Method for improving direct flotation potassium recovery rate of carnallite ore
Through two-stage cold decomposition and ultrasonic enhanced flotation processes, the problem of low potassium recovery rate of phthalite ore is solved, the potassium recovery rate is improved and the concentrate quality is maintained, and it is suitable for potassium salt production units.
Patent Information
- Application Number
- CN202311067058.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-23
- Publication Date
- 2024-11-15
AI Technical Summary
The existing flotation technology is difficult to improve the potassium recovery rate of phthalite ore under the conditions of declining the quality of the raw ore, and the quality of concentrate will decrease by increasing the amount of the agent.
Two-stage cold decomposition process is adopted, in which the first stage does not use ultrasound, the second stage increases the sonication treatment, and the ultrasonic enhanced flotation process is used during the flotation process to improve the recovery of potassium through ultrasonic frequency and dispersion of the agent.
It improves the recovery rate of positive flotation potassium in the balsa ore and has a small impact on the concentrate quality. It can achieve improvement without changing the main process, making the equipment simple and easy to industrially promote.
Abstract
Description
Technical Field
[0001] The invention relates to a method for improving the flotation potassium recovery rate, and in particular to a method for improving the flotation potassium recovery rate of carnallite ore. Background Art
[0002] Due to their unique geographical and climatic conditions, different salt lakes produce different properties of potassium salt. Flotation is a widely used, low-cost, high-efficiency and easy-to-operate technology among various salt separation technologies. There is still room for further improvement in KCl extraction technology from chloride-type salt lakes. Under the condition that the quality of the original ore is gradually declining, it is difficult for the current flotation technology to achieve the goal of quality and quantity production through simple methods such as adjusting the dosage of reagents and adjusting the slurry flow rate.
[0003] Carnallite (KCl·MgCl2·6H2O) is a halide mineral composed mainly of potassium and magnesium, and is one of the important raw materials for the production of potassium chloride. Carnallite is an asymmetric double salt that can separate potassium chloride from magnesium chloride through dissolution, fractional crystallization and other processing steps. During the cold decomposition process of carnallite, due to the small amount of mutual doping of potassium chloride and sodium chloride, it is difficult to increase the potassium recovery rate during the flotation process. If the recovery rate is increased by increasing the dosage of reagents, the quality of the concentrate will decrease, that is, the potassium content in the concentrate will decrease. Summary of the invention
[0004] The technical problem to be solved by the present invention is to overcome the above-mentioned defects of the prior art and provide a method for improving the potassium recovery rate of carnallite ore positive flotation with little influence on the quality of the concentrate.
[0005] The technical solution adopted by the present invention to solve the technical problem is as follows: A method for improving the potassium recovery rate of carnallite ore positive flotation, comprising the following steps:
[0006] (1) Cold decomposition: The raw materials are mixed with fresh water and subjected to two-stage cold decomposition, wherein ultrasound is not used in the first stage and ultrasound treatment is added in the second stage; the raw materials include carnallite and sodium chloride;
[0007] (2) Ultrasonic enhanced flotation: A one-rough and two-fine flotation process is adopted. Each scraping stage is divided into two steps. In the first step, ultrasound is not used in scraping. In the second step, ultrasound treatment is added until flotation is completed and KCl is enriched in the flotation concentrate.
[0008] By adopting the above technical solution, the potassium recovery rate of carnallite ore decomposition flotation can be improved.
[0009] Preferably, in step (1), the KCl content of the raw material is 5% to 20%, the NaCl content is 19% to 55%, and the MgCl2 content is 6% to 27%.
[0010] The above formula can be achieved by mixing carnallite and sodium chloride as raw materials. By adopting the above technical solution, a better cold decomposition effect is achieved.
[0011] Preferably, in step (1), the amount of fresh water used is 10% to 45% of the mass of the raw material.
[0012] By adopting the above technical solution, a better cold decomposition effect is achieved.
[0013] Preferably, in step (1), the ultrasonic frequency is 20 to 200 kHz; the ultrasonic power per unit area is 0.5 to 150 W / cm 2 The action time is 4 to 60 minutes.
[0014] By adopting the above technical solution, a better cold decomposition effect is achieved.
[0015] Preferably, in step (1), mechanical stirring is performed during the cold decomposition process, and the stirring linear speed is 0.5 to 10 m / s.
[0016] By adopting the above technical solution, a better cold decomposition effect is achieved.
[0017] Preferably, in step (2), the flotation reagents are as follows: octadecylamine hydrochloride is used as a collector, and 2# oil is used as a frother.
[0018] By adopting the above technical solution, a better flotation effect is achieved.
[0019] Preferably, in step (2), the dosage of flotation reagents is as follows: the dosage of collector is 40-200 g / t of raw ore, and the dosage of frother is 5-20 g / t of raw ore.
[0020] By adopting the above technical solution, a better flotation effect is achieved.
[0021] Preferably, when preparing the flotation reagent, ultrasonic oscillation is used to disperse the collector in the solvent, the ultrasonic frequency is 20 to 200 kHz, and the power per unit area is 0.5 to 150 W / cm 2 The action time is 4 to 60 minutes.
[0022] Improving the dispersibility of the reagent is helpful for the flotation effect, and it is also feasible to use other methods to promote the dispersion of the collector; by adopting the above technical solution, a better flotation effect is achieved.
[0023] Preferably, in step (2), the flotation concentration is 20-45 wt%, the scraping time of each stage is 2-5 min, and the scraping time of the second step is 1-4 min.
[0024] By adopting the above technical solution, a better flotation effect is achieved.
[0025] Preferably, in step (2), the ultrasonic frequency is 20 to 200 kHz, and the power per unit area is 0.5 to 150 W / cm 2 .
[0026] By adopting the above technical solution, a better flotation effect is achieved.
[0027] Preferably, in step (2), a single tank aerated stirring flotation machine is used.
[0028] The above equipment can be used in the method of the present invention, and the tank volume can be selected according to the actual processing volume; it is also feasible to use other more advanced equipment.
[0029] Preferably, in step (2), the stirring speed during flotation is 800 to 2400 rpm.
[0030] By adopting the above technical solution, a better flotation effect is achieved.
[0031] Preferably, in step (2), an ultrasonic plate is added to one side of the flotation cell to achieve ultrasonic treatment.
[0032] By adopting the above technical solution, the ultrasonic processing function can be added to the original flotation equipment in a simple manner, and the method of the present invention can be applied. It is also feasible to directly use equipment with ultrasonic function.
[0033] The invention introduces ultrasonic waves into potassium salt positive flotation, changes the properties of particles in the cold decomposition process, changes the effects of particles and reagents in the froth flotation process, and ultimately improves the potassium recovery rate in the carnallite ore positive flotation process.
[0034] Beneficial effects of the present invention:
[0035] (1) A simple and easy method is used to improve the potassium recovery rate of carnallite ore decomposition flotation, and the effect on the concentrate quality is small;
[0036] (2) It can be directly applied to potash production units without changing their main processes;
[0037] (3) The equipment used in the present invention is simple and easy to promote industrialization. DETAILED DESCRIPTION
[0038] The present invention will be further described below with reference to the embodiments.
[0039] The raw materials used in the embodiments of the present invention are all obtained through conventional commercial channels.
[0040] Example 1
[0041] The raw materials used in this example come from a salt field carnallite mine, and the composition is shown in the following table:
[0042] Table 1 Example 1 Raw material composition table
[0043] Element KCl NaCl <![CDATA[MgCl2]]> <![CDATA[H2O]]> Content / wt% 18.44 19.74 26.8 35.02
[0044] (1) Cold decomposition: 2500 g of raw material and 1010 g of fresh water were mixed in a container and cold decomposed for 60 min. Ultrasonic waves were introduced 30 min into the decomposition process and the ultrasonic action time was 30 min. The ultrasonic frequency was 22 kHz, the ultrasonic power was 300 W, and the power per unit area was 3 W / cm 2 ; Stirring is also performed during cold decomposition, and the stirring line speed is 4.5m / s;
[0045] (2) Ultrasonic enhanced flotation: flotation was carried out in a 3L flotation tank, using a one-rough and two-fine process, with a stirring speed of 1500rpm, a scraping time of 3min per stage, ultrasonic treatment was carried out after 1.5min of scraping per stage, and scraping was continued until flotation was completed and KCl was enriched in the flotation concentrate; the ultrasonic frequency was 40kHz, the ultrasonic power was 500W, and the power per unit area was 5W / cm 2 .
[0046] The flotation reagents used in step (2) are: octadecylamine hydrochloride as a collector, and 2# oil as a frother; the dosage is: the collector dosage is 120g / t of the original ore, and the frother dosage is 8g / t of the original ore.
[0047] Before flotation, prepare octadecylamine hydrochloride into a solution with a mass concentration of 1% and perform ultrasonic treatment in a container. The ultrasonic frequency is 22kHz, the ultrasonic power is 300W, and the power per unit area is 5W / cm 2 , the action time is 20min.
[0048] The flotation product indexes are shown in Table 2. Although the ultrasonic treatment in this embodiment did not significantly increase the potassium content in the concentrate (nor did it significantly reduce it, and had little effect on the concentrate quality), more concentrate was obtained, and the potassium recovery rate was improved.
[0049] Table 2 Data of the concentrate product obtained in Example 1 and the control group product without ultrasonic treatment
[0050] KCl / % K recovery rate / % Ultrasonic treatment of concentrate 65.04 97.47 Unsonicated concentrate 66.02 91.12
[0051] Example 2
[0052] The raw materials used in this example come from a salt field carnallite mine, and the composition is shown in the following table:
[0053] Table 3 Raw material composition table of Example 2
[0054] Element KCl NaCl <![CDATA[MgCl2]]> <![CDATA[H2O]]> Content / wt% 11.81 44.87 18.38 23.53
[0055] (1) Cold decomposition: 1000 g of raw material and 300 g of fresh water were mixed in a container and cold decomposition was performed for 60 min. Ultrasonic waves were introduced at 40 min into the decomposition process and the ultrasonic action time was 20 min. The ultrasonic frequency was 28 kHz, the ultrasonic power was 500 W, and the power per unit area was 5.5 W / cm 2 ; Stirring is also performed during cold decomposition, and the stirring line speed is 5.5m / s;
[0056] (2) Ultrasonic enhanced flotation: A 1L single tank aerated stirring flotation machine was used for flotation. An ultrasonic plate was added to one side of the flotation tank to achieve ultrasonic treatment. A one-rough and two-fine process was adopted, with a stirring speed of 2000 rpm, a scraping time of 3.5 min per stage, and ultrasonic treatment was performed after 1.5 min of scraping each stage. Scraping continued until flotation was completed and KCl was enriched in the flotation concentrate. The ultrasonic frequency was 44 kHz, the ultrasonic power was 700 W, and the power per unit area was 7 W / cm 2 .
[0057] The flotation reagents used in step (2) are: octadecylamine hydrochloride as a collector, and 2# oil as a frother; the dosage is: the collector dosage is 150g / t of the original ore, and the frother dosage is 10g / t of the original ore.
[0058] Before flotation, prepare octadecylamine hydrochloride into a solution with a mass concentration of 1% and perform ultrasonic treatment in a container. The ultrasonic frequency is 28kHz, the ultrasonic power is 500W, and the power per unit area is 7.5W / cm 2 , the action time is 20min.
[0059] The flotation product indexes are shown in Table 4. Although the ultrasonic treatment in this embodiment did not significantly increase the potassium content in the concentrate (only slightly increased), more concentrate was obtained, which improved the potassium recovery rate.
[0060] Table 4 Data of the concentrate product obtained in Example 2 and the control group product without ultrasonic treatment
[0061] KCl / % K recovery rate / % Ultrasonic treatment of concentrate 62.01 93.25 Unsonicated concentrate 61.44 89.79
[0062] Example 3
[0063] The raw materials used in this example come from a salt field carnallite mine, and the composition is shown in the following table:
[0064] Table 5 Raw material composition of Example 3
[0065] Element KCl NaCl <![CDATA[MgCl2]]> <![CDATA[H2O]]> Content / wt% 5.00 55.00 6.38 33.62
[0066] (1) Cold decomposition: 1000 g of raw material and 160 g of fresh water were mixed in a container and cold decomposed for 60 min. Ultrasonic waves were introduced 30 min into the decomposition process and the ultrasonic action time was 30 min. The ultrasonic frequency was 65 kHz, the ultrasonic power was 600 W, and the power per unit area was 6.5 W / cm 2 ; Stirring is also performed during cold decomposition, and the stirring linear speed is 6.5m / s;
[0067] (2) Ultrasonic enhanced flotation: flotation was carried out in a 1L flotation tank, using a one-rough and two-fine process, with a stirring speed of 2400rpm, a scraping time of 3.5min per stage, ultrasonic treatment was carried out after 2min of scraping, and scraping was continued until flotation was completed and KCl was enriched in the flotation concentrate; the ultrasonic frequency was 60kHz, the ultrasonic power was 800W, and the power per unit area was 8W / cm 2 .
[0068] The flotation reagents used in step (2) are: octadecylamine hydrochloride as a collector, and 2# oil as a frother; the dosage is: the collector dosage is 80g / t of the original ore, and the frother dosage is 15g / t of the original ore.
[0069] Before flotation, prepare octadecylamine hydrochloride into a solution with a mass concentration of 1% and perform ultrasonic treatment in a container. The ultrasonic frequency is 30kHz, the ultrasonic power is 600W, and the power per unit area is 8.5W / cm 2 , the action time is 25min.
[0070] The flotation product indexes are shown in Table 6. Although the ultrasonic treatment in this embodiment did not significantly increase the potassium content in the concentrate (only slightly increased), more concentrate was obtained, which improved the potassium recovery rate.
[0071] Table 6 Data of the concentrate product obtained in Example 3 and the control group product without ultrasonic treatment
[0072] KCl / % K recovery rate / % Ultrasonic treatment of concentrate 63.55 91.77 Unsonicated concentrate 63.04 86.53
Claims
1. A method for improving the potassium recovery rate of carnallite ore flotation, characterized in that: The following steps are involved: (1) Cold decomposition: the raw materials are mixed with fresh water and subjected to two-stage cold decomposition, wherein ultrasound is not used in the first stage and ultrasound treatment is added in the second stage; the raw materials include carnallite and sodium chloride; (2) Ultrasonic enhanced flotation: A one-rough and two-fine flotation process is adopted. Each stage of flotation is divided into two steps. In the first step of flotation, ultrasound is not used. In the second step, ultrasonic treatment is added until flotation is completed and KCl is enriched in the flotation concentrate.
2. The method for improving potassium recovery rate of carnallite ore positive flotation according to claim 1, characterized in that: In step (1), the KCl content of the raw material is 5% to 20%, the NaCl content is 19% to 55%, and the MgCl2 content is 6% to 27%.
3. The method for improving the potassium recovery rate of carnallite ore positive flotation according to claim 1 or 2, characterized in that: In step (1), the amount of fresh water used is 10% to 45% of the mass of the raw material.
4. The method for improving potassium recovery rate of carnallite ore positive flotation according to any one of claims 1 to 3, characterized in that: In step (1), the ultrasonic frequency is 20 to 200 kHz; the ultrasonic power per unit area is 0.5 to 150 W / cm 2 The action time is 4 to 60 minutes; mechanical stirring is carried out during the cold decomposition process, and the stirring linear speed is 0.5 to 10 m / s.
5. The method for improving potassium recovery rate of carnallite ore positive flotation according to any one of claims 1 to 4, characterized in that: In step (2), the flotation reagents are as follows: octadecylamine hydrochloride is a collector, and 2# oil is a frother.
6. The method for improving potassium recovery rate of carnallite ore positive flotation according to any one of claims 1 to 5, characterized in that: In step (2), the dosage of flotation reagents is as follows: the dosage of collector is 40-200 g / t of raw ore, and the dosage of frother is 5-20 g / t of raw ore.
7. The method for improving potassium recovery rate of carnallite ore positive flotation according to any one of claims 1 to 6, characterized in that: When preparing the flotation reagent, ultrasonic oscillation is used to disperse the collector in the solvent. The ultrasonic frequency is 20-200kHz and the power per unit area is 0.5-150W / cm 2 The action time is 4 to 60 minutes.
8. The method for improving potassium recovery rate of carnallite ore positive flotation according to any one of claims 1 to 7, characterized in that: In step (2), the flotation concentration is 20-45 wt%, the scraping time of each stage is 2-5 min, and the scraping time of the second step is 1-4 min.
9. The method for improving potassium recovery rate of carnallite ore positive flotation according to any one of claims 1 to 8, characterized in that: In step (2), the ultrasonic frequency is 20 to 200 kHz, and the power per unit area is 0.5 to 150 W / cm 2 .
10. The method for improving potassium recovery rate of carnallite ore positive flotation according to any one of claims 1 to 9, characterized in that: In step (2), a single-tank aerated stirring flotation machine is used; the stirring speed during flotation is 800 to 2400 rpm; and an ultrasonic plate is added to one side of the flotation tank to achieve ultrasonic treatment.