Copper-doped cobalt-based composite oxide as well as synthesis method and application thereof
Through the synthesis of copper-doped cobalt-based composite oxides, the problems of poor catalytic activity and secondary pollution of cobalt oxides were solved, and the rapid and efficient decomposition of bisphenol A and water pollution control were achieved, demonstrating its advantages in the field of water pollution. performance.
Patent Information
- Application Number
- CN202411034316.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-15
AI Technical Summary
In the prior art, the catalytic activity of cobalt oxides is poor and difficult to use on a large scale. Cobalt ions may cause secondary pollution in super oxidation reactions, limiting their application in the field of water pollution control.
Using the synthesis method of copper-doped cobalt-based composite oxide, the reaction of cobalt salt and 2-methylimidazole in methanol is obtained by reacting dimethylimidazole cobalt, which is then replaced with zinc nitrate and copper ions, and is prepared in a nest shape after calcination. The copper-doped cobalt-based composite oxide of the structure uses ion etching and exchange to introduce vacant oxygen and metal active sites to achieve efficient decomposition of the catalyst.
The rapid and efficient decomposition of bisphenol A is achieved, the consumption of catalysts and oxidants is reduced, the secondary pollution of cobalt ions is avoided, the effect of water pollution control is improved, and the activity of the catalyst is basically lost in multiple cycles.
Smart Images

Figure CN118949992A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material engineering and environmental engineering, and in particular to a copper-doped cobalt-based composite oxide and a synthesis method and application thereof. Background Art
[0002] Bisphenol A (BPA), as one of the components of plastics, is an important chemical raw material. As a fat-soluble substance, it can enter the human body through breathing, digestion, etc., which will affect the endocrine system and cause serious harm. Due to its stable chemical properties and difficulty in automatic decomposition, the treatment of BPA is usually based on the advanced oxidation technology of persulfate. Its effective treatment is achieved by activating the free radical singlet oxygen obtained by permonosulfate (PMS) and peroxydisulfate (PDS). Studies have shown that the generation of active species is more efficient in the presence of transition metal catalysts. Therefore, transition metal ions such as cobalt ions and manganese ions are used to activate persulfate. However, since high concentrations of transition metal ions will bring potential secondary pollution, transition metal oxides have been developed as alternatives and applied to persulfate activation and decomposition of BPA molecules.
[0003] For example, Chinese patent CN112892548B discloses a method for preparing a manganese-based catalyst for sewage treatment and a manganese-based catalyst. The manganese-based catalyst uses a solution containing manganese ions as a precursor solution, a solution containing one or more of iron ions, cobalt ions, cerium ions and copper ions as an auxiliary agent precursor solution, and an organic acid as a reducing complexing agent solution, and the mixture is mixed to obtain a prefabricated mixed solution. The pretreated activated carbon is immersed in the prefabricated mixed solution, and the mixture is calcined at high temperature to obtain a manganese-based catalyst for sewage treatment with manganese oxide as a main catalyst, one or more of iron oxide, cobalt oxide, cerium oxide and copper oxide as a auxiliary catalyst, and the pretreated activated carbon as a carrier. The manganese-based catalyst has high activity, good stability and strong ability in catalytic oxidation of organic matter in sewage. However, current research has found that although cobalt-based oxides have good catalytic activity, cobalt oxides obtained by directly calcining inorganic cobalt salts have poor activity and are difficult to use on a large scale. Therefore, among the catalysts currently in common use, cobalt oxides can only be used as auxiliary catalysts. Summary of the invention
[0004] In view of the problems existing in the prior art, the object of the present invention is to provide a copper-doped cobalt-based composite oxide and a synthesis method and application thereof.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for synthesizing a copper-doped cobalt-based composite oxide comprises the following steps:
[0007] S1 uses cobalt salt and 2-methylimidazole to react in methanol solvent with stirring to obtain dimethylimidazole cobalt;
[0008] S2: reacting dimethylimidazole cobalt with zinc nitrate and 2-methylimidazole in a methanol solvent to obtain a dimethylimidazole zinc-cobalt complex;
[0009] S3 replaces the dimethylimidazole zinc-cobalt complex with copper ions and calcines it to obtain a copper-doped cobalt-based composite oxide.
[0010] The copper-doped cobalt-based composite oxide synthesized by the present invention utilizes ion etching and exchange to introduce the synergistic effect of vacant oxygen and metal active sites to prepare a bird's nest structure rich in vacant oxygen. The bisphenol A molecules can be quickly and efficiently decomposed under low consumption of catalyst and oxidant by activating potassium persulfate, and the potential secondary pollution of transition metals represented by cobalt ions in super oxidation reactions can be overcome, so that the composite oxide can be better applied in the field of water pollution control.
[0011] As a further preferred embodiment of the present invention, in S1, the specific operation is to add the cobalt salt and 2-methylimidazole to methanol in sequence, stir at 150-200 r / min for 10-20 min, let stand for 24-30 h, centrifuge and wash the product 3-5 times, and dry it.
[0012] As a further preferred embodiment of the present invention, in S1, the ratio of the cobalt salt, 2-methylimidazole and methanol is (1.5-1.8) g: (3.2-3.7) g: (50-80) mL.
[0013] As a further preferred embodiment of the present invention, in S2, the specific operation is to add dimethylimidazole cobalt, zinc nitrate and 2-methylimidazole to methanol in sequence, transfer them to a reactor after sufficient mixing, and react at 100-110°C for 10-15h. After the reaction is completed, the product is repeatedly centrifuged and washed, and then dried.
[0014] As a further preferred embodiment of the present invention, in S2, the ratio of dimethylimidazole cobalt, zinc nitrate, 2-methylimidazole and methanol is (0.2-0.5) g: (0.36-0.80) g: (0.2-0.5) g: (20-56) mL.
[0015] As a further preferred embodiment of the present invention, in S3, the specific operation is to stir the dimethylimidazole zinc-cobalt complex and copper nitrate in an ethanol solvent at 180-260 r / min for 6-10 hours, centrifuge and dry the product, calcine it at 300-400° C. for 2-5 hours in an air atmosphere, grind and wash it, and then vacuum dry it.
[0016] As a further preferred embodiment of the present invention, in S3, the ratio of the dimethylimidazole zinc-cobalt complex, copper nitrate and ethanol is (0.12-0.15) g: (24-30) mg: (10-18) mL.
[0017] The application of copper-doped cobalt-based composite oxides in the degradation of bisphenol A in wastewater specifically includes:
[0018] 3 mg of the obtained solid powder was added to 30 mL of synthetic bisphenol A wastewater (concentration of 20 mg / L), and the powder was evenly dispersed in the system by ultrasonication for 2 min, and then stirred for 30 min to achieve adsorption equilibrium between the heterogeneous interfaces, and then 3 mg of potassium permonosulfate was added to carry out the catalytic reaction.
[0019] Compared with the prior art, the present invention has the following beneficial effects:
[0020] The copper-doped cobalt-based composite oxide synthesized by the present invention utilizes ion etching and exchange to introduce the synergistic effect of vacant oxygen and metal active sites to prepare a bird's nest structure rich in vacant oxygen. The bisphenol A molecules can be quickly and efficiently decomposed under low consumption of catalyst and oxidant by activating potassium persulfate, and the potential secondary pollution of transition metals represented by cobalt ions in super oxidation reactions can be overcome, so that the composite oxide can be better applied in the field of water pollution control.
[0021] The copper-doped cobalt-based composite oxide synthesized by this method can quickly activate peroxydisulfate, and a lower peroxydisulfate concentration can also quickly degrade bisphenol A, with almost no peroxymonosulfate remaining after degradation. After multiple cycle experiments, the results show that the activity of the copper-doped cobalt-based composite oxide catalyst is basically not lost. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is the powder diffraction pattern of copper-doped cobalt-based composite oxide.
[0023] Figure 2 Transmission electron microscope image (A), high-resolution electron microscope image (B), high-angle annular dark field scanning transmission (C), EDX image (D), element distribution map Co (E), Zn (F), Cu (G) and element distribution overlap map (H) of copper-doped cobalt-based composite oxide.
[0024] Figure 3 Electronic energy spectra of Co2p (A) and Cu2p (B) of copper-doped cobalt-based composite oxides.
[0025] Figure 4 This is the electron spin resonance spectrum of copper-doped cobalt-based composite oxide.
[0026] Figure 5This is the UV-visible absorption spectrum of BPA decomposed by K2S2O8 activated by copper-doped cobalt-based composite oxide.
[0027] Figure 6 This is the efficiency diagram of decomposing BPA by three consecutive activations of K2S2O8 by copper-doped cobalt-based composite oxides. DETAILED DESCRIPTION
[0028] The present invention is further described in detail through the following embodiments in conjunction with the accompanying drawings.
[0029] (1) Processing process of the method of the present invention
[0030] 1.5g of cobalt nitrate hexahydrate and 3.2g of 2-methylimidazole were added to 50mL of methanol in sequence, stirred at 150r / min for 10min and then allowed to stand for 24h. The product was centrifuged and washed 3 times and dried to obtain dimethylimidazole cobalt; then 0.2g of dimethylimidazole cobalt, 0.36g of zinc nitrate, and 0.2g of 2-methylimidazole were added to 20mL of methanol in sequence, fully mixed and transferred to a reactor, reacted at 100°C for 10h, and after the reaction was completed, the product was repeatedly centrifuged and washed to obtain a dimethylimidazole zinc-cobalt complex; finally, 0.12g of dimethylimidazole zinc-cobalt complex and 24mg of copper nitrate were continuously stirred at 180r / min for 6h in 10mL of ethanol solvent, the product was centrifuged and dried, and then calcined at 350°C for 2h in an air atmosphere. After grinding and washing, vacuum drying was obtained to obtain a copper-doped cobalt-based composite oxide.
[0031] 3 mg of the obtained solid powder was taken into 30 mL of synthetic bisphenol A wastewater (concentration was 20 mg / L), and after ultrasonication for 2 min to evenly disperse the powder in the system, it was stirred for 30 min to allow the adsorption equilibrium to be reached between the heterogeneous interfaces, and then 3 mg of potassium permonosulfate was added to carry out the catalytic reaction.
[0032] The concentration detection method of bisphenol A is as follows: 0.5 mL of the reaction solution is taken into 0.5 mL of sodium sulfite solution (concentration is 0.5 M) at preset time intervals, the resulting sample is mixed and passed through a membrane, and then residual bisphenol A is detected on a high performance liquid chromatography, and the liquid phase condition is methanol: water = 70:30.
[0033] The detection method of PDS (potassium persulfate) is as follows: at a preset time interval, 0.1 mL of sample solution is mixed with 4.9 mL of potassium iodide solution (concentration is 10 mM), and then placed for 5 minutes, and detected by ultraviolet spectrophotometer at a detection wavelength of 352 nm.
[0034] (2) Effects obtained by this embodiment
[0035] The powder diffraction pattern of the synthesized copper-doped cobalt-based composite oxide, such as Figure 1As shown. The powder diffraction pattern confirms the existence of Co3O4, and the crystal planes (220), (311), (400), (422), (511) and (440) are consistent with the spectrum of Co3O4 (JCPDS No.43-1003); 34.6, 47.5, 56.6, 62.8 and 67.9o correspond to the (002), (102), (311), (110), (103) and (112) crystal planes of ZnO (JCPDS no.36-1451); XRD did not detect copper; atomic absorption spectroscopy proved that the metal element contents in the sample were Zn32.1wt.%, Co 24.5wt.%, Cu 4.7wt.%.
[0036] like Figure 2 As shown, transmission electron microscopy (A), high-resolution electron microscopy (B), high-angle annular dark field scanning transmission (C), EDX (D), element distribution Co (E), Zn (F), Cu (G) and element distribution overlap (H) of copper-doped cobalt-based composite oxide; Figure 2 Transmission electron microscopy and high-resolution electron microscopy proved that the structure of the sample was bird's nest-like and Co, Cu, Zn and O were evenly distributed in the sample.
[0037] like Figure 3 As shown, the Co2p electron energy spectrum of the copper-doped cobalt-based composite oxide shows that cobalt has +2 and +3 valence states. Calculation shows that the content of divalent cobalt on the surface of the sample is nearly 1.2 times higher than the normal Co3O4 theoretical value (33%). In addition, the electron energy spectrum shows that the valence state of copper is +1 and +2.
[0038] like Figure 4 As shown, the electron spin resonance spectrum of copper-doped cobalt-based composite oxide proves that the sample contains abundant vacancy oxygen.
[0039] like Figure 5 As shown, Figure 5 The present invention is a UV-visible absorption spectrum of copper-doped cobalt-based composite oxide activating K2S2O8 to decompose BPA; 50 mL of 20 ppm BPA solution is added to a round-bottom flask, 5 mg of Cu-ZnO-Co3O4 is weighed and added to the above solution, after ultrasonic treatment for 10 minutes, the round-bottom flask is placed at 25° C., a magnetic bar of suitable size is added for stirring, 10 minutes later, 10 mL of a solution containing 5 mg of K2S2O8 is added to the above round-bottom flask, the timing is started and 1 mL of the reaction solution is transferred at a determined time, 1 mL of methanol is added and the mixture is centrifuged, and the supernatant is taken for UV-visible spectrum detection, which proves that the copper-doped cobalt-based composite oxide synthesized by the present invention has a high ability to catalyze and activate PDS (potassium persulfate) to degrade bisphenol A.
[0040] like Figure 6 As shown, Figure 6This is the efficiency diagram of K2S2O8 decomposing BPA after three consecutive activations of copper-doped cobalt-based composite oxides. In order to reduce the impact of the loss of recovered samples on the recycling performance, the catalytic performance was tested three times in a row under the conditions of 10mg Cu-ZnO-Co3O4, 50mL20ppm BPA and 5mgPDS. After each test, the catalyst was recovered by centrifugation and washed once with deionized water. The catalytic decomposition efficiency was calculated using the Lambert-Beer law. The results of three consecutive cycle experiments proved that there was basically no loss in catalyst activity.
[0041] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A method for synthesizing a copper-doped cobalt-based composite oxide, characterized in that: The specific steps include: S1 uses cobalt salt and 2-methylimidazole to react in methanol solvent with stirring to obtain dimethylimidazole cobalt; S2: reacting dimethylimidazole cobalt with zinc nitrate and 2-methylimidazole in a methanol solvent to obtain a dimethylimidazole zinc-cobalt complex; S3 replaces the dimethylimidazole zinc-cobalt complex with copper ions and calcines it to obtain a copper-doped cobalt-based composite oxide.
2. The method for synthesizing a copper-doped cobalt-based composite oxide according to claim 1, characterized in that: In S1, the specific operation is to add cobalt salt and 2-methylimidazole to methanol in sequence, stir at 150-200 r / min for 10-20 min, let stand for 24-30 h, centrifuge and wash the product 3-5 times, and dry it.
3. The method for synthesizing a copper-doped cobalt-based composite oxide according to claim 2, characterized in that: In S1, the ratio of the cobalt salt, 2-methylimidazole and methanol is (1.5-1.8) g: (3.2-3.7) g: (50-80) mL.
4. The method for synthesizing a copper-doped cobalt-based composite oxide according to claim 1, characterized in that: In S2, the specific operation is to add dimethylimidazole cobalt, zinc nitrate and 2-methylimidazole to methanol in sequence, transfer them to a reactor after sufficient mixing, and react at 100-110°C for 10-15h. After the reaction is completed, the product is repeatedly centrifuged and washed, and then dried.
5. The method for synthesizing a copper-doped cobalt-based composite oxide according to claim 4, characterized in that: In S2, the ratio of dimethylimidazole cobalt, zinc nitrate, 2-methylimidazole and methanol is (0.2-0.5) g: (0.36-0.80) g: (0.2-0.5) g: (20-56) mL.
6. The method for synthesizing a copper-doped cobalt-based composite oxide according to claim 1, characterized in that: In S3, the specific operation is to stir the dimethylimidazole zinc-cobalt complex and copper nitrate in an ethanol solvent at 180-260 r / min for 6-10 hours, centrifuge and dry the product, calcine it at 300-400° C. for 2-5 hours in an air atmosphere, grind and wash it, and then vacuum dry it.
7. The method for synthesizing a copper-doped cobalt-based composite oxide according to claim 6, characterized in that: In S3, the ratio of the dimethylimidazole zinc-cobalt complex, copper nitrate and ethanol is (0.12-0.15) g: (24-30) mg: (10-18) mL.
8. The copper-doped cobalt-based composite oxide obtained according to the synthesis method according to any one of claims 1 to 7.
9. Use of the copper-doped cobalt-based composite oxide according to claim 8 in degrading bisphenol A in wastewater.
10. Use of the copper-doped cobalt-based composite oxide according to claim 8 as a catalyst in activating potassium persulfate to degrade bisphenol A in waste water.
Citation Information
Patent Citations
A method for preparing a manganese-based catalyst for wastewater treatment and the manganese-based catalyst.
CN112892548B
Preparation method and application of ternary metal composite oxide with ZIF-8 compounded ZIF-67 as template
CN110182859A
Preparation method and application of ZIF-67-ZIF-8 cobalt-based catalyst with core-shell structure
CN116586093A
Copper-doped hydroxyl cobalt oxide and application thereof in peroxymonosulfate catalytic oxidation system dominated by high-valence cobalt carbonyl
CN116618052A
Preparation of Zn-doped cobaltosic oxide-NC nanocage persulfate activator and product and application thereof
CN117583015A
Cited By
Advanced wastewater treatment method based on surface catalytic ozonation
CN120081485A