is a cerium-tin composite oxide carrier. The chemical formula of the cerium-tin composite oxide carrier is Ce 0.6 Sn 0.4 O2;

[0066] The cerium-tin composite oxide carrier has a diameter of 6 nm, a length of 45 nm, and a specific surface area of ​​115 m 2 / g nanorod-like structure;

[0067] The preparation method of the Ru-based catalyst provided in this embodiment comprises the following steps:

[0068] (1) Cerium nitrate hexahydrate and tin tetrachloride pentahydrate were added to water at a Ce:Sn molar ratio of 1.5:1 to dissolve evenly, a sodium hydroxide solution with a concentration of 7 mol / L was added thereto, and after stirring evenly, a hydrothermal reaction was carried out at 100°C for 12 hours, solid-liquid separation and washing were performed until the solution pH was 7, a second drying was carried out at 100°C for 18 hours, and then a second roasting was carried out at 550°C for 4 hours to obtain Ce 0.6 Sn 0.4 O2 carrier;

[0069] The molar ratio of the metal ions in the cerium source to the solute in the sodium hydroxide solution is 0.011:1;

[0070] (2) mixing ruthenium trichloride and water in a mass ratio of 7:1000 to obtain a first mixture, and adding Ce obtained in step (1) 0.6 Sn 0.4 The O2 carrier is added to the first mixture for impregnation, ultrasonicated for 30 minutes, stirred for 1 hour, and then rotary evaporated at a pressure of -0.098 MPa and a temperature of 60°C, first dried at 100°C for 18 hours, and then first calcined at 550°C for 3 hours to obtain the Ru-based catalyst.

[0071] The conversion rate of NH3 of the prepared Ru-based catalyst is as follows Figure 1 As shown, from Figure 1 As can be seen from the results, the conversion rate can reach more than 96% at 250°C, and the selectivity of N2 is as follows: Figure 2 shown.

[0072] Example 2

[0073] This embodiment provides a Ru-based catalyst. Based on the total mass of the Ru-based catalyst being 100 wt%, the content of the active component Ru is 1.5 wt%, and the remainder is a cerium-tin composite oxide support. The chemical formula of the cerium-tin composite oxide support is Ce 0.7 Sn0.3 O2;

[0074] The cerium-tin composite oxide carrier has a diameter of 5.3 nm, a length of 41 nm, and a specific surface area of ​​104 m 2 / g nanorod-like structure;

[0075] The preparation method of the Ru-based catalyst provided in this embodiment comprises the following steps:

[0076] (1) adding cerium nitrate hexahydrate and tin tetrachloride pentahydrate into water at a Ce:Sn molar ratio of 2.33:1 to dissolve uniformly, adding a sodium hydroxide solution with a concentration of 6 mol / L, stirring uniformly, and then hydrothermally reacting at 110° C. for 11 h, solid-liquid separation, washing until the solution pH is 7, second drying at 110° C. for 12 h, and then second calcining at 600° C. for 3 h to obtain Ce 0.7 Sn 0.3 O2 carrier;

[0077] The molar ratio of the metal ions in the cerium source to the solute in the sodium hydroxide solution is 0.004:1;

[0078] (2) ruthenium acetate and water are mixed in a mass ratio of 8:1000 to obtain a first mixture, and Ce obtained in step (1) is added to the mixture. 0.7 Sn 0.3 The O2 carrier is added to the first mixture for impregnation, ultrasonicated for 60 minutes, stirred for 0.5 hours, and then rotary evaporated at a pressure of -0.095 MPa and a temperature of 50°C, first dried at 110°C for 12 hours, and then first calcined at 600°C for 2 hours to obtain the Ru-based catalyst.

[0079] Example 3

[0080] This embodiment provides a Ru-based catalyst. Based on the total mass of the Ru-based catalyst being 100 wt%, the content of the active component Ru is 2 wt%, and the remainder is a cerium-tin composite oxide carrier. The chemical formula of the cerium-tin composite oxide carrier is Ce 0.5 Sn 0.5 O2;

[0081] The cerium-tin composite oxide carrier has a diameter of 6.7 nm, a length of 48 nm, and a specific surface area of ​​127 m 2 / g nanorod-like structure;

[0082] The preparation method of the Ru-based catalyst provided in this embodiment comprises the following steps:

[0083] (1) adding cerium nitrate hexahydrate and tin tetrachloride pentahydrate into water at a Ce:Sn molar ratio of 1:1 to dissolve uniformly, adding a sodium hydroxide solution with a concentration of 8 mol / L, stirring uniformly, and then hydrothermally reacting at 90°C for 14 hours, solid-liquid separation, washing until the solution pH is 8, second drying at 90°C for 24 hours, and then second roasting at 500°C for 5 hours to obtain Ce 0.5 Sn 0.5 O2 carrier;

[0084] The molar ratio of the metal ions in the cerium source to the solute in the sodium hydroxide solution is 0.017:1;

[0085] (2) mixing ruthenium trichloride and water in a mass ratio of 10:1000 to obtain a first mixture, and adding Ce obtained in step (1) 0.5 Sn 0.5 The O2 carrier is added to the first mixture for impregnation, ultrasonicated for 15 minutes, stirred for 2 hours, and then rotary evaporated at a pressure of -0.08 MPa and a temperature of 70°C, first dried at 90°C for 24 hours, and then first calcined at 500°C for 4 hours to obtain the Ru-based catalyst.

[0086] Example 4

[0087] This embodiment provides a Ru-based catalyst, which is different from Embodiment 1 only in that, when preparing the Ru-based catalyst, the temperature of the hydrothermal reaction in step (1) is 80°C.

[0088] Example 5

[0089] This embodiment provides a Ru-based catalyst, which is different from Embodiment 1 only in that, when preparing the Ru-based catalyst, the temperature of the hydrothermal reaction in step (1) is 120°C.

[0090] Example 6

[0091] This embodiment provides a Ru-based catalyst, which is different from Embodiment 1 only in that, when preparing the Ru-based catalyst, the first calcination temperature in step (2) is 700°C.

[0092] Example 7

[0093] This embodiment provides a Ru-based catalyst, which is different from Embodiment 1 only in that, when preparing the Ru-based catalyst, the first calcination temperature in step (2) is 400°C.

[0094] Comparative Example 1

[0095] This comparative example provides a Ru-based catalyst, which is different from Example 1 only in that, based on the total mass of the Ru-based catalyst being 100 wt %, the content of the active component Ru is 0.1 wt %.

[0096] Comparative Example 2

[0097] This comparative example provides a catalyst, which is different from Example 1 only in that the carrier used in preparing the catalyst is titanium oxide, wherein the titanium oxide carrier is purchased from Aladdin.

[0098] Comparative Example 3

[0099] This comparative example provides a Ce 0.6 Sn 0.4 O2 catalyst, the difference from Example 1 is that the Ce obtained in step (1) is 0.6 Sn 0.4 The O2 carrier is used as a catalyst, that is, step (2) is not carried out and no active components are loaded.

[0100] The prepared Ce 0.6 Sn 0.4 The conversion rate of NH3 over O2 catalyst is as follows Figure 1 As shown, the selectivity of N2 is Figure 2 shown.

[0101] Comparative Example 4

[0102] This comparative example provides a Ru / CeO2 catalyst, which is different from Example 1 only in that the carrier used in preparing the catalyst is CeO2, that is, no tin source is added in step (1), and the remaining steps are the same as Example 1.

[0103] The conversion rate of NH3 over the prepared Ru / CeO2 catalyst is as follows: Figure 1 As shown, the selectivity of N2 is Figure 2 shown.

[0104] Comparative Example 5

[0105] This comparative example provides a CeO2 catalyst, which is different from comparative example 4 only in that the CeO2 obtained in step (1) is used as a catalyst, that is, no active component is loaded.

[0106] The conversion rate of NH3 in CeO2 catalyst prepared is as follows Figure 1 As shown, the selectivity of N2 is Figure 2 shown.

[0107] Test method: 100 mg of the prepared Ru catalyst was sieved with a 40-60 mesh screen and placed in a catalyst activity evaluation device (Antaris IGS, Thermo Fisher). The activity evaluation was carried out in a fixed bed reactor. The test conditions were: 500 ppm NH3, 10% O2, N2 balance, and a total flow rate of 200 mL / min. The test results are shown in Table 1.

[0108] Table 1

[0109]

[0110]

[0111] The test results show that:

[0112] (1) It can be seen from Examples 1-3 that the present invention prepares a cerium-tin composite oxide carrier by a hydrothermal method, and loads an active component Ru with a mass fraction of 0.5-2wt% on the carrier by an impregnation method. The prepared Ru-based catalyst has an NH3 conversion rate of more than 85% and a N2 selectivity of less than 66% at 250°C, and has excellent low-temperature ammonia catalytic oxidation activity. When the chemical formula of the cerium-tin composite oxide carrier is Ce 0.6 Sn 0.4 When the loading amount of active component Ru is 1wt%, the obtained catalyst has the highest activity, and the NH3 conversion rate is above 96% under the condition of 250℃.

[0113] (2) By comparing Example 1 with Examples 4-5, it can be seen that the temperature of the hydrothermal reaction in the preparation process of the cerium-tin composite oxide support in the present invention will affect the reaction activity of the catalyst finally prepared. When the reaction temperature is too low, the prepared cerium-tin composite oxide support is not fully crystallized, thereby affecting the activity of the catalyst; if the reaction temperature is too high, the pore structure of the cerium-tin composite oxide support is destroyed, reducing the specific surface area of ​​the catalyst, thereby affecting the loading of the active components, and further resulting in a decrease in the activity of the catalyst.

[0114] (3) By comparing Example 1 with Examples 6-7, it can be seen that in the present invention, the product after impregnation is subjected to the first calcination at 500-600°C. During this process, the active component Ru is tightly combined with the carrier. If the temperature of the first calcination is too low, the prepared catalyst fails to form the target nanorod structure and the Ru distribution is uneven; if the temperature of the first calcination is too high, the nanorod structure of the prepared catalyst is destroyed and Ru agglomerates.

[0115] (4) By comparing Example 1 with Comparative Example 1, it can be seen that the present invention can achieve better catalytic activity at a low loading amount by further controlling the content range of the active component Ru. When the content of the active component Ru is too little, the catalytic efficiency is too low. When the content of the active component Ru is too much, not only the manufacturing cost of the catalyst is increased, but also the active component is agglomerated, so that the catalyst cannot fully function.

[0116] (5) It can be seen from Example 1 and Comparative Example 2 that when conventional titanium oxide is used as a carrier, the NH3 conversion rate of the prepared catalyst at 250°C is only about 63%. It can be seen that the present invention significantly improves the low-temperature NH3 conversion rate of the catalyst by loading the Ru active component on the cerium-tin composite oxide carrier.

[0117] (6) It can be seen from Example 1 and Comparative Example 3 that when no active component is loaded, the prepared Ce 0.6 Sn 0.4 When O2 is used as a catalyst, its NH3 conversion rate at 250°C is only 6.78%. It can be seen that the present invention significantly improves the NH3 conversion rate of the catalyst by loading the Ru active component on the cerium-tin composite oxide carrier.

[0118] (7) It can be seen from Example 1 and Comparative Example 4 that when CeO2 is used as a carrier, the NH3 conversion rate of the prepared catalyst at 250°C is 57.85%. It can be seen that the specific composition of the carrier of the present invention seriously affects the activity of the catalyst. In the absence of Sn, the activity of the catalyst is very low. The present invention significantly improves the NH3 conversion rate of the catalyst by loading the Ru active component on the cerium-tin composite oxide carrier.

[0119] (8) It can be seen from Comparative Examples 4 and 5 that when CeO2 is directly used as a catalyst without loading an active component, the activity of the catalyst is very low. The present invention significantly improves the NH3 conversion rate of the catalyst by loading the Ru active component on the cerium-tin composite oxide carrier.

[0120] In summary, the present invention uses cerium-tin composite oxide as a carrier and Ru as an active component to prepare a catalyst. Ru has good dispersion, and the active component of the catalyst can achieve good low-temperature activity, N2 selectivity and thermal stability at a relatively low content.

[0121] The applicant declares that the above is only a specific implementation mode of the present invention, but the protection scope of the present invention is not limited thereto. Those skilled in the art should understand that any changes or substitutions that can be easily thought of by those skilled in the art within the technical scope disclosed by the present invention shall fall within the protection scope and disclosure scope of the present invention.

Claims

1. A Ru-based catalyst, It is characterized in that The Ru-based catalyst comprises a cerium-tin composite oxide carrier and an active component Ru loaded on the carrier; based on the total mass of the Ru-based catalyst being 100wt%, the content of the active component Ru is 0.5-2wt%, and the remainder is the cerium-tin composite oxide carrier.

2. The Ru-based catalyst according to claim 1, It is characterized in that The chemical formula of the cerium-tin composite oxide support is Ce x Sn 1-x O 2 , wherein 0.20≤x≤0.90, preferably 0.55≤x≤0.65; Preferably, based on the total mass of the Ru-based catalyst being 100 wt%, the content of the active component Ru is 1.0-2.0 wt%, and the remainder is the cerium-tin composite oxide carrier; Preferably, the cerium-tin composite oxide support is a nanorod-like structure; Preferably, the cerium-tin composite oxide carrier has an average diameter of 5-7 nm, an average length of 40-50 nm, and a specific surface area of ​​100-130 m 2 / g.

3. A method for preparing the Ru-based catalyst according to claim 1 or 2, It is characterized in that The preparation method comprises the following steps: The Ru source and water are uniformly mixed to obtain a first mixture; the cerium-tin composite oxide carrier is mixed with the first mixture, impregnated, ultrasonicated, stirred, and then subjected to rotary evaporation, first drying, and first calcination to obtain the Ru-based catalyst.

4. The preparation method according to claim 3, It is characterized in that The Ru source includes any one of ruthenium trichloride, ruthenium acetate or ammonium chlororuthenate, or a combination of at least two thereof; Preferably, the mass ratio of the Ru source to water is (6-10):1000; Preferably, the gauge pressure during the rotary evaporation is -0.08 MPa or less; Preferably, the rotary evaporation temperature is 50-70°C; Preferably, the first drying temperature is 90-110°C; Preferably, the first drying time is 12-24h; Preferably, the temperature of the first calcination is 500-600°C; Preferably, the first calcination time is 2-4 hours.

5. The preparation method according to claim 3 or 4, It is characterized in that The preparation method of the cerium-tin composite oxide carrier comprises: The cerium source, the tin source and water are uniformly mixed to obtain a second mixture; the sodium hydroxide solution is mixed with the second mixture, stirred uniformly and then subjected to hydrothermal reaction, and the cerium-tin composite oxide carrier is obtained after solid-liquid separation, washing, second drying and second calcination.

6. The preparation method according to claim 5, It is characterized in that The cerium source includes any one of hexahydrated cerium nitrate, cerium carbonate or cerium oxalate, or a combination of at least two thereof; Preferably, the tin source comprises any one or a combination of at least two of tin tetrachloride pentahydrate, tin acetate or tin iodide; Preferably, the molar ratio of the cerium source to the tin source is (0.25-9):1; Preferably, the total concentration of metal ions in the second mixture is 0.20-0.25 mol / L; Preferably, the concentration of the sodium hydroxide solution is 6-8 mol / L; Preferably, the molar ratio of the metal ions in the cerium source to the solute in the sodium hydroxide solution is (0.004-0.017):

1.

7. The preparation method according to claim 5 or 6, It is characterized in that The temperature of the hydrothermal reaction is 90-110°C; Preferably, the hydrothermal reaction time is 10-14h; Preferably, the end point of the washing is when the pH of the washing solution is 6-8; Preferably, the second drying temperature is 90-110°C; Preferably, the second drying time is 12-24h; Preferably, the temperature of the second calcination is 500-600°C; Preferably, the second calcination time is 3-5 hours.

8. The preparation method according to claim 3, It is characterized in that The preparation method comprises the following steps: (1) a cerium source and a tin source are dissolved in water at a molar ratio of (0.3-3):1 to obtain a second mixture with a total metal ion concentration of 0.20-0.25 mol / L, a sodium hydroxide solution with a concentration of 6-8 mol / L is mixed and stirred evenly with the second mixture, and then a hydrothermal reaction is carried out at 90-110° C. for 10-14 h, solid-liquid separation is performed, washing is performed until the washing liquid is neutral, a second drying is performed at 90-110° C. for 12-24 h, and then a second calcination is performed at 500-600° C. for 3-5 h to obtain the cerium-tin composite oxide support; The molar ratio of the metal ions in the cerium source to the solute in the sodium hydroxide solution is (0.004-0.017):1; (2) A Ru source and water are uniformly mixed in a mass ratio of (6-10):1000 to obtain a first mixture, the cerium-tin composite oxide support obtained in step (1) is mixed with the first mixture, impregnated, ultrasonicated for 15-60 minutes, stirred for 0.5-2 hours, and then rotary evaporated at a gauge pressure of -0.08 MPa or less and a temperature of 50-70°C, first dried at 90-110°C for 12-24 hours, and then first calcined at 500-600°C for 2-4 hours to obtain the Ru-based catalyst.

9. Use of the Ru-based catalyst according to claim 1 or 2, It is characterized in that The Ru-based catalyst is used for selective catalytic oxidation of ammonia.

10. The use according to claim 9, It is characterized in that The working temperature of the Ru-based catalyst for selective catalytic oxidation of ammonia is 150-300°C.

Citation Information

Patent Citations

  • Transition metal oxide modified composite oxide loaded noble metal three-way catalyst and preparation method thereof

    CN117258802A

  • Ammonia oxidation / decomposition catalyst

    US20130156687A1