Steel pipe machining process and steel pipe

By combining cold drawing and cold rolling processes, cold rolling is directly carried out to control deformation rates to improve the strength and surface smoothness of steel pipes, solving the problems of steel pipe strength and surface quality in traditional processes, shortening the processing cycle and reducing costs .

CN118950736APending Publication Date: 2024-11-15XCMG HYDRAULICS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411367958.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-11-15

AI Technical Summary

Technical Problem

Traditional independent cold drawing and cold rolling processes cannot meet the needs of high strength, high hardness and good surface quality of metal materials at the same time, and increase production costs and processing cycles.

Method used

A steel pipe processing technology is adopted, which is first cold drawing processing, and then directly cold rolling processing. By controlling the deformation rate of cold drawing and cold rolling, the two processes are combined to improve the strength and surface smoothness of the steel pipe and shorten the processing cycle.

Benefits of technology

The high strength, high hardness and smooth surface of steel pipes are achieved, while shortening the processing cycle, solving the problem of wall thickness deviation, and reducing production costs.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a steel pipe machining process and a steel pipe in the field of steel pipe machining processes, and aims to solve the problems that in the prior art, cold drawing and cold rolling processes cannot be well combined to produce the steel pipe, and the two independent process steps increase the production cost and the machining period, the steel pipe machining process comprises the following steps that a hot-rolled pipe blank is subjected to rust removal and lubricating treatment; performing cold-drawing processing on the derusted and lubricated hot-rolled pipe blank to obtain a cold-drawn pipe with a set specification; according to the method, cold-drawing machining and cold-rolling machining are combined, the cold-drawn pipe subjected to cold-drawing is directly subjected to cold-rolling machining, the steps of pretreatment and the like are not needed, the production steps are saved, cold-drawing and cold-rolling act on the whole steel pipe, the material performance of the steel pipe can be brought into full play, and the production efficiency is improved. The surface is smooth, the production cost is saved, and the processing period is shortened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the field of steel pipe processing, and in particular to a steel pipe processing technology and a steel pipe. Background Art

[0002] In the field of metal processing, cold drawing and cold rolling are two commonly used metal plastic deformation processes. The cold drawing process can improve the mechanical properties of metal materials and increase their strength and hardness, while the cold rolling process can obtain a smoother and more precise surface quality. In traditional metal processing technology, cold drawing and cold rolling are often carried out as independent process steps. That is, cold drawing is performed first, and then an independent cold rolling process is performed, or only one of the processes is selected for processing. The traditional independent cold drawing or cold rolling process cannot simultaneously meet the requirements for high strength, high hardness and good surface quality of metal materials. A single cold drawing forming process cannot solve the problem of wall thickness deviation of hot rolled tubes, and a single cold rolling forming process cannot maximize the performance of the material.

[0003] "A new production process for precision cold-drawn steel tubes", application number "202010921266.5", discloses a cold rolling, a secondary pretreatment, and a secondary cold drawing. Although both cold rolling and cold drawing are used on a tube, and a secondary pretreatment operation is performed after cold rolling, they are also two independent process processing. Only the shrinking head of the steel tube is cold drawn multiple times to obtain a steel tube with greater shrinkage stiffness and hardness, while the other sections of the steel tube are only cold rolled. The patent increases the deformation length to make the plasticity more stable and improve the wall thickness deviation of the steel tube. However, as the length of the deformation zone increases, the contact area between the steel tube and the die increases, the friction increases, the pulling force increases, and the stress on the tube cross section increases, resulting in local necking and fracture of the material. Cold rolling is first performed followed by cold drawing, and the pretreatment and cold drawing process after cold rolling will affect the smooth surface and wall thickness deviation obtained after cold rolling.

[0004] Therefore, the existing technology cannot well combine the cold drawing and cold rolling processes to produce steel pipes, and the two independent process steps increase the production cost and processing cycle. Summary of the invention

[0005] The purpose of the present application is to provide a steel pipe processing technology and a steel pipe, wherein the pipe blank is directly cold-rolled after cold drawing, and the strength and hardness of the steel pipe can be improved after cold drawing. The cold rolling is directly performed after cold drawing, so that the surface of the steel pipe is smoother and the processing cycle of the steel pipe can be shortened.

[0006] In order to solve the above technical problems, the following technical solutions are adopted:

[0007] In a first aspect, the present application provides a steel pipe processing process, comprising the following steps:

[0008] A. Derust and lubricate the hot-rolled tube blank;

[0009] B. Cold drawing the hot-rolled tube billet after rust removal and lubrication to obtain a cold-drawn tube of set specifications;

[0010] C. The cold drawn tube is subjected to cold rolling to obtain a steel tube.

[0011] Optionally, the specific steps of the rust removal and lubrication treatment include pickling, phosphating and saponification.

[0012] Optionally, the cold drawing process in step B is to cold draw the hot-rolled tube that has been derusted and lubricated once.

[0013] Optionally, the cold rolling process in step C is to perform one cold rolling on the cold drawn tube.

[0014] Optionally, during the cold drawing process in step B, the deformation rate is between 1.15 and 1.4.

[0015] Optionally, during the cold rolling process in step C, the deformation rate is between 1.15-1.35.

[0016] Optionally, after obtaining the steel pipe in step C, the steel pipe is subjected to stress relief annealing, straightening and sawing to length to obtain a finished product.

[0017] In a second aspect, the present application provides a steel pipe, which is manufactured using the steel pipe processing process described in any one of the first aspects.

[0018] Compared with the prior art, the present invention has the following beneficial effects:

[0019] 1. The present invention combines cold drawing and cold rolling, directly cold rolling the cold drawn tube after cold drawing, without the need for pretreatment and other steps, thus saving production steps. Cold drawing and cold rolling act on the entire steel tube, which can maximize the material properties of the steel tube and make the surface smooth, thus saving production costs and processing cycles.

[0020] 2. The present invention performs a cold rolling after a cold drawing. It only needs to design the deformation rate and other parameters during the cold drawing and cold rolling processes to obtain a steel pipe with sufficient rigidity and meeting the smoothness requirements. By controlling the cold drawing deformation rate, the cold rolling deformation rate and the total rolling deformation rate, material classification can be achieved. DETAILED DESCRIPTION

[0021] The technical solutions in the embodiments of the present application are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present application and its application or use.

[0022] Example 1

[0023] This embodiment provides a steel pipe processing process, comprising the following steps:

[0024] A. Derust and lubricate the hot-rolled tube blank;

[0025] B. Cold drawing the hot-rolled tube billet after rust removal and lubrication to obtain a cold-drawn tube of set specifications;

[0026] C. The cold drawn tube is subjected to cold rolling to obtain a steel tube.

[0027] The hot rolled tube is processed by cold drawing to obtain the set wall thickness, inner diameter and outer diameter and other specification parameters. After obtaining the cold drawn tube of the set specifications, it is directly cold rolled to obtain a steel tube with high strength and hardness and a smooth surface.

[0028] Example 2

[0029] Step B in Example 1 is to perform a cold drawing process, and the cold drawn tube after the cold drawing directly enters step C for a cold rolling process to obtain a high-precision steel tube, and the wall thickness deviation is controlled within ±3%. During the cold drawing process, the cold drawing deformation rate is designed to be within the range of 1.15-1.4, and during the cold rolling process, the cold rolling deformation rate is designed to be within the range of 1.15-1.35. The obtained steel tube is then subjected to stress annealing, straightening, sawing and cutting to size to obtain a finished product, which has high strength and hardness, a smooth surface, and a wall thickness deviation of ≤±3%.

[0030] A single cold drawing process can maximize the performance of the processed steel pipe and obtain a high-strength and high-hardness steel pipe, but it cannot solve the problem of wall thickness deviation of the hot-rolled pipe. The wall thickness deviation of the steel pipe obtained by a single cold drawing process is generally ±10%, and even if the control is tightened, it can only be ±8%. Generally, the wall thickness deviation is improved by removing material, that is, rough turning the outer ring, which will cause material waste and low material utilization. In addition, there is residual stress in the cold-drawn tube. Rough turning of the outer circle has a greater impact on the cold-drawn tube (especially the slender cold-drawn tube), and there are quality risks such as deterioration of straightness and unstable inner hole processing size, which seriously affect the first-time qualified rate of the product.

[0031] Single cold rolling can improve the wall thickness deviation and obtain a smooth surface steel pipe, but it cannot bring out the maximum performance of the material. It is necessary to use materials with greater strength and hardness to process the steel pipe with the required strength and hardness. The improvement of strength is mainly achieved by improving the performance of the billet, and the improvement of billet performance is mainly achieved by increasing carbon content, tempering, adding alloy elements, etc. Different materials require steel mills to open furnaces for smelting, which brings problems such as high minimum order quantity, high procurement cost, long procurement cycle, increased costs, and poor raw material selectivity;

[0032] This application combines the cold drawing and cold rolling processes to solve the problem of wall thickness deviation of hot-rolled tubes, and at the same time obtain high-strength materials to meet the lightweight requirements of products. First, a cold drawing process is carried out. During the cold drawing process, the processing inner diameter and outer diameter are set, and the cold drawing deformation rate is determined. A cold-drawn tube of set specifications is obtained by one cold drawing. The strength and hardness of the obtained cold-drawn tube are not much different from the strength and hardness of the material used, which maximizes the performance of the material. After one cold drawing, a cold rolling process is directly carried out. The cold rolling process can not only improve the wall thickness deviation of the steel pipe, but also make the surface of the steel pipe smooth. After the cold rolling process, stress annealing, straightening, sawing and cutting to size are carried out to obtain a finished product. The finished product has high strength and hardness, a smooth surface, and a small deviation in the wall thickness of the steel pipe. After the cold rolling process, the wall thickness deviation will no longer change.

[0033] Example 3

[0034] This embodiment provides a steel pipe based on Embodiment 1 or Embodiment 2. The steel pipe is manufactured by the steel pipe processing technology provided in Embodiment 1 or Embodiment 2.

[0035] The following describes a steel pipe made from a billet of a specific alloy material using the above steel pipe processing technology.

[0036] The blank contains, in mass%, 0.20% carbon, 0.38% silicon, 1.26% manganese, 0.008% sulfur, 0.010% phosphorus, 0.13% chromium, 0.03% nickel, 0.02% molybdenum, 0.08% copper, 0.05% vanadium, and the balance is iron.

[0037] When the cold drawing deformation rate is controlled at 1.35-1.4, the cold rolling deformation rate is controlled at 1.2-1.35, and the total deformation rate is greater than 1.6, the yield strength of the produced steel pipe is not less than 760MPa, the tensile strength is not less than 820MPa, the elongation after fracture is not less than 17%, the impact energy at -20℃ is not less than 100J, and the comprehensive mechanical properties are excellent.

[0038] Example 1: The billet is φ210×14, first cold drawn to φ196×φ174, and then cold rolled to φ178×φ160.

[0039] Specifically: the hot-rolled tube billet specification (outer diameter × wall thickness) is φ210×14, and after pickling, phosphating and saponification treatment, it is cold drawn to φ196×φ174 (outer diameter × inner diameter), and the deformation rate of one cold drawing is 1.35; then cold rolled to φ178×φ160 (outer diameter × inner diameter), the cold rolling deformation rate is 1.27; the total deformation rate is 1.71.

[0040] The steel pipe produced by the above process was subjected to mechanical property tests, and the test results are as follows: the elongation strength Rp0.2=780MPa, the tensile strength Rm=820MPa, A=18.3%, and the impact energy KV2=123J when the non-proportional elongation is specified to be 0.2%.

[0041] Example 2: The billet is φ245×16, first cold drawn to φ234×φ210, and then cold rolled to φ219×φ200.

[0042] Specifically: the hot-rolled tube billet specification (outer diameter × wall thickness) is φ245×16, and after pickling, phosphating and saponification treatment, it is cold drawn to φ234×φ210 (outer diameter × inner diameter), and the deformation rate of one cold drawing is 1.38; then cold rolled to φ219×φ200 (outer diameter × inner diameter), the cold rolling deformation rate is 1.28; the total deformation rate is 1.75.

[0043] The steel pipe produced by the above process was tested for mechanical properties, and the test results were as follows: Rp0.2=795MPa, Rm=846MPa, A=18.1%, and impact energy KV2=138J.

[0044] Through the above two examples, it can be concluded that the mechanical properties of the steel pipes obtained at different cold drawing deformation rates and different cold rolling deformation rates are different. When the cold drawing deformation rate and the cold rolling deformation rate are larger and the total deformation rate is larger, the mechanical properties are better. It can be concluded that the deformation rate, cold rolling deformation rate and total deformation rate are proportional to the mechanical properties.

[0045] In summary, by designing the cold drawing deformation rate, cold rolling deformation rate and total rolling deformation rate, materials with different performance grades can be obtained at different levels to meet different product requirements. The cold drawing deformation rate, cold rolling deformation rate and total rolling deformation rate are controlled through the above-mentioned processing technology to achieve material classification.

[0046] The above is only a preferred implementation of the present application. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the technical principles of the present application. These improvements and modifications should also be regarded as the scope of protection of the present application.

Claims

1. A steel pipe processing technology, characterized in that: The following steps are involved: A. Derust and lubricate the hot-rolled tube blank; B. Cold drawing the hot-rolled tube billet after rust removal and lubrication to obtain a cold-drawn tube of set specifications; C. The cold drawn tube is subjected to cold rolling to obtain a steel tube.

2. The steel pipe processing process according to claim 1, characterized in that: The specific steps of the rust removal and lubrication treatment include pickling, phosphating and saponification.

3. The steel pipe processing process according to claim 1, characterized in that: The cold drawing process in step B is to perform a cold drawing on the hot-rolled tube that has been derusted and lubricated.

4. The steel pipe processing process according to claim 1, characterized in that: The cold rolling process in step C is to perform a cold rolling on the cold drawn tube.

5. The steel pipe processing process according to claim 1, characterized in that: When the cold drawing process is performed in step B, the deformation rate is between 1.15 and 1.

4.

6. The steel pipe processing process according to claim 1, characterized in that: When cold rolling is performed in step C, the deformation rate is between 1.15 and 1.

35.

7. The steel pipe processing process according to claim 1, characterized in that: After the steel pipe is obtained in step C, the steel pipe is subjected to stress relief annealing, straightening and sawing to length processing to obtain a finished product.

8. A steel pipe, characterized in that: The steel pipe is made by the steel pipe processing technology described in any one of claims 1-7.

Citation Information

Patent Citations

  • Manufacturing process of small-diameter seamless steel tubes

    CN102233365A

  • Production process of stainless steel tube for vehicle exhaust system

    CN107267731A

  • Production process of novel precise cold-drawn steel pipe

    CN112108531A

  • Lubricating oil for cold drawing, lubrication coating and method of producing cold-drawn steel tube

    JP2005177816A