Non-fuzzing and non-wrinkling plain woven fabric netting material and preparation method thereof
By pasting on the polymer film and hot pressing and bonding with the plain cloth, the burrs and wrinkles of the plain cloth clamping material during cutting and welding are solved, and a flat finished product is achieved, expanding its application range. .
Patent Information
- Application Number
- CN202411390163.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-08
- Publication Date
- 2024-11-15
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The problem of plain woven fabric clamping materials being easy to blem after cutting and wrinkle easily after high-frequency welding limits its application range.
After the paste is applied on one side of the polymer film, dry it and the paste film is hot pressed to bond with a plain cloth to improve the shrinkage of the polymer film material to solve the burrs and wrinkles during cutting and welding question.
The plain woven fabric clamp material prepared by the above method is burnt after cutting, and is flat and wrinkle-free after welding, which expands its application range and ease of use.
Smart Images

Figure CN118952679A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of sandwich composite materials, and particularly relates to a plain woven sandwich material that is not prone to fuzzing and wrinkling and a preparation method thereof. Background Art
[0002] The mesh material, also known as the interlayer material or sandwich material, is a composite material consisting of two or more layers of membrane material and a mesh cloth. For a mesh cloth with a denser knitting, it is necessary to apply paste on both sides of the mesh cloth before bonding with the membrane. For example, the Chinese invention patent with application number 201811421269.1 discloses a mesh cloth for high-pressure PVC tent air column, which is obtained by applying the paste coating slurry on the high-strength polyester fiber mesh cloth by a coating machine by infiltration and scraping, and then plasticizing at high temperature; then the first film, the second film and the mesh cloth are fully heated or preheated, and the three layers are bonded together at the bonding embossing device. When plain woven cloth is used as the mesh cloth to prepare the mesh material, since the mesh of the plain woven cloth is larger, it is not necessary to apply paste. When bonding, the films on both sides of the mesh cloth can be directly contacted through the mesh of the mesh cloth to achieve bonding without the use of paste. However, the mesh material produced by this method is prone to fuzzing at the cutting point and wrinkling due to high-frequency welding. Summary of the invention
[0003] The technical problem to be solved by the present invention is to provide a plain woven cloth sandwich material which does not fuzz after cutting and does not wrinkle after welding, and a preparation method thereof.
[0004] In order to solve the above technical problems, the technical solution adopted by the present invention is: a method for preparing a plain woven mesh material that is not easy to pilling and wrinkling, comprising the following steps: applying a paste to one side of a polymer film, and obtaining a pasted polymer film after drying; then placing the two polymer films with the paste side facing the two sides of the plain woven fabric respectively, and hot pressing and bonding them.
[0005] Another technical solution adopted by the present invention is: the flat woven cloth sandwich material which is not easy to fuzz and wrinkle is prepared by the above-mentioned preparation method.
[0006] The beneficial effect of the present invention is that: the preparation method provided by the present invention first performs a pasting treatment on the polymer film to be bonded, improves the shrinkage of the polymer film material, and then bonds it to the plain woven mesh. When the obtained plain woven mesh material is subsequently cut, the cutting part is flat and has no burrs; the obtained plain woven mesh material is also very flat when high-frequency welding is subsequently performed, and no wrinkles will occur. This makes the product application simpler and more extensive. BRIEF DESCRIPTION OF THE DRAWINGS
[0007] Figure 1 This is a diagram showing the effect of a flat woven mesh material that is not prone to fuzzing and wrinkling after cutting according to an embodiment of a specific embodiment of the present invention;
[0008] Figure 2 This is a picture showing the effect of a flat woven mesh material that is not prone to fuzzing and wrinkling after high-frequency welding in an embodiment of a specific implementation manner of the present invention;
[0009] Figure 3 This is a diagram showing the effect of a plain woven mesh material of a comparative example after cutting in a specific embodiment of the present invention;
[0010] Figure 4 This is a diagram showing the effect of a plain woven mesh material of a comparative example after high-frequency welding in a specific embodiment of the present invention. DETAILED DESCRIPTION
[0011] In order to explain the technical content, achieved objectives and effects of the present invention in detail, the following is an explanation in conjunction with the implementation modes and the accompanying drawings.
[0012] The method for preparing a flat woven fabric sandwich material which is not easy to fuzz and wrinkle comprises the following steps: applying paste to one side of a polymer film, drying to obtain the pasted polymer film; and then placing the two polymer films with the paste on the two sides of the flat woven fabric and hot pressing them together.
[0013] From the above description, it can be seen that the beneficial effect of the present invention is that: in the common method of preparing mesh cloth, there is also a method of using paste for pre-treatment, but the mesh cloth is first soaked in paste, or the paste is applied on both sides of the mesh cloth. However, when this method is applied to a large-mesh plain woven mesh cloth, it cannot improve the problem of burrs after cutting and wrinkles after high-frequency welding of the finished product. The present invention breaks through conventional thinking by first applying paste to the polymer film to be bonded, and then bonding it to the plain woven mesh cloth, thereby solving this problem. The obtained plain woven mesh material has no burrs after cutting and trimming, and the cutting area is smooth and flat; and it is also very flat during high-frequency welding, and the welding area is smooth and wrinkle-free. The plain woven mesh material obtained by the preparation method of the present invention is simpler to use and has a wider application space.
[0014] Furthermore, the polymer film is a PVC film or a TPU film. Both are commonly used polymer films for preparing sandwich materials, and the specific choice can be selected according to the subsequent practical application field. The PVC film and the TPU film are any commercially available products.
[0015] Furthermore, when the polymer film is a PVC film, the amount of glue applied during the glue treatment is 60 to 80 g / m 2 .
[0016] Furthermore, when the polymer film is a PVC film, the paste used in the pasting process includes 100 parts of E-PVC paste resin, 60-80 parts of plasticizer, 3-4 parts of liquid stabilizer and 1-3 parts of adhesive by weight. The paste composed of the above formula can effectively adjust the shrinkage of the PVC film.
[0017] Furthermore, the plasticizer is DOP, DINP or DOTP.
[0018] Furthermore, the liquid stabilizer is a barium zinc liquid stabilizer.
[0019] Furthermore, the adhesive is a PVC adhesive, preferably an isocyanate adhesive.
[0020] Furthermore, the mesh size of the plain woven fabric is 0.5-1 mm. The plain woven fabric is preferably a 500D*18*17 plain woven polyester fabric.
[0021] Furthermore, the temperature of the hot pressing bonding is 170-180° C., and the pressure is 30-40 KGF.
[0022] Furthermore, the pasted PVC film and the plain woven mesh cloth need to be preheated at 160-180° C. before lamination.
[0023] Embodiment 1 of the present invention is:
[0024] A method for preparing a flat woven mesh material that is not prone to fuzzing and wrinkling comprises the following steps:
[0025] Step 1: Apply 70g / m2 of paste on one side of the PVC film. 2 , and after drying, a PVC film with a paste is obtained; the paste is prepared by blending 100kg E-PVC paste resin, 72kg DOTP, 3kg barium zinc liquid stabilizer and 1.6kg isocyanate adhesive;
[0026] Step 2: After the PVC film and 500D*18*17 plain woven polyester cloth are preheated at 165℃ and 175℃ respectively, the two preheated PVC films with the paste facing the two sides of the plain woven mesh cloth (500D*18*17 plain woven polyester cloth) are heat-pressed at 180℃ and 30kgf to obtain a plain woven mesh material that is not easy to fuzz and wrinkle. The effect of cutting and welding the obtained plain woven mesh material that is not easy to fuzz and wrinkle is shown in the figure. Figure 1 and Figure 2 shown.
[0027] Embodiment 2 of the present invention is:
[0028] A method for preparing a flat woven mesh material that is not prone to fuzzing and wrinkling comprises the following steps:
[0029] Step 1: Apply 80g / m2 of paste on one side of the PVC film. 2 , and after drying, a PVC film with paste is obtained; the paste is prepared by blending 100kg E-PVC paste resin, 80kg DINP, 3.5kg barium zinc liquid stabilizer and 1kg isocyanate adhesive;
[0030] Step 2: After the pasted PVC film and the 500D plain woven polyester cloth with a mesh size of 0.5 mm are preheated at 160° C. and 170° C. respectively, the two preheated pasted PVC films with the paste side facing the two sides of the plain woven mesh cloth (500D plain woven polyester cloth with a mesh size of 0.5 mm) are hot-pressed and laminated at 170° C. and 40 kgf to obtain a plain woven mesh material that is not easy to pilling or wrinkle.
[0031] Embodiment 3 of the present invention is:
[0032] A method for preparing a flat woven mesh material that is not prone to fuzzing and wrinkling comprises the following steps:
[0033] Step 1: Apply 60g / m2 of paste on one side of the PVC film. 2 , and after drying, a PVC film with paste is obtained; the paste is prepared by blending 100kg E-PVC paste resin, 60kg DOP, 4kg barium zinc liquid stabilizer and 2.5kg isocyanate adhesive;
[0034] Step 2: After the pasted PVC film and the 500D plain woven polyester cloth with a mesh size of 1 mm are preheated at 170° C. and 180° C. respectively, the two preheated pasted PVC films with the paste side facing the two sides of the plain woven mesh (500D plain woven polyester cloth with a mesh size of 1 mm) are hot-pressed at 175° C. and 35 kgf to obtain a plain woven mesh material that is not easy to pilling or wrinkle.
[0035] Embodiment 4 of the present invention is:
[0036] Preparation method of flat woven mesh material that is not easy to fuzz and wrinkle 75g / m 2 , including the following steps:
[0037] Step 1, applying a paste on one side of a PVC film, and drying to obtain a pasted PVC film; the paste is prepared by blending 100 kg of E-PVC paste resin, 70 kg of DOTP, 2.8 kg of barium zinc liquid stabilizer and 3 kg of isocyanate adhesive;
[0038] Step 2: The pasted PVC film and the 500D plain woven polyester cloth with a mesh size of 0.8 mm are preheated at 168° C. and 175° C. respectively, and the two preheated pasted PVC films with the paste side facing the two sides of the plain woven mesh (500D plain woven polyester cloth with a mesh size of 0.8 mm) are hot-pressed and laminated at 178° C. and 32 kgf to obtain a plain woven mesh material that is not prone to pilling and wrinkling.
[0039] Comparative Example 1:
[0040] The method for preparing a plain woven mesh material comprises the following steps:
[0041] Step 1: Apply paste on both sides of a 500D*18*17 plain woven polyester cloth, and dry to obtain a pasted mesh cloth; the paste used and the amount of paste applied on one side are the same as those in Example 1;
[0042] Step 2: Preheat the PVC film and the pasted mesh cloth as in Example 1 at 165°C and 175°C respectively, and place the two PVC films on both sides of the preheated pasted mesh cloth, and heat-press and bond them at 180°C and 30kgf to obtain a plain woven mesh material. The effect of cutting and welding the obtained plain woven mesh material is shown in FIG. Figure 3 and Figure 4 (left side).
[0043] Comparative Example 2:
[0044] The difference between the comparative example 2 and the comparative example 1 is that the 500D*18*17 plain woven polyester cloth is replaced with a 500D plain woven polyester cloth with a mesh size of 0.5 mm. The effect of the obtained plain woven cloth sandwich material after welding is shown in FIG. Figure 4 (right side).
[0045] All raw materials with the same name in the examples and comparative examples have the same source. The comparison results show that the plain woven mesh material obtained by the preparation method provided by the present invention has no burrs after cutting and trimming, and the cutting part is smooth and flat; and it is also very flat after welding, and the welding part is smooth and has no wrinkles.
[0046] In summary, the preparation method provided by the present invention is easy to operate. It only requires adding a pasting device before the laminating device, and it is easy to optimize and improve the production line. The plain woven mesh material prepared by the above preparation method is not prone to pilling, welding, and wrinkling, has good physical properties, and is easy to be processed and used subsequently.
[0047] The above descriptions are merely embodiments of the present invention and are not intended to limit the patent scope of the present invention. Any equivalent transformations made using the contents of the present invention's specification and drawings, or directly or indirectly applied in related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A method for preparing a flat woven mesh material that is not prone to fuzzing or wrinkling, characterized in that: The method comprises the following steps: applying paste to one side of a polymer film, drying to obtain the pasted polymer film; and placing the two polymer films with the paste on both sides of the plain woven fabric, respectively, and hot pressing and bonding them.
2. The preparation method according to claim 1, characterized in that: The polymer film is a PVC film or a TPU film.
3. The preparation method according to claim 2, characterized in that: When the polymer film is a PVC film, the amount of glue applied during the gluing process is 60 to 80 g / m 2 .
4. The preparation method according to claim 2, characterized in that: When the polymer film is a PVC film, the paste used in the pasting treatment includes, by weight, 100 parts of E-PVC paste resin, 60-80 parts of plasticizer, 3-4 parts of liquid stabilizer and 1-3 parts of adhesive.
5. The preparation method according to claim 4, characterized in that: The plasticizer is DOP, DINP or DOTP.
6. The preparation method according to claim 4, characterized in that: The liquid stabilizer is a barium zinc liquid stabilizer.
7. The preparation method according to claim 1, characterized in that: The mesh size of the plain woven fabric is 0.5-1 mm.
8. The preparation method according to claim 1, characterized in that: The temperature of the hot pressing bonding is 170-180°C.
9. The preparation method according to claim 1, characterized in that: The pressure of the thermal pressing bonding is 30-40 kgf.
10. A flat woven mesh material that is not prone to fuzzing or wrinkling, characterized in that: The compound is prepared by the preparation method according to any one of claims 1 to 9.
Citation Information
Patent Citations
Inflating cloth
CN101225608A
Method for processing thermoplastic elastomer toughening thin film composite fabric
CN101372164A
Random-texture pigment liquid for air die material and application of pigment liquid
CN103696285A