Microlens optical fiber opto-acoustic transducer with high opto-acoustic conversion efficiency and method

By designing a recessed or spherical structure at the tail end of the optical fiber and filling a composite material of PDMS and gold nanoparticles, combined with a nanosecond pulse laser to form a microlens photoacoustic transducer, the existing photoacoustic transducer is solved by low efficiency and complex structure of existing photoacoustic transducers. The problem of this method achieves efficient and low-cost photoacoustic conversion effect and is suitable for a variety of application scenarios.

CN118950438APending Publication Date: 2024-11-15HARBIN ENG UNIV

Patent Information

Application Number
CN202411154820.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-22
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

The existing photoacoustic transducers have problems such as low transduction efficiency, complex production and high cost. Especially due to the separation of the absorption layer and the thermoelastic expansion layer, the sound pressure intensity is not greatly improved, and the risk of PDMS falling off is high.

Method used

A nanosecond pulse laser is used to combine with quartz fiber. The tail end of the quartz fiber is designed as a recessed or spherical structure, filled with composite materials of PDMS and gold nanoparticles. The optical fiber is used as a carrier for light transmission and excitation sound waves to form a microlens structure to improve light. Energy density and light absorption layer is formed through liquid tension and gravity to achieve photoacoustic conversion.

Benefits of technology

It improves photoacoustic conversion efficiency, simplifies structural design, reduces material costs, enhances anti-electromagnetic interference capabilities, and has a smaller structure and is easier to integrate. It is suitable for technical fields such as ultrasonic cleaning, microfluidic control and oscillation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118950438A_ABST
    Figure CN118950438A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of photoacoustic transduction, and particularly relates to a high-photoacoustic-conversion-efficiency microlens optical fiber photoacoustic transducer which comprises a nanosecond pulse laser, a lens and a silica optical fiber, the silica optical fiber is a multimode optical fiber, one end of the silica optical fiber penetrates through the lens and is connected with the nanosecond pulse laser, and the other end of the silica optical fiber is connected with the lens. The end face of the tail end of the silica optical fiber is of a concave structure or a spherical structure, the concave structure of the tail end of the silica optical fiber is filled with a composite material, and the composite material (5) comprises a mixture of PDMS and a light absorption material. The light absorption material comprises gold nanoparticles, the diameter of the gold nanoparticles is 40-60 nm, and the resonance absorption peak of the gold nanoparticles is 530-535 nm. The method can be applied to the technical aspects of ultrasonic cleaning, ultrasonic microfluidics, ultrasonic concussion and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photoacoustic transduction, and in particular relates to a microlens optical fiber photoacoustic transducer with high photoacoustic conversion efficiency and a method thereof. Background Art

[0002] The photoacoustic effect refers to the phenomenon that sound waves are generated when a substance is irradiated with light of periodic intensity modulation. When a material is irradiated with light, the material's absorption of light will change its internal temperature, causing the structure and volume of certain areas in the material to change in a short period of time; when we use a pulsed light source to irradiate the material, the material will also expand and contract periodically with the frequency of the pulsed light, thus generating sound wave signals that propagate outward. The frequency of ultrasound generated based on the photoacoustic effect is generally above MHz, so it is a high-frequency ultrasound.

[0003] The Chinese patent with the patent publication number CN110339992A proposes a photoacoustic transducer based on transition metal sulfide and its preparation method. The transducer is arranged from bottom to top in sequence as a light absorption layer composed of carbon nanotubes and transition metal sulfide composite particles and a thermoelastic expansion layer composed of PDMS. However, due to the separation of the absorption layer and the thermoelastic expansion layer, the amount of PDMS should not be too much, resulting in a small increase in the sound pressure intensity, and there is a possibility of PDMS falling off.

[0004] Therefore, existing photoacoustic transducers have problems that still need to be solved, such as low transduction efficiency, complex manufacturing, and high cost. Summary of the invention

[0005] The purpose of the present invention is to provide a high photoacoustic conversion efficiency microlens fiber photoacoustic transducer and method, which can be applied to ultrasonic cleaning, ultrasonic microfluidics, ultrasonic oscillation and other technical aspects.

[0006] The technical solution adopted by the present invention is as follows:

[0007] A high photoacoustic conversion efficiency microlens fiber photoacoustic transducer comprises a nanosecond pulse laser, a lens and a quartz fiber, one end of the quartz fiber passes through the lens and is connected to the nanosecond pulse laser, the end face of the quartz fiber tail end is a concave structure or a spherical structure, the concave structure at the quartz fiber tail end is filled with a composite material, and the composite material (5) comprises a mixture of PDMS and a light absorbing material.

[0008] The light absorbing material comprises gold nanoparticles, the diameter of the gold nanoparticles is 40-60nm, and the resonance absorption peak is 530-535nm.

[0009] The quartz optical fiber is a multimode optical fiber with a core diameter of 40-500 μm.

[0010] The nanosecond pulse laser is used to generate nanosecond pulse laser with a wavelength of 532nm, a pulse width of 10-200ns, a repetition frequency of 1-100kHz, and a power of 400-800mW.

[0011] The size of the concave structure or the spherical structure is equal to the diameter of the quartz optical fiber, and the convex and deep radii of the concave structure or the spherical structure are 40-500 μm.

[0012] The ratio of the PDMS matrix to the gold nanoparticles is any one of 10:1, 5:1, and 20:1, and the refractive index of the PDMS matrix material is 1.4.

[0013] A method for preparing a microlens optical fiber photoacoustic transducer with high photoacoustic conversion efficiency, the method comprising the following steps:

[0014] S1: Use a fiber cleaver to cut both ends of the optical fiber to ensure that the end faces of the optical fiber are flush, so that it produces a stable spherical structure under the action of the laser, and use a femtosecond laser to carve a smooth and stable spherical surface on the flat end face of the optical fiber;

[0015] S2: Evenly mix the configured PDMS matrix material and the light absorption layer to form a photoacoustic medium, immerse a section of the engraved optical fiber into the mixture, use liquid tension to fill the end face with the mixture, then hang the optical fiber vertically, and form a hemispherical droplet on the end face of the optical fiber through the gravity and tension of the mixture itself, and then heat the end face of the optical fiber to solidify the mixture to form an absorption layer;

[0016] S3: At the other end of the optical fiber, the positions of the nanosecond pulse laser, lens, and quartz optical fiber are adjusted so that the input laser can be stably coupled into the quartz optical fiber. The laser converges on the light absorption layer after being transmitted through the optical fiber, making the energy more concentrated.

[0017] S4: After the laser enters the light absorption layer, the light radiation energy is absorbed and converted into heat energy. Then, due to the thermoelastic effect of the light absorption layer, elastic expansion occurs. When a pulsed laser is used as the light source, the heat generated is also modulated by the time interval of the pulses. In the gap between the transmission of two pulses, the light absorption layer will shrink due to the loss of heat. During the expansion and contraction of the material, ultrasonic waves are generated in the liquid environment.

[0018] S5: When the sound waves can propagate stably in the surrounding liquid medium, it means that the structure has become stable and the fiber photoacoustic transducer is completed.

[0019] The PDMS matrix material and the spherical structure at the tail end of the quartz optical fiber are used to make a microlens, which is used to converge the incident light in the light absorption layer to increase the light energy density; by controlling the radius of the spherical structure and the retention amount of the PDMS matrix material on the end face, photoacoustic transducers with different focal points and efficiencies are obtained.

[0020] The concave structure at the tail end of the quartz optical fiber is made by etching with chemical reagents, and a microlens is constructed on the end face of the optical fiber by any one of 3D printing and two-photon polymerization printing.

[0021] The technical effects achieved by the present invention are:

[0022] A high photoacoustic conversion efficiency microlens fiber photoacoustic transducer and method of the present invention forms a microlens on the fiber end face and the light absorption layer, which can converge light and has a higher energy density on the light propagation path. Under the same material conditions, the light source power required to excite ultrasonic signals is lower than that of other fiber ultrasonic transducers. In addition, optical fiber is used as a carrier for transmitting light and exciting sound waves. Compared with a spatial light photoacoustic converter, it has a simpler structure, a smaller size, is easier to integrate, and has more flexible application scenarios.

[0023] The high photoacoustic conversion efficiency microlens fiber photoacoustic transducer and method of the present invention are simple to prepare, and only require multimode optical fiber, light absorbing material, PDMS and a small amount of lithium bromide powder to complete the preparation; and for those with damaged end face structures, the tail end can be directly cut off, and then the end face can be remade and filled with absorbing material for reuse.

[0024] The high photoacoustic conversion efficiency microlens fiber photoacoustic transducer and method of the present invention use optical fiber as the carrier of the photoacoustic converter. Compared with the traditional electrical acoustic wave transducer, its volume is greatly reduced, and its anti-electromagnetic interference ability is greatly improved, and it can be applied to a wider range of fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 is a schematic structural diagram of a fiber optic photoacoustic transducer according to an embodiment of the present invention;

[0026] Figure 2 is a schematic diagram of a fiber photoacoustic transducer according to an embodiment of the present invention;

[0027] Figure 3 It is a structural schematic diagram of the spherical structure and the concave structure of the end face of the quartz optical fiber tail end according to an embodiment of the present invention;

[0028] Figure 4 It is a flow chart of preparing the fiber optic photoacoustic transducer according to an embodiment of the present invention.

[0029] In the accompanying drawings, the components represented by the reference numerals are listed as follows:

[0030] 1. Nanosecond pulse laser; 2. Lens; 3. Quartz optical fiber; 4. Recessed structure; 5. Light absorption layer; 6. Gold nanoparticles. DETAILED DESCRIPTION

[0031] In order to make the purpose and advantages of the present invention more clearly understood, the present invention is specifically described below in conjunction with embodiments. It should be understood that the following text is only used to describe one or several specific embodiments of the present invention, and does not strictly limit the scope of protection of the specific claims of the present invention.

[0032] Embodiment 1:

[0033] like Figure 1-Figure 4 As shown, a high photoacoustic conversion efficiency microlens fiber photoacoustic transducer includes a nanosecond pulse laser 1, a lens 2 and a quartz fiber 3, one end of the quartz fiber 3 passes through the lens 2 and is connected to the nanosecond pulse laser 1, the end face of the tail end of the quartz fiber 3 is a concave structure 4 or a spherical structure, and the concave structure 4 at the tail end of the quartz fiber 3 is filled with a composite material 5, and the composite material 5 includes a mixture of PDMS and a light absorbing material. Based on the light absorbing material absorbing the excitation laser and converting the light energy into heat energy and transferring it to the thermal expansion material, the thermal elastic expansion thereof is triggered, thereby converting the pulse laser into an ultrasonic pulse.

[0034] The light absorbing material comprises gold nanoparticles 6, the diameter of the gold nanoparticles 6 is 40-60 nm, and the resonance absorption peak is 530-535 nm.

[0035] The quartz optical fiber 3 is a multimode optical fiber, the depth and radius of the spherical surface can be adjusted according to actual needs, and the core diameter is 40-500 μm.

[0036] The nanosecond pulse laser 1 is used to generate a nanosecond pulse laser with a wavelength of 532nm, a pulse width of 10-200ns, a repetition frequency of 1-100kHz, and a power of 400-800mW. Other nanosecond pulse light sources such as 650nm, 980nm, 1064nm, 1310nm and 1550nm can also be used. The nanosecond pulse laser is focused by the lens 2 and coupled into the quartz optical fiber 3.

[0037] The size of the concave structure 4 or the spherical structure is equal to the diameter of the quartz optical fiber 3, and the convex and deep radii of the concave structure 4 or the spherical structure are 40-500 μm.

[0038] The ratio of the PDMS matrix to the gold nanoparticles 6 is any one of 10:1, 5:1, and 20:1, and the refractive index of the PDMS matrix material is 1.4, which is lower than the refractive index of the optical fiber core. By adding lithium bromide or other high refractive index materials, the refractive index after curing can be higher than the refractive index of the core, or other matrix materials or adhesive materials with higher thermoelastic effects can also be used.

[0039] Embodiment 2:

[0040] like Figure 4 As shown in the figure, the fabrication process of the microlens fiber photoacoustic transducer is described:

[0041] Turn on the pulse laser, determine the best positions for lens 2 and quartz optical fiber 3 according to the focal length of lens 2 and the light propagation direction, determine the focal length of lens 2 by detecting the light spot size after lens 2, and determine the best position for optical fiber by detecting the output optical power at the end of quartz optical fiber 3;

[0042] Use an optical fiber stripper to remove the coating layers at both ends of the multimode quartz optical fiber 3, and use an optical fiber cutter to cut the optical fiber with the coating layer removed to ensure that both ends of the optical fiber are flat, so that the optical fiber can form a regular spherical depression under the etching of the femtosecond laser. The size of the depression is designed to be a smooth spherical depression with a diameter of 125 μm, a curved radius of 190 μm, and a depth of 22 μm;

[0043] A PDMS matrix and a curing agent are mixed in a ratio of 10:1 as a matrix material, lithium bromide is quantitatively added thereto to gradually increase the refractive index of the matrix material until the refractive index of the matrix material after curing is higher than the core refractive index of the quartz optical fiber 3, and gold nanoparticles 6 are added with a mass equivalent to about 10% of the matrix material and a particle size of 40-60 nm, and the mixture is mixed evenly using an ultrasonic oscillator to complete the pre-preparation of the liquid absorption layer material;

[0044] Specifically, the PDMS uses a product of the brand Dow Corning, model DC184, which consists of two parts when purchased, namely A glue and B glue, which are mixed to form PDMS. A glue is the PDMS base, and B glue is its special curing agent, and the two are usually mixed in a ratio of 10:1.

[0045] The quartz optical fiber 3 is controlled by a micro-manipulator, and its end is vertically immersed in the light absorbing layer material. The liquid tension is used to fill the depression with the liquid light absorbing layer material. The mechanical arm is raised to allow the liquid to naturally fall on the end surface to form a hemispherical droplet. The optical fiber is kept vertical, and the end surface of the optical fiber is heated to solidify the absorption layer material into a photoacoustic absorption layer.

[0046] A nanosecond pulsed green laser is provided and coupled into the quartz optical fiber 3 through the coupling lens 2. The tail end of the quartz optical fiber 3 generates stable ultrasonic waves that can be detected in the liquid environment, thereby completing the preparation of the microlens optical fiber photoacoustic transducer.

[0047] In this way, for the microlens high photoacoustic conversion efficiency optical fiber photoacoustic transducer prepared according to the above steps, the nanosecond pulse laser emits laser light, which is coupled into the quartz optical fiber 3 through the lens 2. Since the optical fiber has a certain numerical aperture, the laser light evenly reaches the concave surface at the tail end of the quartz optical fiber. Since the refractive index of the light absorption layer is higher than that of the core at this time, the light absorption layer plays the role of a microlens, which can converge the input light to the center, and the converged light beam energy is more concentrated, so that the light absorption layer has a higher photothermal conversion efficiency.

[0048] Embodiment 3:

[0049] Turn on the femtosecond laser, determine the best positions for lens 2 and quartz optical fiber 3 according to the focal length of lens 2 and the light propagation direction, determine the focal length of lens 2 by detecting the light spot size after lens 2, and determine the best position for optical fiber by detecting the output light power at the end of quartz optical fiber 3;

[0050] Use an optical fiber stripper to remove the coating layers at both ends of the multimode quartz optical fiber 3, and use an optical fiber cutter to cut the optical fiber with the coating removed to ensure that both ends of the optical fiber are flat, so that the optical fiber can form a regular spherical protrusion under the etching of the femtosecond laser, and the protrusion is a spherical surface with a radius of 300 μm;

[0051] The PDMS substrate and the curing agent are mixed in a ratio of 10:1 as the substrate material, and gold nanoparticles 6 with a mass equivalent to about 10% of the substrate material and a particle size of 40-60 nm are added, and the mixture is mixed evenly using an ultrasonic oscillator to complete the pre-preparation of the liquid absorption layer material;

[0052] The quartz optical fiber 3 is controlled by a micro-manipulator, and its end is vertically immersed in the absorption layer material. The liquid absorption layer material is filled with the depression by using liquid tension. The mechanical arm is raised to allow the liquid to naturally fall on the end surface to form a hemispherical droplet. The optical fiber is kept vertical, and the end surface of the optical fiber is heated to solidify the absorption layer material into a photoacoustic absorption layer. This operation can be repeated many times to gradually increase the thickness of the absorption layer. The thickness adopted in this embodiment is 50 μm.

[0053] A nanosecond pulsed green laser is set up and coupled into the quartz optical fiber through the coupling lens 2. The tail end of the quartz optical fiber 3 generates stable ultrasonic waves that can be detected in the liquid environment, completing the preparation of the microlens fiber photoacoustic transducer.

[0054] In this way, for the microlens high photoacoustic conversion efficiency optical fiber photoacoustic transducer prepared according to the above steps, the nanosecond pulse laser emits laser light, which is coupled into the quartz optical fiber 3 through the lens 2. Since the optical fiber has a certain numerical aperture, the laser light evenly reaches the concave surface at the tail end of the quartz optical fiber. Since the refractive index of the light absorption layer is lower than that of the fiber core at this time, the laser light entering the light absorption layer will be deflected toward the center direction, playing the role of a microlens. The energy of the converged light beam is more concentrated, which reduces the optical power required for the absorption layer to reach the limit expansion value, shortens the expansion time, and improves the photoacoustic conversion efficiency.

[0055] Embodiment 4:

[0056] According to the operating steps of Example 2, with other operations unchanged, the light absorbing material in the light absorbing layer can be replaced by multi-walled carbon nanotubes.

[0057] The PDMS matrix and the curing agent are mixed in a ratio of 20:1 as the matrix material, and multi-arm carbon nanotubes with a mass equivalent to about 10% of the matrix material and a diameter of about 10-20 nm are added, and the mixture is mixed evenly using an ultrasonic oscillator to complete the pre-preparation of the liquid absorption layer material;

[0058] The quartz optical fiber 3 is controlled by a micro-manipulator, and its end is vertically immersed in the absorption layer material. The liquid absorption layer material is filled with the depression by using the liquid tension. The mechanical arm is raised to allow the liquid to naturally fall on the end surface to form a hemispherical droplet. The optical fiber is kept vertical, and the end surface of the optical fiber is heated to solidify the absorption layer material into a photoacoustic absorption layer.

[0059] A nanosecond pulsed green laser is provided and coupled into the quartz optical fiber 3 through the coupling lens 2. The tail end of the quartz optical fiber 3 generates stable ultrasonic waves that can be detected in the liquid environment, thereby completing the preparation of the microlens optical fiber photoacoustic transducer.

[0060] The above embodiments provide a group of specific components of the ultrasonic transducer:

[0061] The core diameter of the quartz fiber 3 used in the above embodiments is 105 / 125, based on the all-quartz fiber 3 structure, with a standard core diameter of 105 μm and a cladding diameter of 125 μm;

[0062] The gold nanoparticles 6 have a particle size of 50 nm, and the absorption peak of the corresponding nanoparticles is at 535 nm;

[0063] The diameter of multi-walled carbon nanotubes is about 10-20nm, and the absorption rate in the ultraviolet and visible light bands is as high as 99.5%, and the absorption rate in the slightly longer wavelength band and far infrared band is also up to 98%;

[0064] The lens 2 is selected as a 10×, 0.25NA objective lens, and the size of the light spot at the focus can reach less than 100 microns;

[0065] The wavelength of the nanosecond pulse laser 1 is 532 nm, the pulse width is 50 ns, the repetition frequency is 10 kHz, and the average power is 400 to 800 mW.

[0066] The tail end of the quartz optical fiber 3 can be engraved with specific concave and convex structures on the end face by femtosecond laser engraving, and the processing accuracy can reach the micron level. When conditions are insufficient, the chemical etching method can be used to corrode the optical fiber end face with hydrofluoric acid. By controlling the etching time and the concentration of hydrofluoric acid, a conical depression can be etched in the optical fiber. The optical fiber end face can also be ground to make it a truncated cone. By controlling the grinding angle and depth, the incident laser can be totally reflected at the side of the truncated cone, so that the incident laser is reflected and converges to the center.

[0067] Embodiment 5:

[0068] A method for preparing a microlens optical fiber photoacoustic transducer with high photoacoustic conversion efficiency, the method comprising the following steps:

[0069] S1: Use a fiber cleaver to cut both ends of the optical fiber to ensure that the end faces of the optical fiber are flush, so that it produces a stable spherical structure under the action of the laser, and use a femtosecond laser to carve a smooth and stable spherical surface on the flat end face of the optical fiber;

[0070] S2: Evenly mix the configured PDMS matrix material and the light absorption layer to form a photoacoustic medium, immerse a section of the engraved optical fiber into the mixture, use liquid tension to fill the end face with the mixture, then hang the optical fiber vertically, and form a hemispherical droplet on the end face of the optical fiber through the gravity and tension of the mixture itself, and then heat the end face of the optical fiber to solidify the mixture to form an absorption layer;

[0071] S3: The positions of the nanosecond pulse laser 1, lens 2, and quartz fiber 3 are adjusted at the other end of the optical fiber so that the input laser can be stably coupled into the quartz fiber 3. The laser converges on the light absorption layer after being transmitted through the optical fiber, making the energy more concentrated.

[0072] S4: After the laser enters the light absorption layer, the light radiation energy is absorbed and converted into heat energy. Then, due to the thermoelastic effect of the light absorption layer, elastic expansion occurs. When a pulsed laser is used as the light source, the heat generated is also modulated by the time interval of the pulses. In the gap between the transmission of two pulses, the light absorption layer will shrink due to the loss of heat. During the expansion and contraction of the material, ultrasonic waves are generated in the liquid environment.

[0073] S5: When the sound waves can propagate stably in the surrounding liquid medium, it means that the structure has become stable and the fiber photoacoustic transducer is completed.

[0074] The spherical structure of the PDMS matrix material and the tail end of the quartz optical fiber 3 is used to make a microlens, which is used to converge the incident light in the light absorption layer to increase the light energy density; the threshold power for exciting the photoacoustic effect is reduced, and the photoacoustic conversion efficiency of the transducer is enhanced. Under the same input power, due to the higher energy density, the sound pressure generated by the excitation is also stronger. By controlling the radius of the spherical structure and the retention amount of the PDMS matrix material on the end face, photoacoustic transducers with different focal points and efficiencies can be obtained.

[0075] The recessed structure 4 at the tail end of the quartz optical fiber 3 is made by etching with chemical reagents (such as hydrofluoric acid, etc.), and a microlens is constructed on the end face of the optical fiber by any one of 3D printing and two-photon polymerization printing.

[0076] The above is only a preferred embodiment of the present invention. It should be noted that, for those skilled in the art, several improvements and modifications can be made without departing from the principles of the present invention, and these improvements and modifications should also be considered as the protection scope of the present invention. The structures, devices and operating methods not specifically described and explained in the present invention shall be implemented according to the conventional means in the art unless otherwise specified and limited.

Claims

1. A microlens fiber photoacoustic transducer with high photoacoustic conversion efficiency, characterized in that: The invention comprises a nanosecond pulse laser (1), a lens (2) and a quartz optical fiber (3) which are arranged in sequence, wherein one end of the quartz optical fiber (3) passes through the lens (2) and is connected to the nanosecond pulse laser (1), the end face of the tail end of the quartz optical fiber (3) is a concave structure (4) or a spherical structure, and the concave structure (4) at the tail end of the quartz optical fiber (3) is filled with a composite material (5); The composite material (5) comprises a mixture of PDMS and a light absorbing material.

2. A high photoacoustic conversion efficiency microlens fiber photoacoustic transducer according to claim 1, characterized in that: The light absorbing material comprises gold nanoparticles (6), the diameter of the gold nanoparticles (6) is 40-60 nm, and the resonance absorption peak is 530-535 nm.

3. The high photoacoustic conversion efficiency microlens fiber photoacoustic transducer according to claim 1, characterized in that: The quartz optical fiber (3) is a multimode optical fiber, and the core diameter is 40-500 μm.

4. The high photoacoustic conversion efficiency microlens fiber photoacoustic transducer according to claim 1, characterized in that: The nanosecond pulse laser (1) is used to generate nanosecond pulse laser with a wavelength of 532nm, a pulse width of 10-200ns, a repetition frequency of 1-100kHz, and a power of 400-800mW.

5. The high photoacoustic conversion efficiency microlens fiber photoacoustic transducer according to claim 1, characterized in that: The size of the concave structure (4) or the spherical structure is equal to the diameter of the quartz optical fiber (3), and the convex and deep radii of the concave structure (4) or the spherical structure are 40-500 μm.

6. The high photoacoustic conversion efficiency microlens fiber photoacoustic transducer according to claim 1, characterized in that: The refractive index of the PDMS matrix material is 1.

4.

7. A method for preparing a microlens fiber photoacoustic transducer with high photoacoustic conversion efficiency, used for manufacturing the microlens fiber photoacoustic transducer with high photoacoustic conversion efficiency as claimed in any one of claims 1 to 6, characterized in that: The preparation method comprises the following steps: S1: Use a fiber cleaver to cut both ends of the optical fiber to ensure that the end faces of the optical fiber are flush, so that it produces a stable spherical structure under the action of the laser, and use a femtosecond laser to carve a smooth and stable spherical surface on the flat end face of the optical fiber; S2: Evenly mix the configured PDMS matrix material and the light absorption layer to form a photoacoustic medium, immerse a section of the engraved optical fiber into the mixture, use liquid tension to fill the end face with the mixture, then hang the optical fiber vertically, and form a hemispherical droplet on the end face of the optical fiber through the gravity and tension of the mixture itself, and then heat the end face of the optical fiber to solidify the mixture to form an absorption layer; S3: The positions of the nanosecond pulse laser (1), the lens (2) and the quartz optical fiber (3) are adjusted at the other end of the optical fiber so that the input laser can be stably coupled into the quartz optical fiber (3). The laser is transmitted through the optical fiber and converges on the light absorption layer, so that the energy is more concentrated. S4: After the laser enters the light absorption layer, the light radiation energy is absorbed and converted into heat energy. Then, due to the thermoelastic effect of the light absorption layer, elastic expansion occurs. When a pulsed laser is used as the light source, the heat generated is also modulated by the time interval of the pulses. In the gap between the transmission of two pulses, the light absorption layer will shrink due to the loss of heat. During the expansion and contraction of the material, ultrasonic waves are generated in the liquid environment. S5: When the sound waves can propagate stably in the surrounding liquid medium, it means that the structure has become stable and the fiber photoacoustic transducer is completed.

8. The method for preparing a microlens fiber photoacoustic transducer with high photoacoustic conversion efficiency according to claim 7, characterized in that: The PDMS matrix material and the spherical structure at the end of the quartz optical fiber (3) are used to make a microlens, which is used to converge the incident light in the light absorption layer to increase the light energy density; by controlling the radius of the spherical structure and the amount of PDMS matrix material retained on the end face, photoacoustic transducers with different focal points and efficiencies are obtained.

9. The method for preparing a microlens fiber photoacoustic transducer with high photoacoustic conversion efficiency according to claim 8, characterized in that: The recessed structure (4) at the tail end of the quartz optical fiber (3) is produced by etching with chemical reagents, and a microlens is constructed on the end face of the optical fiber by using any one of 3D printing and two-photon polymerization printing.

Citation Information

Patent Citations

  • High-consistency photoacoustic excitation and detecting integrated fiber probe, manufacturing method and testing method thereof

    CN109781625A

  • High-directivity optical fiber photoacoustic transducer and method

    CN112317285A

  • Ultrasonic fixed-point cleaning device and method based on photoacoustic jet flow effect

    CN112317450A

  • Micro-actuator device

    JP2005040874A

  • Ultrasound transducer assembly, probe, endoscopy system and manufacturing method

    US20220133262A1

Cited By

  • Broadband omnidirectional point sound source generation device

    CN114189784A