Preparation method of antioxidant nano copper powder and low-temperature sintered copper paste

Through the liquid-solid reaction of L-ascorbic acid and surface modifier, the oxidized copper-based nanopowder is reduced to antioxidant nanocopper powder, solving the problem of copper nanoparticles oxidation, and achieving efficient nanocopper powder preparation and low-temperature sintering performance The improvement ensures the high strength and reliability of the sintered body.

CN118951005AActive Publication Date: 2024-11-15SHENZHEN BAROY NEW MATERIAL TECH CO LTD

Patent Information

Application Number
CN202411188697.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-15
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

Copper nanoparticles are prone to spontaneous oxidation in the air, leading to the formation of copper oxide, reducing the mechanical properties, electrical properties, thermal properties and reliability of the sintered body, and limiting its application.

Method used

The oxidized copper-based nanopowder is reduced to antioxidant nanocopper powder by liquid-solid reaction using L-ascorbic acid and surface modification agent. Ultrasonic dispersion and heating treatment are used to form nanocopper powder with oxidation resistance and is used for low-temperature sintering. Preparation of copper slurry.

Benefits of technology

It realizes efficient reduction and surface modification of copper powder, improves the oxidation resistance and sintering performance of nano copper powder, ensures the high strength and reliability of low-temperature sintered bodies, can be mass-produced, and saves resources.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118951005A_ABST
    Figure CN118951005A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of antioxidant nano copper powder and low-temperature sintered copper paste. The preparation method of the anti-oxidation nano copper powder comprises the following steps: adding a reducing agent L-ascorbic acid and a surface modifier into pure water, and dissolving and dispersing to prepare a solution; adding copper-based nano powder into the solution, and putting the solution into ultrasonic dispersion equipment for ultrasonic dispersion to obtain dispersion liquid; the copper-based nano powder comprises at least one of nano-scale copper oxide, nano-scale cuprous oxide and nano-scale pure copper; under the stirring condition, the dispersion liquid is heated to 40-60 DEG C, and heat preservation is conducted for 10-30 min; and the dispersion liquid is subjected to centrifugal separation, ethanol cleaning and vacuum drying, and then the anti-oxidation nano copper powder is prepared. The antioxidant copper powder can be prepared through a simple liquid-solid reaction, has low-temperature sinterability, can be used for sintering copper, is simple in process, can be produced in a large scale, and saves resources.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of preparation of nano copper powder, and in particular to a preparation method of anti-oxidation nano copper powder and a low-temperature sintered copper slurry. Background Art

[0002] The integration and miniaturization of the electronic packaging industry have put forward high thermal conductivity and high reliability requirements for Cu-Cu interconnect materials, which are key processes for three-dimensional integrated circuits, chip stacking, and through-silicon via (TVS) vertical interconnection. They require low-temperature bonding and high-temperature service. Sintered silver is the welding replacement technology currently in use. Copper is cheaper than silver and has good resistance to ion migration. The current literature reports experimental verification that sintered copper is superior to sintered silver in terms of connection strength and environmental reliability.

[0003] However, copper nanoparticles are prone to spontaneous oxidation in the air. Currently, the nano copper available on the market is very easy to oxidize when exposed to air, and copper oxide forms on the surface. For relatively small particles (less than 50nm), the surface atoms account for a large proportion, and basically all of them will form copper oxide when exposed to air. The formation of copper oxide will increase the sintering temperature of copper-based nanopowders, reduce bonding performance, and reduce the mechanical properties, electrical properties, thermal properties and reliability of the sintered body, which limits the application of nano copper.

[0004] The physical vapor phase method is a relatively mature method for preparing nanopowders. In an inert atmosphere, nano copper powders can be stably produced in large quantities through steam condensation. The particle size distribution is below 200nm, and the activity is high. The nano copper powders finally obtained are partially oxidized into copper oxide and cuprous oxide, and lose the low-temperature sintering activity and conductivity of nano copper. This patent provides a simple treatment method for treating oxidized copper-based nano powders to obtain surface-modified anti-oxidation nano copper powders. It has low-temperature sintering properties and can be used for sintering interconnect copper paste applications. Summary of the invention

[0005] In order to overcome the above-mentioned shortcomings and deficiencies of the prior art, the purpose of the present invention is to provide a method for preparing an antioxidant nano copper powder, which uses copper-based nano powder (including at least one of nano-grade copper oxide, nano-grade cuprous oxide, and nano-grade pure copper) as a raw material, and can be prepared by a simple liquid-solid reaction. The process is simple and can be mass-produced. The oxidized copper powder can be reduced to nano copper powder for reuse, thereby saving resources.

[0006] The purpose of the present invention is achieved through the following technical solutions: The present invention provides a method for preparing an antioxidant nano copper powder, comprising the following steps: Adding a reducing agent, L-ascorbic acid, and a surface modifier into pure water to dissolve and disperse to form a solution; Adding copper-based nanopowder to the solution, placing it in an ultrasonic dispersion device for ultrasonic dispersion, and obtaining a dispersion; the copper-based nanopowder comprises at least one of nano-grade copper oxide, nano-grade cuprous oxide, and nano-grade pure copper; Under stirring conditions, heat the dispersion to 40-60°C and keep warm for 10-30 minutes; more preferably, the heating temperature is 50-60°C and the time is 15 minutes. ; The dispersion liquid is centrifuged, washed with ethanol, and vacuum dried to obtain the antioxidant nano copper powder.

[0007] Preferably, the surface modifier includes organic small molecules containing N functional groups and alkyd small molecules; the N functional group is an amino group or a nitrogen-containing heterocycle.

[0008] Preferably, the amount of the surface modifier is 4%-10% of the mass of the copper-based nanopowder.

[0009] Preferably, the organic small molecule containing N functional group is one of fatty amine, alanine, proline, and N-methylpyrrolidone; and the alkyd small molecule is one of lactic acid, malic acid, and citric acid.

[0010] Preferably, the molar ratio of the reducing agent L-ascorbic acid to the copper-based nanopowder is (0.1-2):1.

[0011] Preferably, the particle size of the copper-based nanopowder is 20-200 nm; the particle size of the antioxidant nano-copper powder is 50-300 nm.

[0012] Preferably, the ultrasonic dispersion time is 10-60 min; more preferably, the ultrasonic dispersion time is 15-30 min, and the powder is dispersed into a paste in the solution without agglomerated particles.

[0013] Preferably, the stirring is specifically: stirring at a rate of 200-600 rpm; more preferably, the stirring rate is 300-400 rpm.

[0014] Preferably, the concentration of the reducing agent L-ascorbic acid used is a saturated aqueous solution.

[0015] Preferably, the vacuum drying temperature is set below 45°C.

[0016] The present invention also provides a low-temperature sintered copper paste, comprising the antioxidant nano copper powder prepared by the preparation method of the antioxidant nano copper powder.

[0017] Preferably, the low-temperature sintered copper paste comprises the nano copper powder, micron copper powder and a solvent; the weight ratio of the nano copper powder to the micron copper powder is 1:(0.8-1.2); and the sintering temperature of the low-temperature sintered copper paste in an air atmosphere is 200-250°C.

[0018] Preferably, the low-temperature sintered copper paste is used for Cu-Cu interconnection on a Cu substrate, the sintering temperature in air atmosphere is 200-250° C., the insulation time is 8-12 min, the sintering pressure is 15-25 MPa, and the interconnection strength can reach above 30 MPa.

[0019] Compared with the prior art, the present invention has the following advantages and beneficial effects: (1) The method for preparing the antioxidant nano copper powder of the present invention uses copper-based nano powder (including one or more of nano copper oxide, nano cuprous oxide, and nano copper) as raw materials, uses pure water as a reaction medium, and uses a saturated aqueous solution of a reducing agent, L-ascorbic acid, to increase the concentration of the reaction system and prepare nano copper powder in large quantities; the antioxidant copper powder can be prepared by a simple liquid-solid reaction, the process is simple, and it can be produced in large quantities.

[0020] (2) The method for preparing the antioxidant nano copper powder of the present invention utilizes N-containing functional groups, -COOH functional groups and Cu to form coordination bonds or chemical bonds to coat the surface of nano copper. -OH effectively blocks the action of oxygen, making the nano copper powder antioxidant.

[0021] (3) The preparation method of the antioxidant nano copper powder of the present invention adopts a modifier having a decomposition temperature or boiling point lower than 250°C and close to the sintering temperature, so that the nano copper powder is not oxidized under pre-baking conditions and can be decomposed or volatilized at the sintering temperature. There is little or almost no organic matter remaining in the sintered body, thereby improving the interconnection strength of the sintered body.

[0022] (4) The method for preparing the antioxidant nano copper powder of the present invention is not limited to the copper-based nano powder prepared by the physical vapor phase method. The nano copper powder purchased on the market is oxidized during storage. This method can be used to reduce the nano copper powder for reuse, thus saving resources.

[0023] (5) The method for preparing the antioxidant nano copper powder of the present invention can ensure that the particle size distribution of the nano powder does not change substantially by controlling the concentration of the modifier, the ultrasonic dispersion time, and the heating temperature, and can prepare the antioxidant nano copper powder in large quantities at high concentration. If the ultrasonic time is too long and the heating and stirring temperature exceeds 70°C, the particle size of the obtained nano copper powder will be larger. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 This is a SEM image of copper-based nanopowder prepared by the steam condensation method according to an embodiment of the present invention.

[0025] Figure 2 This is the XRD diagram of the copper-based nanopowder prepared by the steam condensation method according to an embodiment of the present invention.

[0026] Figure 3 This is a SEM image of nano copper powder prepared in an embodiment of the present invention.

[0027] Figure 4 This is the XRD spectrum of the nano copper powder prepared in the embodiment of the present invention.

[0028] Figure 5 XRD comparison diagram of the nano copper powder prepared in the embodiment of the present invention stored at room temperature for different time periods.

[0029] Figure 6 SEM image of the fracture surface of the nano-copper paste sintered body in the embodiment of the present invention. DETAILED DESCRIPTION

[0030] The present invention will be further described in detail below in conjunction with examples, but the embodiments of the present invention are not limited thereto. Example

[0031] The method for preparing the antioxidant nano copper powder of the embodiment of the present invention comprises the following steps: Adding a reducing agent, L-ascorbic acid, and a surface modifier into pure water to dissolve and disperse to form a solution; Adding copper-based nanopowder to the solution, placing it in an ultrasonic dispersion device for ultrasonic dispersion, and obtaining a dispersion; the copper-based nanopowder comprises at least one of nano-grade copper oxide, nano-grade cuprous oxide, and nano-grade pure copper; Under stirring conditions, heat the dispersion to 40-60°C and keep warm for 10-30 minutes; The dispersion liquid is centrifuged, washed with ethanol, and vacuum dried to obtain the antioxidant nano copper powder.

[0032] In some embodiments of the present invention, the surface modifier includes organic small molecules containing N functional groups and alkyd small molecules; the N functional groups are amino groups or nitrogen-containing heterocycles.

[0033] In some embodiments of the present invention, the amount of the surface modifier is 4%-10% of the mass of the copper-based nanopowder.

[0034] In some embodiments of the present invention, the organic small molecule containing N functional group is one of fatty amine, alanine, proline, and N-methylpyrrolidone; the alkyd small molecule is one of lactic acid, malic acid, and citric acid.

[0035] In some embodiments of the present invention, the molar ratio of the reducing agent L-ascorbic acid to the copper-based nanopowder is (0.1-2):1.

[0036] In a specific embodiment, the preparation process of the antioxidant nano copper powder is as follows: weigh 80g of L-ascorbic acid, 7g of proline, and 3g of lactic acid, add them into 300mL of pure water to dissolve and disperse to form solution A; then weigh the copper-based nano powder (containing copper oxide and copper nano powder, SEM morphology as shown below 200nm) prepared by steam condensation method. Figure 1 , XRD Figure 2 ) 100g was added to solution A, placed in an ultrasonic dispersion device for ultrasonic dispersion for 30 minutes, and the dispersion changed from dark green to wine red. The wine red dispersion was placed on a heating device, set to 60℃ and heated and stirred for 15 minutes. Then centrifuged, washed with ethanol, and vacuum dried at 30℃ for 1 hour. Purple-red nano copper powder was obtained, the SEM morphology is shown in 3, the particle size is below 200nm, and the XRD pattern is shown in Figure 4 The prepared nano copper powder was stored at room temperature for 1 to 7 weeks. The XRD patterns of the nano copper powders at different storage times are shown in Figure 5 The results show that the characteristic peaks of copper oxide were not detected in the samples stored for 1 and 3 weeks, while trace amounts of copper oxide were detected in the samples stored for 5 and 7 weeks, indicating that the nano copper powder prepared in this example has excellent antioxidant properties.

[0037] The nano copper powder prepared in the above embodiment is configured with a press-sintered nano-micro composite copper slurry: 50 g of the prepared nano copper powder, 50 g of purchased micron powder (particle size 1 μm~3 μm), and 30 g of a mixed solvent (ethylene glycol: butoxycarbonyl alcohol: terpineol: ethyl cellulose = 8:10:5:0.6), stirred, mixed with a three-roll mill, and degassed to prepare a nano-micro composite copper slurry.

[0038] Coat a 100-micron thick copper paste on a clean copper substrate, pre-bake at 80°C for 20 minutes, then place another clean copper substrate on the workbench of the hot press bonding equipment, pressurize to 20MPa, keep warm at 220°C for 10 minutes, take it out and cool it naturally. Use a push-pull tester to test the bonding strength, the bonding strength is 36.04MPa. Push open the cross section and use SEM to analyze the microstructure, such as Figure 6 Nano-copper and micro-copper form a sintered interconnected network, and the cross section is obviously plastic fracture when pushed open.

[0039] The present invention utilizes the small size of nano powder and the large specific surface area, and the oxidized part is reduced in situ in the presence of a modifier. By controlling the concentration of the modifier, the ultrasonic dispersion time, and the heating temperature, the particle size distribution of the nano powder can be ensured to remain substantially unchanged, and the anti-oxidation nano copper powder can be prepared in large quantities at a high concentration. If the ultrasonic time is too long and the heating and stirring temperature exceeds 70°C, the particle size of the obtained nano copper powder will be larger than that of the raw material nano powder.

[0040] The nano-micro composite sintered copper paste prepared by the present invention is used for Cu-Cu interconnection on a Cu substrate. The air atmosphere is 220° C., the sintering pressure is 20 MPa, and the heat preservation is 10 minutes. The interconnection strength can reach more than 30 MPa.

[0041] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.

Claims

1. A method for preparing an antioxidant nano copper powder, It is characterized in that The following steps are involved: Adding a reducing agent, L-ascorbic acid, and a surface modifier into pure water to dissolve and disperse to form a solution; Adding copper-based nanopowder to the solution, placing it in an ultrasonic dispersion device for ultrasonic dispersion, and obtaining a dispersion; the copper-based nanopowder comprises at least one of nano-grade copper oxide, nano-grade cuprous oxide, and nano-grade pure copper; Under stirring conditions, heat the dispersion to 40-60°C and keep warm for 10-30 minutes; The dispersion liquid is centrifuged, washed with ethanol, and vacuum dried to obtain the antioxidant nano copper powder.

2. The method for preparing the antioxidant nano copper powder according to claim 1, It is characterized in that The surface modifier comprises organic small molecules containing N functional groups and alkyd small molecules; the N functional groups are amino groups or nitrogen-containing heterocycles.

3. The method for preparing the antioxidant nano copper powder according to claim 2, It is characterized in that The amount of the surface modifier used is 4%-10% of the mass of the copper-based nanopowder.

4. The method for preparing the antioxidant nano copper powder according to claim 2, It is characterized in that The organic small molecule containing N functional group is one of fatty amine, alanine, proline and N-methylpyrrolidone; the alkyd small molecule is one of lactic acid, malic acid and citric acid.

5. The method for preparing the antioxidant nano copper powder according to claim 1, It is characterized in that The molar ratio of the reducing agent L-ascorbic acid to the copper-based nanopowder is (0.1-2):

1.

6. The method for preparing the antioxidant nano copper powder according to claim 1, It is characterized in that The particle size of the copper-based nano powder is 20-200 nm; the particle size of the anti-oxidation nano copper powder is 50-300 nm.

7. The method for preparing the antioxidant nano copper powder according to claim 1, It is characterized in that The ultrasonic dispersion time is 10-60 min.

8. The method for preparing the antioxidant nano copper powder according to claim 1, It is characterized in that The stirring is specifically: stirring at a speed of 200-600 / min.

9. A low-temperature sintered copper paste, comprising the antioxidant nano copper powder prepared by the method for preparing the antioxidant nano copper powder according to any one of claims 1 to 9.

10. The low temperature sintered copper paste according to claim 1, It is characterized in that The invention comprises the nano copper powder, micron copper powder and solvent; the weight ratio of the nano copper powder to the micron copper powder is 1:(0.8-1.2); the sintering temperature of the low-temperature sintered copper paste in air atmosphere is 200-250°C.

Citation Information

Patent Citations

  • Nano copper particle and low-cost green environment-friendly preparing method thereof

    CN108971513A

  • Preparation method of copper nano material

    CN113996799A

  • Palladium submicron sphere-like silver powder and preparation method thereof

    CN116786833A

  • Method for preparing cuprous oxide in nanoscale cubicform and cuprous oxide in nanoscale cubic formprepared by the same

    KR1020050119451A

  • Superfine copper powder slurry and process for producing the same

    WO2006068061A1

Cited By

  • Preparation method of wide-distribution nano copper powder

    CN121669916A